A method and device for measuring the thickness of carbon film for replicating precipitation phase in steel

By spraying the Pt layer in the FIB sample preparation equipment and performing transmission electron microscopy analysis, combined with a special thickness measurement device, the problem of inaccurate measurement of carbon film thickness is solved, the efficiency and success rate of carbon recombination is improved, and the carbon film thickness is ensured consistency and optimal process parameters.

CN118500310BActive Publication Date: 2024-11-26INST OF RES OF IRON & STEEL JIANGSU PROVINCE +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410968680.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-26
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

The prior art lacks methods for accurately measuring carbon film thickness, resulting in low carbon recombination efficiency and success rate. Thickness control depends on artificial color judgment, and there are differences in controllability and repeatability.

Method used

A carbon film thickness measurement method for precipitation phase replica in steel is adopted. By spraying the Pt layer in the FIB sample preparation equipment and performing transmission electron microscope line analysis, the carbon film thickness is measured using the intersection of Pt and C elements, combined with the special thickness The measuring device ensures consistency in the thickness of the carbon film during carbon spraying.

Benefits of technology

Accurate measurement of carbon film thickness, improve the efficiency and success rate of carbon composite, reduce human interference, ensure the optimal carbon film sputtering process parameters for different samples, and ensure that the carbon film is transparent and without interference under the electron beam .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118500310B_ABST
    Figure CN118500310B_ABST
Patent Text Reader

Abstract

The present invention relates to a thickness measurement method and device for a carbon film used for replicating a precipitated phase in steel. A sample is hot-mounted for grinding and polishing, and the sample is deeply etched after polishing, blown dry after etching, acetone is dripped on the etched surface of the sample, and the acetone solution is spread all over the surface, and then a cellulose acetate film is covered and dissolved in the etched surface. After the cellulose acetate film is dry, the cellulose acetate film is taken out and fixed on a thickness measuring device, and carbon is sprayed on the sample; the carbon film thickness measuring device is loaded in a FIB sample preparation device, and Pt is sprayed at any position on the sample surface to prepare a FIB sample with a thickness of less than 100nm. The sample is placed in a transmission electron microscope for line analysis to obtain the surface distribution of C, Pt and Al elements. The intersection of the Al and C lines is used as the end point, and the horizontal coordinate corresponding value A2 is measured. The intersection of the C and Pt lines is used as the starting point, and the horizontal coordinate corresponding value A1 is measured. The actual thickness of the carbon film H=A2-A1.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel, and in particular to a method and a device for measuring the thickness of a carbon film for replicating a precipitated phase in steel. Background Art

[0002] Usually, the precipitate phase in steel is analyzed by transmission electron microscopy to obtain information such as the composition, structure and distribution of the precipitate phase. There are strict requirements for sample thickness during transmission electron microscopy testing. Generally, the sample thickness is at least less than 200nm, and the thinner the better. For precipitate phase analysis, replica technology is generally used for sample preparation, and the replica is divided into primary replica and secondary replica. The primary replica is to deeply etch the sample and then spray a layer of carbon film on the sample surface with a high vacuum carbon spraying device, and then separate the carbon film from the sample surface. At this time, the precipitate phase will be taken out with the carbon film and adsorbed on the carbon film; the secondary replica is to deeply etch the sample and cover it with a layer of cellulose acetate film. After the dissolved film is dried, the cellulose acetate is removed from the sample surface, and then the surface of the removed cellulose acetate film in contact with the sample is sprayed with a layer of carbon film in a high vacuum carbon spraying instrument, and the cellulose acetate is dissolved by acetone and the carbon film is fished out. The carbon film separated by the two methods is fished out with a copper mesh and used for transmission electron microscopy analysis of the precipitate phase.

[0003] When using a copper mesh to fish out the carbon film, it is necessary to put the carbon film in deionized water for fishing. The thickness of the carbon film has a great influence on the success or failure of fishing: 1. If the carbon film is too thick, the precipitated phase information is covered by the thickness of the carbon film, and the tension of the water cannot make the carbon film fully unfold, and the carbon film forms wrinkles, and the position information of the precipitated phase cannot be analyzed; 2. If the carbon film is too thin, the tension of the water will cause the carbon film to break and the sample preparation will fail. Therefore, the thickness of the carbon film is an important control parameter during high vacuum carbon spraying.

[0004] The actual thickness of the carbon film directly affects the success rate of the precipitate preparation and the success or failure of the subsequent precipitate analysis. A carbon film of appropriate thickness can ensure that the carbon film does not break under the tension of deionized water during stripping, and can also ensure that it can be quickly unfolded in deionized water for easy scooping; at the same time, a suitable carbon film thickness can be used as a background when analyzing the precipitate, with uniform thickness and transparency under the electron beam, without interfering with the analysis of the precipitate.

[0005] The existing method is to judge the thickness of the carbon film by color, and estimate it based on the color change of the milky white ceramic piece placed next to the sample. A drop of oil is dropped on the ceramic piece in advance. When carbon is sprayed, the ceramic piece on the oil drop part does not deposit carbon and basically maintains its original color. The other parts gradually turn light brown and dark brown as the carbon film thickens. Generally, when the ceramic piece is light brown, the carbon film thickness just meets the requirements.

[0006] Since different people have different responses to facial radiation, and the feedback of colors under different lights is also different, the thickness of carbon spraying is affected by human factors, and the thickness controllability and repeatability are poor. Since it is impossible to ensure that the sample surface and the droplet surface are on the same plane, there is an error in the estimation of the actual thickness of the carbon film.

[0007] Currently, there is no quantitative method to accurately measure the thickness of the carbon film, thereby improving the efficiency and success rate of carbon replication. Summary of the invention

[0008] To solve the above problems, the present invention provides a method and device for measuring the thickness of a carbon film for replicating a precipitated phase in steel, which can quantitatively and accurately measure the thickness of the carbon film, thereby improving the efficiency and success rate of carbon replication.

[0009] The technical solution of the present invention is to provide a method for measuring the thickness of a carbon film for replicating a precipitated phase in steel, comprising the following steps:

[0010] S101: After hot mounting, the sample is ground and polished according to the standard steps of metallographic sample preparation, and the sample is deeply etched after polishing, and then rinsed with water and directly dried with a hair dryer after etching;

[0011] S103: one replication;

[0012] S105: secondary replication;

[0013] S107: Load the thickness measuring device into the FIB sample preparation device, spray Pt with a thickness of 2µm at any position on the surface of the sample treated in S105, and prepare a FIB sample with a thickness of less than 100nm;

[0014] S109: placing the prepared FIB sample in a transmission electron microscope for line analysis to obtain the surface distribution of C, Pt and Al elements;

[0015] S111: The intersection of Al and C lines is taken as the end point, and the horizontal axis corresponding value A2 is measured. The intersection of C and Pt lines is taken as the starting point, and the horizontal axis corresponding value A1 is measured. The actual thickness of the carbon film is H=A2-A1.

[0016] Furthermore, the specific steps of the primary replication in step S103 are: placing the sample processed in step S101 on a thickness measuring device, and carbon spraying the entire sample surface.

[0017] Furthermore, the specific steps of the secondary replication of S105 are: dripping acetone on the corrosion surface of the sample after the primary replication treatment, so that the acetone solution covers the entire surface, and then covering the corrosion surface with cellulose acetate film to dissolve in the corrosion surface, waiting for the cellulose acetate film to dry, taking out the cellulose acetate film, and placing it on a thickness measuring device, and spraying carbon on the entire sample surface.

[0018] Furthermore, the carbon spraying parameters in the primary and secondary replications are as follows: the distance between the sample surface and the carbon rod is ≥15 mm, and the vacuum degree is better than 9×10 -4 mbar, evaporation current 40A, time 40s, carbon injection current 70A, carbon injection time 1s.

[0019] Furthermore, the specific method for preparing the FIB sample in S107 is: depositing 2µm thick Pt at any position on the surface of the sample containing the carbon film, the length and width of Pt are 6µm×2µm, and after fine-tuning the pits, taking out the thin slice and welding it on the semi-copper mesh for thinning, the pit depth is 3µm, and when thinned to an electron beam acceleration voltage of 5kV, a current of 2nA, a brightness of 50%, and a contrast of 20%, the sample is transparent.

[0020] Furthermore, the specific method of S109 is: placing the half-copper mesh with the sample into a transmission electron microscope, tilting the thickness measuring device at an angle of 0°, and performing energy spectrum line analysis. During the analysis, the starting point of the line is on the Pt layer and the end point is on the Al layer, and a composite line distribution map of Pt, C and Al is obtained.

[0021] Another technical solution of the present invention is to provide a thickness measuring device for a carbon film for replicating a precipitated phase in steel, comprising a base, a first column adapted to the size of a fixing hole on a carbon injection instrument is provided at the bottom of the base, the thickness measuring device is inserted into the fixing hole through the first column to be fixed to the carbon injection instrument, a dovetail mortise is provided on the upper part of the base for mounting a film placement table, and a dovetail tenon matching the dovetail mortise is provided at the bottom of the film placement table;

[0022] A through slot is provided in the middle of the film placement platform, and the through slot divides the film placement platform into two separate left and right parts;

[0023] After the dovetail mortise is arranged on the upper part of the base, the upper surface of the base forms a first surface and a second surface, the first surface is the upper surface of the dovetail mortise, the second surface is the initial upper surface of the base without the dovetail mortise, the first surface is higher than the second surface, a first through hole is arranged on the first surface, a second through hole is arranged on the second surface, the first through hole and the second through hole are both used to install a carbon film deposition stage, after the film placement stage is installed on the base, the first through hole is located directly below the through slot, the carbon film deposition stage passes through the through slot and is installed to the base through the first through hole;

[0024] When the replica sample is directly placed on the first surface, the carbon film deposition platform is mounted to the base through the second through hole, and the height of the upper surface of the carbon film deposition platform is lower than the height of the upper surface of the replica sample.

[0025] Furthermore, the carbon film deposition platform includes a second column, the outer diameter of the second column is adapted to the inner diameters of the first through hole and the second through hole, and the upper portion of the second column is connected to the deposition platform.

[0026] Furthermore, a first threaded hole is provided at the bottom of the second column, and the first threaded hole is used to connect an extension screw, and the outer diameter of the extension screw is the same as the outer diameter of the second column.

[0027] Furthermore, the base is provided with a second threaded hole connected to the side of the first through hole and the second through hole, the central axis of the second threaded hole is perpendicular to the central axis of the first through hole and the second through hole, the second threaded hole is used to install a fastening screw, and a third threaded hole is provided on the side of the extension screw, and the fastening screw is screwed into the second threaded hole and the third threaded hole in sequence to tighten the extension screw.

[0028] Beneficial Effects

[0029] 1. The design of the thickness measuring device and the assembly method thereof in the present invention can ensure the consistency between the carbon film thickness measured during the carbon spraying process and the carbon film thickness on the actual sample, so that the measurement result is accurate. At the same time, the thickness measuring platform can be directly placed in the FIB sample preparation equipment for sample preparation after carbon spraying, thereby improving the sample preparation efficiency.

[0030] 2. The present invention solves the problems caused by the inability to accurately measure the thickness of carbon films with current replica samples through a dedicated sample stage and a corresponding thickness measurement method: 1) Since different people have different feedback on color and different feedback on color under different light, the thickness of the carbon spraying is poorly controllable and repeatable due to human influence factors; 2) The color judgment method cannot ensure that the sample surface and the droplet surface are in the same plane, so there is an error in estimating the actual thickness of the carbon film.

[0031] 3. This method can not only accurately obtain the thickness of the carbon film, but also eliminate the interference of human factors in traditional methods. Therefore, this method can determine the optimal carbon film sputtering process parameters for different samples to ensure that an unbreakable, transparent and interference-free carbon film under the electron beam can be obtained. At the same time, there are no special requirements for operators and they can be operated with simple training.

[0032] 4. The method of the present invention is simple, has a wide range of applications and is highly efficient.

[0033] 5. The formula for calculating the thickness of the carbon film is H=A2-A1, where A1 is the horizontal coordinate value of the intersection of the Pt and C element line distribution curves, and A2 is the horizontal coordinate value of the intersection of the Al and C element line distribution curves. Line analysis can accurately and intuitively reflect the concentration changes of different elements at different positions, avoiding errors in visual recognition. At the same time, during line analysis, the element lines intersect at a point, and the horizontal coordinate is the distance. The thickness is measured through the intersection point, avoiding boundary interference and ensuring the accuracy of the measurement.

[0034] 6. Line analysis data is the line scanning data measured by the energy spectrum when the tilt angle of the transmission electron microscope sample stage is 0°. The signal quantity detected by the analysis equipment is different at different tilt angles of the sample stage. In order to ensure the consistency and accuracy of the measurement results and take into account operability, the sample is required to be measured at 0°.

[0035] It should be appreciated that all combinations of the foregoing concepts, as well as additional concepts described in greater detail below, may be considered to be part of the inventive subject matter of the present disclosure, provided such concepts are not mutually inconsistent.

[0036] The foregoing and other aspects, embodiments and features of the present invention can be more fully understood from the following description in conjunction with the accompanying drawings. Other additional aspects of the present invention, such as the features and / or beneficial effects of the exemplary embodiments, will be apparent from the following description or learned from the practice of the specific embodiments according to the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] The accompanying drawings are not drawn to scale according to actual reference objects. In the accompanying drawings, each identical or nearly identical component shown in various figures may be represented by the same reference numeral. For the sake of clarity, not every component is labeled in each figure. Now, embodiments of various aspects of the present invention will be described by way of example and with reference to the accompanying drawings, in which:

[0038] Figure 1 This is a state diagram of the device for measuring the thickness of the carbon film for replicating the precipitated phase in the steel of the present invention when assembling the secondary replica sample.

[0039] Figure 2 This is a state diagram of the device for measuring the thickness of the carbon film for replicating the precipitated phase in steel of the present invention when assembling a primary replica sample.

[0040] Figure 3 Exploded view of the thickness measuring device of the carbon film for replicating the precipitated phase in the steel of the present invention.

[0041] Figure 4 This is a diagram of the actual position of the sample analyzed in the method of the present invention.

[0042] Figure 5This is the composite line distribution diagram of the elements corresponding to the line analysis of Example 1 of the present invention.

[0043] Figure 6 This is a measurement value diagram of Example 1 of the present invention.

[0044] Figure 7 This is a diagram showing the actual effect of the carbon replica according to Example 1 of the present invention.

[0045] Figure 8 This is a measurement value diagram of Example 2 of the present invention.

[0046] Fig. 9 This is a diagram showing the actual effect of the carbon replica of Example 2 of the present invention.

[0047] Description of Figure Numbers:

[0048] Base 1; fastening screw 2; film placement platform 3; extension screw 4; carbon film deposition platform 5; sample 6; first through hole 1-1; second through hole 1-2; second threaded hole 1-3; first column 1-6. DETAILED DESCRIPTION

[0049] In order to make the purpose, technical solution and advantages of the embodiment of the present invention clearer, the technical solution of the embodiment of the present invention will be clearly and completely described below in conjunction with the drawings of the embodiment of the present invention. Obviously, the described embodiment is a part of the embodiment of the present invention, not all of the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Unless otherwise defined, the technical terms or scientific terms used herein should be the common meaning understood by people with general skills in the field to which the present invention belongs.

[0050] The words "include" or "comprises" and the like used in the patent application specification and claims of the present invention mean that the elements or objects appearing before "include" or "comprises" include the features, wholes, steps, operations, elements and / or components listed after "include" or "comprises", and do not exclude the existence or addition of one or more other features, wholes, steps, operations, elements, components and / or their collections. "Up", "down", "left", "right" and the like are only used to indicate relative positional relationships. When the absolute position of the described object changes, the relative positional relationship may also change accordingly.

[0051] The existing method for measuring the thickness of carbon film is to judge the thickness of carbon film by color, and estimate it according to the color change of milky white ceramic sheet placed next to the sample. A drop of oil is dropped on the ceramic sheet in advance. When carbon is sprayed, the ceramic sheet on the oil drop part does not deposit carbon and basically maintains its original color. The other parts gradually turn into light brown and dark brown as the carbon film thickens. Generally, when the ceramic sheet is light brown, the thickness of the carbon film just meets the requirements.

[0052] Since different people have different responses to facial radiation, and the feedback of colors under different lights is also different, the thickness of carbon spraying is affected by human factors, and the thickness controllability and repeatability are poor. Since it is impossible to ensure that the sample surface and the droplet surface are on the same plane, there is an error in the estimation of the actual thickness of the carbon film.

[0053] Currently, there is no quantitative method to accurately measure the thickness of the carbon film, thereby improving the efficiency and success rate of carbon replication.

[0054] Based on the above problems, the present invention provides a method and device for measuring the thickness of a carbon film for replicating a precipitated phase in steel, which can quantitatively measure the thickness of the carbon film.

[0055] A technical solution of the present invention: a method for measuring the thickness of a carbon film for replicating a precipitated phase in steel, comprising the following steps:

[0056] S101: After hot mounting, the sample is ground and polished according to the standard steps of metallographic sample preparation, and the sample is deeply etched after polishing, and then rinsed with water and directly dried with a hair dryer after etching;

[0057] S103: one replication;

[0058] S105: secondary replication;

[0059] S107: Load the thickness measuring device into the FIB sample preparation device, spray Pt with a thickness of 2µm at any position on the surface of the sample treated in S105, and prepare a FIB sample with a thickness of less than 100nm;

[0060] S109: placing the prepared FIB sample in a transmission electron microscope for line analysis to obtain the surface distribution of C, Pt and Al elements;

[0061] S111: The intersection of Al and C lines is taken as the end point, and the horizontal axis corresponding value A2 is measured. The intersection of C and Pt lines is taken as the starting point, and the horizontal axis corresponding value A1 is measured. The actual thickness of the carbon film is H=A2-A1.

[0062] The actual thickness of the carbon film directly affects the success rate of the precipitate preparation and the success or failure of the subsequent precipitate analysis. A carbon film of appropriate thickness can ensure that the carbon film does not break under the tension of deionized water during stripping, and can also ensure that it can be quickly unfolded in deionized water for easy scooping; at the same time, a suitable carbon film thickness can be used as a background when analyzing the precipitate, with uniform thickness and transparency under the electron beam, without interfering with the analysis of the precipitate.

[0063] In some embodiments of the present invention, the specific steps of the primary replication in step S103 are: placing the sample processed in step S101 on a thickness measuring device, and carbon spraying the entire sample surface.

[0064] In some embodiments of the present invention, the specific steps of the secondary replication of S105 are: dripping acetone on the corrosion surface of the sample after the primary replication treatment to make the acetone solution cover the entire surface, then covering the corrosion surface with cellulose acetate film to dissolve in the corrosion surface, waiting for the cellulose acetate film to dry, taking out the cellulose acetate film, placing it on a thickness measuring device, and spraying carbon on the entire sample surface.

[0065] In some embodiments of the present invention, the carbon spraying parameters in the primary and secondary replications are: the distance between the sample surface and the carbon rod is ≥15 mm, the vacuum degree is better than 9×10 -4 mbar, evaporation current 40A, time 40s, carbon injection current 70A, carbon injection time 1s.

[0066] If the distance between the sample surface and the carbon rod is less than 15 mm, the film will be damaged by the high temperature of the carbon rod; if the vacuum degree is lower than 9×10 -4 mbar, the carbon film sprayed is not dense, and the carbon film is easy to break when taking it; the current of 40A and the time of 40s are used to remove the gas in the carbon rod, otherwise the sprayed carbon particles are too large to form a film; when the carbon spraying current is 70A and the carbon spraying time is 1s, the density and thickness of the carbon film are optimal.

[0067] In some embodiments of the present invention, the specific method for preparing the FIB sample in S107 is: depositing 2µm thick Pt at any position on the surface of the sample containing the carbon film, the length and width of Pt are 6µm×2µm, and after fine-tuning the pits, taking out the thin slice and welding it on a semi-copper mesh for thinning, the pit depth is 3µm, and when thinned to an electron beam acceleration voltage of 5kV, a current of 2nA, a brightness of 50%, and a contrast of 20%, the sample is transparent.

[0068] When the Pt deposition thickness is less than 2µm, Pt will gradually become thinner during the preparation process and will not be able to protect the sample. When the Pt deposition thickness is greater than 2µm, Pt is a consumable product and too thick will affect the processing efficiency. Therefore, the Pt deposition thickness of 2µm can both protect the sample and improve the processing efficiency. The length and width of Pt are 6µm×2µm, the pit depth is 3µm, and thinning to an electron beam acceleration voltage of 5kV and a current of 2nA are the optimal values ​​for sample presentation. The brightness of 50% and the contrast of 20% are the most appropriate parameters for judging the sample thickness.

[0069] In some embodiments of the present invention, the specific method of S109 is: placing the half-copper mesh with the sample into a transmission electron microscope, tilting the thickness measuring device at an angle of 0°, performing energy spectrum line analysis, and when analyzing, the starting point of the line is on the Pt layer and the end point is on the Al layer, to obtain a composite line distribution map of Pt, C and Al.

[0070] Line analysis data is the line scan data measured by the spectrum when the tilt angle of the transmission electron microscope sample stage is 0°. The signal quantity detected by the analysis equipment is different at different tilt angles of the sample stage. In order to ensure the consistency and accuracy of the measurement results and take into account operability, the sample is required to be measured when the tilt angle of the thickness measurement device is 0°.

[0071] Another technical solution of the present invention is to provide a thickness measuring device for a carbon film for replicating a precipitated phase in steel, comprising a base 1, a first column 1-6 adapted to the size of a fixing hole on a carbon injection instrument is provided at the bottom of the base 1, the thickness measuring device is inserted into the fixing hole through the first column 1-6 to be fixed to the carbon injection instrument, a dovetail mortise is provided on the upper part of the base 1 for mounting a film placement table 3, and a dovetail tenon matching the dovetail mortise is provided at the bottom of the film placement table 3;

[0072] A through slot is provided in the middle of the film placement platform 3, and the through slot divides the film placement platform 3 into two separate left and right parts;

[0073] After the dovetail mortise is arranged on the upper part of the base 1, the upper surface of the base 1 forms a first surface and a second surface, the first surface is the upper surface of the dovetail mortise, the second surface is the initial upper surface of the base without the dovetail mortise, the first surface is higher than the second surface, a first through hole 1-1 is arranged on the first surface, a second through hole 1-2 is arranged on the second surface, the first through hole 1-1 and the second through hole 1-2 are both used to install a carbon film deposition stage 5, after the thin film placement stage 3 is installed on the base 1, the first through hole 1-1 is located directly below the through slot, the carbon film deposition stage 5 passes through the through slot and is installed to the base through the first through hole 1-1;

[0074] When the replica sample 6 is directly placed on the first surface, the carbon film deposition platform 5 is mounted to the base through the second through hole 1 - 2 , and the upper surface height of the carbon film deposition platform 5 is lower than the upper surface height of the replica sample 6 .

[0075] The thickness measuring device of the carbon film for replicating the precipitated phase in Benxi steel is designed in this way to meet the needs of primary and secondary replication of the sample.

[0076] When the sample is replicated once, the installation method of the thickness measuring device is as follows: adhere the sample 6 to the upper surface of the dovetail mortise on the base, and then install the carbon film deposition platform 5 to the base 1 through the second through hole 1-2, ensuring that the height of the upper surface of the carbon film deposition platform 5 is lower than the height of the upper surface of the sample, place filter paper on the horizontal table, and place the assembled sample platform upside down on the filter paper, that is, the first column 1-6 faces upward, and adjust the carbon film deposition platform 5 so that the surface of the carbon film deposition platform 5 fits the surface of the filter paper.

[0077] When the sample is secondary replicated, the thickness measuring device is installed as follows: the carbon film deposition platform 5 is fixed to the base 1 by being installed in the first through hole 1-1 opened on the upper surface of the dovetail tenon, and the secondary replica sample film is placed on the upper surface of the film placement platform 3, flattened and firmly attached. Filter paper or other items that can keep the sample surface clean after contact are placed on the horizontal table, the assembled thickness measuring device is placed upside down on the filter paper, and the carbon film deposition platform 5 is adjusted so that the surface of the carbon film deposition platform 5 fits the surface of the filter paper.

[0078] In some embodiments of the present invention, the carbon film deposition platform 5 includes a second column, the outer diameter of the second column is adapted to the inner diameter of the first through hole 1-1 and the second through hole 1-2, and the upper part of the second column is connected to the deposition platform.

[0079] In some embodiments of the present invention, a first threaded hole is provided at the bottom of the second column, and the first threaded hole is used to connect an extension screw 4 , and the outer diameter of the extension screw 4 is the same as the outer diameter of the second column.

[0080] In some embodiments of the present invention, the base 1 is provided with a second threaded hole 1-3 connected to the side of the first through hole 1-1 and the second through hole 1-2, the central axis of the second threaded hole 1-3 is perpendicular to the central axis of the first through hole 1-1 and the second through hole 1-2, the second threaded hole 1-3 is used to install a fastening screw 2, and a third threaded hole is provided on the side of the extension screw 4, and the fastening screw 2 is screwed into the second threaded hole 1-3 and the third threaded hole in turn to fasten the extension screw 4.

[0081] When the sample is subjected to primary and secondary replication, the carbon film deposition platform 5 is adjusted by loosening the fastening screws 2 so that the surface of the carbon film deposition platform 5 fits the surface of the filter paper, and then tightening the fastening screws 2 .

[0082] The present invention is described in detail below in conjunction with the embodiments.

[0083] Example 1

[0084] A steel sample with a length, width and thickness of 10mm×15mm×3mm was selected as the test sample for testing. The specific steps are as follows:

[0085] Step 1: After hot mounting, the sample is ground and polished according to the standard metallographic sample preparation steps, and then rinsed with water and dried after deep etching;

[0086] Step 2: drip acetone solution on the corrosion surface, and when the corrosion surface is covered with a layer of acetone solution, stick the cellulose acetate film and dissolve it on the sample surface without bubbles;

[0087] Step 3: After the dissolved cellulose acetate film is dried, take out the film and place it on the film placement table 3 with the surface of the film in contact with the sample facing upwards. Use transparent tape to fix the edge of the film and ensure that the film is flat.

[0088] Step 4: Grind and polish the surface of the carbon film deposition platform 5 with 1500-grit sandpaper, corrode, clean and blow dry, and install it according to the standard assembly method;

[0089] Step 5: Place the sample stage into a high vacuum carbon spraying device for carbon spraying. Carbon spraying parameters: the distance between the sample surface and the carbon rod is 25 mm, and the vacuum degree is better than 9×10 -4 mbar, evaporation current 40A, time 40s, carbon injection current 70A, time 1s;

[0090] Step 6: After carbon spraying, take out the sample to prepare a carbon replica sample, take out the carbon film deposition table 5, put it into the FIB sample preparation equipment, deposit 2µm thick Pt at any position on the surface containing the carbon film, the length and width of Pt are 6µm×2µm, and after pit finishing, take out the thin slice and weld it on the semi-copper mesh for thinning, the pit depth is 3µm, and the sample is in a transparent state when the electron beam is 5kV, the current is 2nA, the brightness is 50%, and the contrast is 20%;

[0091] Step 7: Place the half copper mesh with the sample into the transmission electron microscope, tilt the sample stage to 0°, and perform energy spectrum line analysis. During the analysis, the starting point of the line is on the Pt layer and the end point is on the Al layer, and the composite line distribution map of Pt, C and Al is obtained;

[0092] Step 8: The horizontal coordinate value A2 of the intersection of the curves of Pt and C is measured to be 223nm, and the horizontal coordinate value A1 of the intersection of the curves of C and Al is 175nm. By H=A2-A1, the thickness of the carbon film is calculated to be H=223nm-175nm=48nm.

[0093] Figure 7 This is the actual effect of carbon replica after the thickness adjustment process is measured. The precipitated phase particles in the picture are clearly shown with distinct outlines and the carbon film is translucent.

[0094] Example 2

[0095] A steel sample with a length, width and thickness of 10mm×10mm×5mm was selected as the test sample for testing. The specific steps are as follows:

[0096] Step 1: After hot mounting, the sample is ground and polished according to the standard metallographic sample preparation steps, and then rinsed with water and dried after deep etching;

[0097] Step 2: Glue the prepared mounting sample onto the plane of the first surface of the base by using carbon conductive glue;

[0098] Step 3: Install the extension screw on the carbon film deposition platform 5 and fasten it into the second through hole 1-2 on the second surface of the base, ensure that the upper surface of the carbon film deposition platform 5 is lower than the surface of the embedded sample, place the filter paper on the table, and place the assembled thickness measuring device upside down on the filter paper, loosen the fastening screw 2, let the surface of the carbon film deposition platform 5 fit the surface of the filter paper, and tighten the fastening screw 2;

[0099] Step 4: Place the assembled sample stage into a high vacuum carbon spraying device for carbon spraying. The carbon spraying parameters are as follows: the sample surface is 15 mm away from the carbon rod, and the vacuum degree is better than 9×10 -4 mbar, evaporation current 40A, time 40s, carbon injection current 70A, time 1s;

[0100] Step 5: After carbon spraying, take out the sample to prepare a carbon replica sample, take out the carbon film deposition table 5, put it into the FIB sample preparation equipment, deposit 2µm thick Pt at any position on the surface containing the carbon film, the length and width of Pt are 6µm×2µm, and after pit finishing, take out the thin slice and weld it on the semi-copper mesh for thinning, the pit depth is 3µm, and the sample is in a transparent state when the electron beam is 5kV, the current is 2nA, the brightness is 50%, and the contrast is 20%;

[0101] Step 6: Place the half copper mesh with the sample into the transmission electron microscope, tilt the sample stage to 0°, and perform energy spectrum line analysis. During the analysis, the starting point of the line is on the Pt layer and the end point is on the Al layer, and the composite line distribution map of Pt, C and Al is obtained;

[0102] Step 7: The horizontal coordinate value A2 of the intersection of the curves of Pt and C is measured to be 223nm, and the horizontal coordinate value A1 of the intersection of the curves of C and Al is 176nm. The thickness of the carbon film is calculated to be H=A2-A1, which is 47nm;

[0103] Fig. 9 This is the actual effect of carbon replica after the thickness adjustment process is measured. The precipitated phase particles in the picture are clearly shown with distinct outlines and the carbon film is translucent.

[0104] The FIB mentioned in the article refers to focused ion beam, and the sample stage is the thickness measurement device.

[0105] In summary, the method of the present invention can accurately obtain the thickness of the carbon film and eliminates the interference of human factors in the traditional method. The method can determine the optimal carbon film sputtering process parameters for different samples to ensure that an unbreakable, transparent and interference-free carbon film under the electron beam can be obtained. At the same time, there are no special requirements for operators, the installation steps of the device are simple and easy to understand, and the device can be operated after simple training.

[0106] Although the present invention has been disclosed as above with preferred embodiments, it is not intended to limit the present invention. A person with ordinary knowledge in the technical field to which the present invention belongs may make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be determined by the definition of the claims.

Claims

1. A method for measuring the thickness of a carbon film for replicating a precipitated phase in steel, characterized in that: The following steps are involved: S101: After hot mounting, the sample is ground and polished according to the standard steps of metallographic sample preparation, and the sample is deep-etched after polishing, and then rinsed with water and blown dry after etching; S103: primary replication; the specific steps of the primary replication of S103 are: placing the sample processed in step S101 on a thickness measuring device, and carbon spraying the entire sample surface; S105: secondary replication; the specific steps of the secondary replication of S105 are: dripping acetone on the corrosion surface of the sample after the primary replication treatment, so that the acetone solution covers the entire surface, and then covering the cellulose acetate film to dissolve on the corrosion surface, waiting for the cellulose acetate film to dry, taking out the cellulose acetate film, and placing it on a thickness measuring device, and spraying carbon on the entire sample surface; S107: Load the thickness measuring device into the FIB sample preparation device, spray Pt with a thickness of 2µm at any position on the surface of the sample treated in S105, and prepare a FIB sample with a thickness of less than 100nm; S109: placing the prepared FIB sample in a transmission electron microscope for line analysis to obtain the surface distribution of C, Pt and Al elements; S111: The intersection of Al and C lines is taken as the end point, and the horizontal axis corresponding value A2 is measured. The intersection of C and Pt lines is taken as the starting point, and the horizontal axis corresponding value A1 is measured. The actual thickness of the carbon film is H=A2-A1.

2. The method for measuring the thickness of a carbon film for replicating a precipitated phase in steel according to claim 1, characterized in that: The carbon spraying parameters in the primary and secondary replications are as follows: the distance between the sample surface and the carbon rod is ≥15 mm, and the vacuum degree is better than 9×10 -4 mbar, evaporation current 40A, time 40s, carbon injection current 70A, carbon injection time 1s.

3. The method for measuring the thickness of a carbon film for replicating a precipitated phase in steel according to claim 1, characterized in that: The specific method for preparing the FIB sample in S107 is: depositing 2µm thick Pt at any position on the surface of the sample containing the carbon film, the length and width of Pt are 6µm×2µm, and after fine-tuning the pits, taking out the thin slice and welding it on the semi-copper mesh for thinning, the pit depth is 3µm, and when thinned to an electron beam acceleration voltage of 5kV, a current of 2nA, a brightness of 50%, and a contrast of 20%, the sample is transparent.

4. The method for measuring the thickness of a carbon film for replicating a precipitated phase in steel according to claim 1, characterized in that: The specific method of S109 is: placing the half copper mesh with the sample into a transmission electron microscope, tilting the thickness measuring device at an angle of 0°, and performing energy spectrum line analysis. During the analysis, the starting point of the line is on the Pt layer and the end point is on the Al layer, and a composite line distribution map of Pt, C and Al is obtained.

5. A thickness measuring device applicable to the thickness measuring method of carbon film for replicating precipitation phase in steel according to claim 1, characterized in that: The device comprises a base, wherein a first column having a size adapted to a fixing hole on a carbon injection instrument is provided at the bottom of the base, and a thickness measuring device is inserted into the fixing hole through the first column so as to be fixed to the carbon injection instrument. The device is characterized in that a dovetail mortise is provided at the upper part of the base for mounting a film placement table, and a dovetail tenon matching the dovetail mortise is provided at the bottom of the film placement table; A through slot is provided in the middle of the film placement platform, and the through slot divides the film placement platform into two separate left and right parts; After the dovetail mortise is arranged on the upper part of the base, the upper surface of the base forms a first surface and a second surface, the first surface is the upper surface of the dovetail mortise, the second surface is the initial upper surface of the base without the dovetail mortise, the first surface is higher than the second surface, a first through hole is arranged on the first surface, a second through hole is arranged on the second surface, the first through hole and the second through hole are both used to install a carbon film deposition stage, after the film placement stage is installed on the base, the first through hole is located directly below the through slot, the carbon film deposition stage passes through the through slot and is installed to the base through the first through hole; When the replica sample is directly placed on the first surface, the carbon film deposition platform is mounted to the base through the second through hole, and the height of the upper surface of the carbon film deposition platform is lower than the height of the upper surface of the replica sample.

6. The device for measuring the thickness of a carbon film for replicating a precipitated phase in steel according to claim 5, characterized in that: The carbon film deposition platform comprises a second column, the outer diameter of the second column is matched with the inner diameters of the first through hole and the second through hole, and the upper part of the second column is connected to the deposition platform.

7. The device for measuring the thickness of a carbon film for replicating a precipitated phase in steel according to claim 6, characterized in that: A first threaded hole is provided at the bottom of the second column. The first threaded hole is used to connect an extension screw. The outer diameter of the extension screw is the same as the outer diameter of the second column.

8. The device for measuring the thickness of a carbon film for replicating a precipitated phase in steel according to claim 7, characterized in that: The base is provided with a second threaded hole connected to the first through hole and the side of the second through hole, the central axis of the second threaded hole is perpendicular to the central axis of the first through hole and the second through hole, the second threaded hole is used to install a fastening screw, and the side of the extension screw is provided with a third threaded hole, and the fastening screw is screwed into the second threaded hole and the third threaded hole in sequence to fasten the extension screw.