A method for growing LED epitaxial layers to improve luminous efficiency
By inserting a pause annealing layer with low temperature, high N2, low H2, and low NH3 after the LP layer or HP layer of the LED epitaxial layer, the problems of low Mg doping efficiency and insufficient hole concentration in the prior art are solved, and LEDs are realized Improved luminous efficiency.
Patent Information
- Application Number
- CN202410757149.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-06-13
AI Technical Summary
In the existing LED epitaxial layer structure, low-temperature LP-doped Mg layer and high-temperature HP-doped Mg layer grow under high concentration H2 conditions, resulting in low Mg doping efficiency and insufficient hole concentration and lattice mass, which limits the improvement of LED luminescence efficiency. .
The pause annealing layer of low temperature, high N2, low H2, and low NH3 environment is inserted after the LP layer or HP layer. By adjusting the generation temperature, gas concentration and annealing time, the activation efficiency and hole concentration of Mg are improved, thereby improving the luminescence of LEDs efficiency.
By inserting the pause annealing layer, the activation efficiency and hole concentration of Mg are significantly improved, the luminous efficiency of LEDs are improved, and the lattice quality is improved and the light efficiency is improved through annealing treatment.
Smart Images

Figure CN118507606B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of LED preparation, and in particular relates to a method for growing an LED epitaxial layer for improving luminous efficiency. Background Art
[0002] Nowadays, light emitting diodes (LEDs), especially nitride light emitting diodes, have been widely used in the field of general lighting due to their high luminous efficiency. How to improve the luminous efficiency of light emitting diodes (LEDs) has become an important issue that needs to be solved.
[0003] In the existing LED epitaxial layer structure, the low-temperature LP Mg-doped layer, the high-temperature HP Mg-doped layer, and the PP layer all need to be grown under high-concentration H2 conditions. Although this is beneficial to Mg doping, only the PP layer is annealed in the normal structure, and the efficiency of Mg-H2 bond breaking is relatively low. The hole concentration increased by the annealing layer is still low, which restricts the improvement of light efficiency. Therefore, it is necessary to develop a method to effectively improve the luminous efficiency of LEDs. Summary of the invention
[0004] The technical problem to be solved by the present invention is to overcome the deficiencies and defects mentioned in the above background technology and provide an epitaxial layer growth method for improving the luminous efficiency of LEDs. By inserting a low temperature, high N2, low H2, low NH3 environment pause annealing layer after the LP layer or / and the HP layer through a new design, the activation efficiency of Mg can be greatly improved, the hole concentration and the lattice quality can be improved, and thus the luminous efficiency of LEDs can be improved.
[0005] In order to solve the above technical problems, the technical solution proposed by the present invention is:
[0006] A method for growing an LED epitaxial layer for improving luminous efficiency, wherein the LED epitaxial layer comprises a low-temperature Mg-doped LP layer and a high-temperature Mg-doped HP layer, and a pause annealing layer is inserted after the LP layer or / and the HP layer, namely, an LPR pause annealing layer and / or an HPR pause annealing layer; and the generation temperature, H2 concentration, and NH3 concentration of the LPR pause annealing layer are all lower than those of the LP layer, and the N2 concentration is higher than that of the LP layer; and the generation temperature, H2 concentration, and NH3 concentration of the HPR pause annealing layer are all lower than those of the HP layer, and the N2 concentration is higher than that of the HP layer.
[0007] Furthermore, the LPR pause annealing layer has a generation temperature 50-150° C. lower than that of the LP layer, a N2 concentration more than 50% higher, a H2 concentration 170-270slm lower, and a NH3 concentration more than 20% lower.
[0008] Furthermore, the generation temperature of the LPR pause annealing layer is 700-750° C., the N2 concentration is 200-400 slm, the H2 concentration is 0-100 slm, and the NH3 concentration is 20-100 slm.
[0009] Furthermore, the HPR pause annealing layer has a generation temperature 50-150° C. lower than that of the HP layer, a N2 concentration more than 50% higher, a H2 concentration 250-350slm lower, and a NH3 concentration more than 20% lower.
[0010] Furthermore, the generation temperature of the HPR pause annealing layer is 820-900° C., the N2 concentration is 200-350 slm, the H2 concentration is 0-100 slm, and the NH3 concentration is 20-200 slm.
[0011] Furthermore, in the LPR pause annealing layer or / and the HPR pause annealing layer, the TEG flow rate is 0 sccm, the CP2Mg flow rate is 0 sccm, the annealing time is 0 s to 3 min, the pressure is 200 to 250 Torr, and the rotation speed is 1000 to 1200 rpm.
[0012] Furthermore, the growth thickness of the LP layer and / or the HP layer is 150-200 Å, the CP2Mg flow rate is 300-3000 sccm, the pressure is 200-250 Torr, and the rotation speed is 1000-1200 rpm.
[0013] Furthermore, when the CP2Mg flow rate of the LP layer is 600 sccm, the annealing time of the LPR pause annealing layer is 30 s; when the CP2Mg flow rate of the LP layer is 3000 sccm, the annealing time of the LPR pause annealing layer is 3 min.
[0014] Furthermore, when the CP2Mg flow rate of the HP layer is 300 sccm, the annealing time of the HPR pause annealing layer is 30 s; when the CP2Mg flow rate of the HP layer is 1500 sccm, the annealing time of the HPR pause annealing layer is 3 min.
[0015] Furthermore, the growth process of the LED epitaxial layer includes in sequence: processing the substrate, growing a buffer layer, growing a UGaN layer, growing a NGaN buffer layer, growing a stress release layer, growing a MQW layer, growing a LP layer, growing a LPR pause annealing layer, growing a PAI layer, growing a HP layer, growing a HP pause annealing layer, growing a PP layer, growing an annealing layer, and processing an END layer.
[0016] Compared with the prior art, the present invention has the following beneficial effects:
[0017] 1. The present invention can activate Mg efficiency, increase hole concentration, and thus improve luminescence efficiency by inserting a pause annealing layer after the LP layer and / or the HP layer.
[0018] 2. When the pause annealing layer is inserted in the present invention, through different carrier gas atmospheres, the lattice part with poor quality in the grown UGaN layer is effectively dissociated and decomposed into the structural layer in a timely and effective manner in the subsequent annealing and recasting step due to the annealing treatment, and the lattice part with low quality can be disposed of in time, and the functional layer with high lattice quality is retained, thereby improving the lattice quality and improving the luminous efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0020] Figure 1 is a schematic structural diagram of an LED epitaxial layer in an embodiment of the present invention;
[0021] Figure 2 Schematic diagram of the relationship between the LPR pause annealing layer and the LP layer growth in an embodiment of the present invention;
[0022] Figure 3 1 is a comparison of annealing conditions and light effects in the embodiments of the present invention. DETAILED DESCRIPTION
[0023] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the present invention, but the protection scope of the present invention is not limited to the following specific embodiments.
[0024] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0025] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0026] The present invention provides a method for growing an LED epitaxial layer with improved luminous efficiency. After the LP layer, an LPR pause annealing layer is inserted (growth condition requirements: the temperature is about 100 °C lower than that of the LP layer, the N2 ratio is more than 50% higher than that of the LP layer, the H2 is low (H2 can be 0), and the NH3 component is low (the NH3 ratio is less than 20% higher than that of the LP layer)). Through low temperature, low H2, and high N2 conditions, the LP layer is annealed to activate the Mg efficiency, and multiple cycles are repeated to further improve the Mg activation efficiency; an HPR pause annealing layer is inserted into the HP layer (growth condition requirements: the temperature is about 100 °C lower than that of the HP layer, the N2 ratio is more than 50% higher than that of the HP layer, the H2 is low (H2 can be 0), and the NH3 component is low (the NH3 ratio is less than 20% higher than that of the HP layer)). Through low temperature, low H2, and high N2 conditions, the HP layer is annealed to activate the Mg efficiency, and multiple cycles are repeated to further improve the Mg activation efficiency. The LPR pause annealing layer and the HPR pause annealing layer can exist alone or both in a structure. Through this design, the Mg efficiency is maximally improved, the hole concentration is increased, and thus the luminous efficiency is improved. The specific structure design is as follows Figure 1 。
[0027] In the specific experimental process, the present invention found that there is a certain correlation between the Mg concentration and the gas flow rate of the pause annealing layer, and between the Mg concentration of the LP layer / HP layer and the growth time of the pause annealing layer. Taking the growth conditions of the LPR layer as the only variable condition, it is shown that when the Mg concentration and the LP growth conditions are certain (LP growth conditions: rotation speed 1200 rpm, reaction chamber pressure 200 Torr, Temp: 800 °C, N2: 150 slm, H2: 270 slm, NH3: 135 slm; growth time 3 min), the growth conditions of the LPR layer are set as: Temp: 720 °C, N2: 300 slm, H2: 50 slm, NH3: 60 slm, TEG flow rate: 0 sccm, CP2Mg flow rate: 0 sccm, growth 3 min, and the Mg activation efficiency is the best, and the Mg concentration is increased by 30% compared with the comparison. See specifically Figure 2 。And according to the annealing mechanism, high N2 content, low temperature, and long annealing time are beneficial to annealing. Therefore, in the actual production process, it is defined that when the Mg flow rate of the LP layer = 600 sccm, the annealing time of the LPR layer is 30 s, and when the Mg flow rate of the LP layer = 3000 sccm, the annealing time of the LPR layer is 3 min, which can maximally improve the Mg efficiency. Similarly, when the Mg flow rate of the HP layer = 300 sccm, the annealing time of the HPR layer is 30 s, and when the Mg flow rate of the HP layer = 1500 sccm, the annealing time of the HPR layer is 3 min, which can maximally improve the Mg efficiency.
[0028] Specific growth condition range of the P layer:
[0029] 1. LP layer growth conditions: Temp: 800°C, N2: 150slm, H2: 270slm, NH3: 135slm, LP layer growth thickness: 150A, CP2Mg flow: 600~3000sccm, pressure P=200Torr; rotation speed: 1200rpm;
[0030] 2. LPR layer growth conditions: Temp: 700~750℃, N2: 200~400slm, H2: 0~100slm, NH3: 20~100slm, TEG flow: 0sccm, CP2Mg flow: 0sccm, annealing time 30s~3min, pressure P=200Torr; rotation speed: 1200rpm;
[0031] HP / HPR conditions are similarly defined as follows:
[0032] 3. HP layer growth conditions: Temp: 950°C, N2: 50slm, H2: 350slm, NH3: 150slm, HP layer growth thickness: 200A, CP2Mg flow: 300~1500sccm, pressure P=200Torr; rotation speed: 1000rpm;
[0033] 4. HPR layer growth conditions: Temp: 820~900℃, N2: 200~350slm, H2: 0~100slm, NH3: 20~135slm, TEG flow: 0sccm, CP2Mg flow: 0sccm, annealing time 30s~3min, pressure P=200Torr; rotation speed: 1000rpm.
[0034] In order to further compare the light effects under various annealing conditions, the present invention also provides the following experiments. Taking conventional PP layer annealing as the control, experimental groups 1 to 3 are respectively conventional PP layer annealing + LP followed by an LPR pause annealing layer, conventional PP layer annealing + LP followed by an HPR pause annealing layer, conventional PP layer annealing + LP followed by an LPR pause annealing layer + LP followed by an HPR pause annealing layer. Other parameter conditions are the same as those in this embodiment. Epitaxial layers and their LEDs are obtained, and the light effects of their chips are tested. Figure 3 It can be seen that the chip luminous efficiency is best when the annealing conditions are conventional PP layer annealing + LPR pause annealing layer inserted after LP + HPR pause annealing layer inserted after LP. Compared with the chip luminous efficiency of conventional PP layer annealing, the improvement is more than 2%, indicating that the method of the present invention can effectively improve the luminous efficiency of LEDs.
Claims
1. A method for growing an LED epitaxial layer to improve luminous efficiency, wherein the LED epitaxial layer comprises a low-temperature Mg-doped LP layer and a high-temperature Mg-doped HP layer, characterized in that: Insert a pause annealing layer after the LP layer or / and the HP layer, i.e., an LPR pause annealing layer / and an HPR pause annealing layer; and the generation temperature, H2 concentration, and NH3 concentration of the LPR pause annealing layer are all lower than those of the LP layer, and the N2 concentration is higher than that of the LP layer; the generation temperature, H2 concentration, and NH3 concentration of the HPR pause annealing layer are all lower than those of the HP layer, and the N2 concentration is higher than that of the HP layer; The LPR pause annealing layer has a generation temperature 50-150°C lower than that of the LP layer, a N2 concentration of more than 50%, a H2 concentration of 170-270slm lower, and a NH3 concentration of more than 20% lower; The HPR pause annealing layer has a generation temperature 50-150°C lower than that of the HP layer, a N2 concentration of more than 50%, a H2 concentration of 250-350slm lower, and a NH3 concentration of more than 20% lower; In the LPR pause annealing layer or / and the HPR pause annealing layer, the TEG flow rate is 0 sccm, the CP2Mg flow rate is 0 sccm, and the annealing time is 0 s to 3 min; The CP2Mg flow rate of the LP layer and / or the HP layer is 300-3000 sccm; When the CP2Mg flow rate of the LP layer is 600sccm, the annealing time of the LPR pause annealing layer is 30s; when the CP2Mg flow rate of the LP layer is 3000sccm, the annealing time of the LPR pause annealing layer is 3min; When the CP2Mg flow rate of the HP layer is 300 sccm, the annealing time of the HPR pause annealing layer is 30 s; when the CP2Mg flow rate of the HP layer is 1500 sccm, the annealing time of the HPR pause annealing layer is 3 min.
2. The LED epitaxial layer growth method for improving luminous efficiency according to claim 1, characterized in that: The generation temperature of the LPR pause annealing layer is 700-750° C., the N2 concentration is 200-400slm, the H2 concentration is 0-100slm, and the NH3 concentration is 20-100slm.
3. The LED epitaxial layer growth method for improving luminous efficiency according to claim 1, characterized in that: The generation temperature of the HPR pause annealing layer is 820-900° C., the N2 concentration is 200-350 slm, the H2 concentration is 0-100 slm, and the NH3 concentration is 20-200 slm.
4. The LED epitaxial layer growth method for improving luminous efficiency according to claim 1, characterized in that: In the LPR pause annealing layer and / or the HPR pause annealing layer, the pressure is 200-250 Torr, and the rotation speed is 1000-1200 rpm.
5. The LED epitaxial layer growth method for improving luminous efficiency according to claim 1, characterized in that: The growth thickness of the LP layer and / or the HP layer is 150-200A, the pressure is 200-250 Torr, and the rotation speed is 1000-1200 rpm.
6. The LED epitaxial layer growth method for improving luminous efficiency according to any one of claims 1 to 5, characterized in that: The growth process of the LED epitaxial layer includes: processing a substrate, growing a buffer layer, growing a UGaN layer, growing an NGaN buffer layer, growing a stress release layer, growing an MQW layer, growing an LP layer, growing an LPR pause annealing layer, growing a PAI layer, growing an HP layer, growing an HP pause annealing layer, growing a PP layer, growing an annealing layer, and processing an END layer.
Citation Information
Patent Citations
LED epitaxial layer growth method for improving luminous efficiency and LED epitaxial layer
CN104009136A
P-type GaN layer preparation method and LED epitaxial structure preparation method
CN105047534A
LED epitaxial structure with stress release layer and growth method thereof
CN117650210A
LED epitaxial structure with N-type electron blocking layer and LED device
CN211700321U
Epitaxial-wafer manufacturing method and epitaxial wafer
JP2009206283A