A carbon dioxide-based (polycarbonate-polyurea) block copolymer solid electrolyte and preparation method thereof

Through carbon dioxide-based (polycarbonate-polyurea) block copolymer solid electrolyte, the problems of flammability and leakage of liquid electrolytes in lithium-ion batteries are solved, and high-performance lithium-ion battery electrolytes are achieved, with high performance Ion conductivity, mechanical strength and electrochemical stability improve the safety and energy density of the battery.

CN118507825BActive Publication Date: 2024-11-08SUN YAT SEN UNIV +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410941272.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-08
Estimated Expiration
2044-07-15

AI Technical Summary

Technical Problem

The liquid electrolytes used in existing lithium-ion batteries are flammable and easy to leak, have low energy density, and have side reactions with the lithium metal negative electrode, resulting in insufficient safety and performance.

Method used

Carbon dioxide-based (polycarbonate-polyurea) block copolymer is used as solid electrolyte, and the polycarbonate and polyurea prepolymer are copolymerized with isocyanate through the preparation process, lithium salts and plasticizers are added to form a high ionic conductivity , solid electrolyte with mechanical strength and wide electrochemical stability window.

Benefits of technology

It achieves high ion conductivity, high lithium ion migration number, low glass transition temperature, good mechanical strength and electrochemical stability, avoids leakage and side reactions of liquid electrolytes, and improves the safety and energy density of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118507825B_ABST
    Figure CN118507825B_ABST
Patent Text Reader

Abstract

The present invention discloses a carbon dioxide-based (polycarbonate-polyurea) block copolymer solid electrolyte and a preparation method thereof, which is composed of a (polycarbonate-polyurea) block copolymer, a lithium salt and a plasticizer. The present invention uses carbon dioxide as a raw material to prepare polycarbonate and polyurea prepolymer respectively, and then block copolymerizes the polycarbonate and polyurea prepolymer with isocyanate, obtains the (polycarbonate-polyurea) block copolymer as a base film after separation and purification, and obtains it after adding lithium salt and plasticizer. The present invention has a unique microphase separation structure, and the highly crystallized polyurea segment can provide sufficient mechanical strength for the electrolyte, while not affecting the segment swing of the polycarbonate, reducing the impact on lithium ion conductivity. The present invention has high ionic conductivity, high lithium ion migration number, low glass transition temperature, wide electrochemical stability window, and good mechanical strength and film-forming properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of organic polymer functional materials and electrochemical technology, and more specifically, to a carbon dioxide-based solid polymer electrolyte and a preparation method thereof. Background Art

[0002] As the most commonly used battery system at present, lithium-ion batteries have been widely used in mobile communications, digital cameras, personal computers, electric vehicles and other fields.

[0003] The existing lithium-ion battery system uses organic liquid electrolytes, which have problems such as flammability, leakage, low energy density, and serious side reactions with lithium metal negative electrodes. Unlike liquid electrolytes, solid polymer electrolytes do not have leakage problems, and can also avoid the use of diaphragms to increase battery energy density. At the same time, they can reduce side reactions with lithium metal negative electrodes and inhibit the growth of lithium dendrites. Due to its safety, reliability, easy processing, and good interface compatibility, solid polymer electrolytes are considered to be one of the most promising development directions for lithium-ion batteries.

[0004] Common solid polymer electrolytes include polyethylene oxide (PEO), polyacrylonitrile (PAN), polymethyl methacrylate (PMMA), polyvinylidene fluoride (PVDF) and polycarbonate (PC). At present, there have been many studies on solid polymer electrolytes at home and abroad, but practice has proved that it is difficult for a single-component solid polymer electrolyte to simultaneously meet the requirements of ionic conductivity, mechanical strength, electrochemical stability window, lithium ion migration number and interface compatibility, especially ionic conductivity and mechanical properties. Block copolymers with reasonable structural design can solve this problem and take into account different performance parameters. Summary of the invention

[0005] The purpose of the present invention is to solve the problems of flammability, leakage and low energy density of liquid electrolytes, and to provide a carbon dioxide-based (polycarbonate-polyurea) block copolymer solid electrolyte and a preparation method thereof.

[0006] To achieve the above object, the present invention adopts the following technical solution:

[0007] A carbon dioxide-based (polycarbonate-polyurea) block copolymer solid electrolyte, comprising a (polycarbonate-polyurea) block copolymer, a lithium salt and a plasticizer, wherein the (polycarbonate-polyurea) block copolymer has a structural formula as shown in (I), wherein R1 represents hydrogen, methyl, a chlorine-containing side chain group, an oxygen-containing side chain group, a nitrogen-containing side chain group or a double-bond side chain group; R2 represents an ethyl group, a butyl group or a hexyl group; and R3 represents toluene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate or dicyclohexylmethane-4,4'-diisocyanate;

[0008] Preferably, in the above-mentioned carbon dioxide-based (polycarbonate-polyurea) block copolymer solid electrolyte, the lithium salt is one or more of LiFSI, LiTFSI, LiPF6, LiBF6, LiODFB, LiBOB and LiPO2F2.

[0009] Preferably, in the above-mentioned carbon dioxide-based (polycarbonate-polyurea) block copolymer solid electrolyte, the plasticizer is one or more of succinonitrile, dimethyl carbonate, diethyl carbonate, ethylene carbonate, diethylene glycol dimethyl ether, dioxolane, polyethylene glycol, polyethylene glycol dimethacrylate, and ethylene urea.

[0010] Preferably, in the above-mentioned carbon dioxide-based (polycarbonate-polyurea) block copolymer solid electrolyte, the mass percentage of the lithium salt ranges from 5% to 60%, the mass percentage of the plasticizer ranges from 5% to 80%, and the balance is the (polycarbonate-polyurea) block copolymer.

[0011] A method for preparing a carbon dioxide-based (polycarbonate-polyurea) block copolymer solid electrolyte comprises the following steps:

[0012] S1. Using carbon dioxide as a raw material to prepare polycarbonate prepolymer and polyurea prepolymer respectively;

[0013] S2. The polycarbonate prepolymer and the polyurea prepolymer obtained in step S1 are copolymerized with isocyanate, and separated and purified to obtain a (polycarbonate - polyurea) block copolymer;

[0014] S3. The (polycarbonate-polyurea) block copolymer obtained in step S2 is mixed with a lithium salt and a plasticizer to obtain a carbon dioxide-based (polycarbonate-polyurea) block copolymer solid electrolyte.

[0015] Preferably, in the above-mentioned method for preparing the carbon dioxide-based (polycarbonate-polyurea) block copolymer solid electrolyte, the polycarbonate prepolymer is obtained by reacting carbon dioxide and an epoxy compound.

[0016] Preferably, in the above-mentioned method for preparing the carbon dioxide-based (polycarbonate-polyurea) segmented copolymer solid electrolyte, the polyurea prepolymer is obtained by reacting carbon dioxide and a monomer containing a terminal amino group.

[0017] Preferably, in the above-mentioned method for preparing the carbon dioxide-based (polycarbonate-polyurea) segmented copolymer solid electrolyte, the method adopted for the copolymerization reaction in step S2 is solution polymerization or melt polymerization; the steps of the copolymerization reaction are first reacting the isocyanate with the polycarbonate prepolymer for 0.5 to 6 h, and then adding the polyurea prepolymer to react for 0.5 to 10 h.

[0018] Preferably, in the above-mentioned method for preparing the carbon dioxide-based (polycarbonate-polyurea) block copolymer solid electrolyte, the isocyanate in step S2 is one or more of toluene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate and dicyclohexylmethane-4,4'-diisocyanate.

[0019] Preferably, in the above-mentioned method for preparing the carbon dioxide-based (polycarbonate-polyurea) block copolymer solid electrolyte, the mass ratio of the polycarbonate prepolymer to the polyurea prepolymer in step S2 is in the range of 20:1 to 0.5:1.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The present invention uses carbon dioxide as a raw material to prepare polycarbonate and polyurea prepolymer respectively, then blocks and copolymerizes the polycarbonate and polyurea prepolymer with isocyanate, obtains a (polycarbonate-polyurea) block copolymer as a base film after separation and purification, and obtains a carbon dioxide-based (polycarbonate-polyurea) block copolymer solid electrolyte after adding lithium salt and plasticizer. The polycarbonate segment and the polyurea segment can synergistically promote the dissociation of the lithium salt, while improving the lithium ion conductivity and the lithium ion migration number, and the polyurea segment can reduce the side reaction and stabilize the lithium metal negative electrode by anchoring the lithium salt anion. The (polycarbonate-polyurea) block copolymer of the present invention has a unique microphase separation structure, and the highly crystallized polyurea segment can provide sufficient mechanical strength for the electrolyte, while not affecting the segment swing of the polycarbonate, and reducing the impact on the lithium ion conductivity. The copolymer solid electrolyte prepared by the present invention has high ionic conductivity, high lithium ion migration number, low glass transition temperature, wide electrochemical stability window, good mechanical strength and film-forming performance. In addition, the preparation method of the carbon dioxide-based (polycarbonate-polyurea) block copolymer solid electrolyte of the present invention is simple, environmentally friendly, and has low raw material prices. It can achieve the recycling of greenhouse gas carbon dioxide and has excellent economic and social benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 Schematic diagram of the reaction steps of (polycarbonate-polyurea) block copolymer;

[0023] Figure 2The differential calorimetric scanning diagram of (polycarbonate-polyurea) block copolymer under different synthesis conditions;

[0024] Figure 3 Characterization of the microphase separation structure of (polycarbonate-polyurea) block copolymers;

[0025] Figure 4 The electrochemical impedance spectroscopy of the electrolyte at different temperatures;

[0026] Figure 5 It is the fitting diagram of the Arrhenius relationship between ionic conductivity and temperature;

[0027] Figure 6 This is the linear voltammetric scan test result of the electrolyte. DETAILED DESCRIPTION

[0028] The preparation of some compounds involved in the present invention and the performance test results are listed below to further illustrate the present invention in detail, but the embodiments of the present invention are not limited thereto.

[0029] The preparation process of the present invention is as follows:

[0030] The reactor was purged with hot air at 400 °C using a heat gun and then vacuumed for 15 min. Then, 20 mL of amino-terminated monomer A was added to the reactor in a glove box filled with N2, and CO2 was introduced at a pressure of 5 MPa. The reaction temperature was set at 180 °C and the reaction time was 6 h. After the reaction was completed, the product was taken out, the sample was purified to remove residual monomers and by-products, and dried in a vacuum drying oven at 120 °C for 48 h to obtain a polyurea prepolymer.

[0031] In a glove box filled with N2, initiator (ASA), triethyl boron (TEB), epoxy compound B and 1-4 butanediol (BDO) were added to a 50 mL reactor, and then the reactor was heated to a reaction temperature of 45°C, a reaction pressure of 1 MPa, and a reaction time of 10 h. After the reaction was completed, the reactor was cooled to room temperature, CO2 was slowly discharged by opening the outlet valve, and then impurities were removed by stirring with deionized water, and then vacuum dried at 80°C until transparent to obtain a polycarbonate prepolymer.

[0032] mg polycarbonate prepolymer was placed in a three-necked flask, the temperature was raised to 120°C for vacuum dehydration for 2 h, after which an appropriate amount of anhydrous NMP was added for dissolution, and then isocyanate C was added for preliminary polymerization at 120°C for 2 h, and finally ng polyurea prepolymer was added for chain extension at 120°C for 3 h to obtain a (polycarbonate-polyurea) block copolymer, the reaction product was precipitated with pure water, and dried by air and vacuum for 24 h respectively.

[0033] Using tetrahydrofuran as solvent, (polycarbonate-polyurea) block copolymer, lithium salt D and plasticizer E were mixed at a solid-liquid ratio of 1 g: 10 mL. After stirring for 2 h, a uniform mixed solution was obtained. 0.3-0.5 mL of the mixed solution was dripped into the positive electrode shell, and the solvent was evaporated at 80°C for 6 h. Then, vacuum drying was continued at 80°C for 12 h to obtain a (polycarbonate-polyurea) block copolymer solid polymer electrolyte. The reaction steps of (polycarbonate-polyurea) block copolymer are as follows: Figure 1 shown.

[0034] With reference to the above preparation method, the specific results are shown in Table 1.

[0035]

[0036] Taking Example 1 as an example, the mass proportion of the (polycarbonate-polyurea) block copolymer in the solid polymer electrolyte is adjusted to 40%, the mass proportion of the lithium salt in the solid polymer electrolyte is 15%, and the mass proportion of succinonitrile in the solid polymer electrolyte is 45%. A solid polymer electrolyte is prepared, and an electrochemical impedance spectroscopy test is performed on it at different temperatures using an electrochemical workstation. The ionic conductivity characterization results of the solid polymer electrolyte are calculated and shown in Table 2 below:

[0037]

[0038] It can be seen from Table 1 that the room temperature ionic conductivity of the solid polymer electrolyte based on Example 1 can reach 1.31×10 -4 S cm -1 At 60 °C, its ionic conductivity is as high as 4.75×10 -4 S cm -1 In addition, the charge transfer resistance R ct The resistance is less than 100 Ω at different temperatures, showing good interfacial compatibility. Figure 2 The differential scanning calorimetry (DSC) test results of the (polycarbonate-polyurea) block copolymers prepared under different synthesis conditions based on Example 1 are shown. The glass transition temperature T g All are below 30 ℃, which provides support for the higher ionic conductivity of the electrolyte from another perspective. Figure 3 This is the transmission electron microscopy (TEM) characterization result of the (polycarbonate-polyurea) block copolymer based on Example 1. From the figure, an obvious "island" structure can be found, that is, the polyurea segment (dark area) and the polycarbonate segment (light area) produce a microphase separation structure, which can take into account both mechanical strength and ionic conductivity. Figure 4This is the electrochemical AC impedance spectrum of the solid electrolyte based on Example 1. It can be seen from the figure that the interface impedance decreases significantly with the increase of temperature, which helps to improve the energy density and reduce the energy loss during battery operation. Figure 5 This is a fitting diagram of the Arrhenius relationship between ionic conductivity and temperature based on Example 1. The fitting result shows good consistency with the test result, indicating the reliability of the test result. Figure 6 This is the linear voltammetry (LSV) result of the solid electrolyte based on Example 1. It can be seen from the figure that the electrolyte has good electrochemical stability and the electrochemical stability window is as high as 4.5 V.

[0039]

[0040] Table 3 shows the ionic conductivity test results of Example 3. Due to the similar block structure, it can achieve similar performance to Example 1. Other Examples 2 and Examples 4-9 can also achieve similar performance to Example 1.

Claims

1. A carbon dioxide-based (polycarbonate-polyurea) block copolymer solid electrolyte, characterized in that The invention is composed of a (polycarbonate-polyurea) block copolymer, a lithium salt and a plasticizer; the structural formula of the (polycarbonate-polyurea) block copolymer is shown in (I), wherein R1 represents hydrogen, methyl, a chlorine-containing side chain group, an oxygen-containing side chain group, a nitrogen-containing side chain group or a double-bond side chain group; R2 represents an ethyl group, a butyl group or a hexyl group; and R3 represents toluene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate or dicyclohexylmethane-4,4'-diisocyanate; ; The lithium salt is one or more of LiFSI, LiTFSI, LiPF6, LiBF6, LiODFB, LiBOB and LiPO2F2; The plasticizer is one or more of succinonitrile, dimethyl carbonate, diethyl carbonate, ethylene carbonate, diethylene glycol dimethyl ether, dioxolane, polyethylene glycol, polyethylene glycol dimethacrylate, and ethylene urea; The method for preparing the carbon dioxide-based (polycarbonate-polyurea) block copolymer solid electrolyte comprises the following steps: S1. Using carbon dioxide as a raw material to prepare polycarbonate prepolymer and polyurea prepolymer respectively; S2. The polycarbonate prepolymer and the polyurea prepolymer obtained in step S1 are copolymerized with isocyanate, and separated and purified to obtain a (polycarbonate - polyurea) block copolymer; S3. The (polycarbonate-polyurea) block copolymer obtained in step S2 is mixed with a lithium salt and a plasticizer to obtain a carbon dioxide-based (polycarbonate-polyurea) block copolymer solid electrolyte.

2. The carbon dioxide-based (polycarbonate-polyurea) block copolymer solid electrolyte according to claim 1, characterized in that: The mass percentage of the lithium salt is in the range of 5% to 60%, the mass percentage of the plasticizer is in the range of 5% to 80%, and the balance is the (polycarbonate-polyurea) block copolymer.

3. The carbon dioxide-based (polycarbonate-polyurea) block copolymer solid electrolyte according to claim 1, characterized in that: The polycarbonate prepolymer is obtained by reacting carbon dioxide and an epoxy compound.

4. The carbon dioxide-based (polycarbonate-polyurea) block copolymer solid electrolyte according to claim 1, characterized in that: The polyurea prepolymer is obtained by reacting carbon dioxide and a monomer containing a terminal amino group.

5. The carbon dioxide-based (polycarbonate-polyurea) block copolymer solid electrolyte according to claim 1, characterized in that: The method adopted for the copolymerization reaction in step S2 is solution polymerization or melt polymerization; the steps of the copolymerization reaction are to first react the isocyanate with the polycarbonate prepolymer for 0.5 to 6 hours, and then add the polyurea prepolymer to react for 0.5 to 10 hours.

6. The carbon dioxide-based (polycarbonate-polyurea) block copolymer solid electrolyte according to claim 1, characterized in that: The isocyanate in step S2 is one or more of toluene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate and dicyclohexylmethane-4,4'-diisocyanate.

7. The carbon dioxide-based (polycarbonate-polyurea) block copolymer solid electrolyte according to claim 1, characterized in that: The mass ratio of the polycarbonate prepolymer to the polyurea prepolymer in step S2 is in the range of 20:1 to 0.5:1.

Citation Information

Patent Citations

  • Solid electrolyte composition, solid-electrolyte-containing sheet and all-solid-state secondary battery, production method for solid-electrolyte-containing sheet and all-solid-state secondary battery, segmented polymer, and non-aqueous-solvent dispersion of polymer and segmented polymer

    CN109526241A

  • Oxygen-enriched polymer electrolyte as well as preparation method and application thereof

    CN109755643A

  • Polyurea-based gel electrolyte, preparation method and application

    CN115763963A

  • Precursor composition for preparing polymer electrolyte, and polymer electrolyte and secondary battery prepared using same

    CN115868057A

  • Carbon dioxide-based poly-cyclic carbonate electrolyte as well as preparation method and application thereof

    CN116979140A