Antistatic PET release film and preparation method thereof

By using a composite polyester layer and protective layer structure in the PET release film, combining strength and antistatic properties, the problems of poor antistatic properties and insufficient waterproof properties of traditional PET release film are solved, and high strength, self-repair, The antibacterial and antistatic effects extend the service life.

CN118514406BActive Publication Date: 2024-11-08WORLD STAR TECH INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410491774.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-23
Publication Date
2024-11-08
Estimated Expiration
2044-04-23

AI Technical Summary

Technical Problem

Traditional PET release films have poor anti-static properties, which are prone to electrostatic accumulation, resulting in dust deposition and damage, and are insufficient waterproof, resulting in short service life.

Method used

The composite polyester layer and protective layer structure are adopted. The composite polyester layer is composed of PET, dispersant, solvent and composite carbon nanotube. The protective layer is composed of silicone polyurethane and composite carbon nanotubes, and is melt-extruded through a double-layer coextrusion die head. The extraction and bidirectional tensile process is prepared to increase the bond strength of the antistatic layer and the substrate layer, and a protective layer is applied to the surface to improve the antistatic and water resistance.

Benefits of technology

It achieves antibacterial, water-resistant and antistatic properties of the self-healing surface, extends the service life of the PET release film, and improves the resistance to mechanical damage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004805626980000081
    Figure BDA0004805626980000081
Patent Text Reader

Abstract

The invention relates to the technical field of PET release films, in particular to an antistatic PET release film and a preparation method thereof. A polyester base material and an antistatic polyester layer material are co-extruded to prepare a composite polyester layer; sodium lignin sulfonate is grafted and modified to obtain quaternized sodium lignin sulfonate; carbon nanotubes are modified together with dihydroxy imidazole salt ionic liquid and quaternized sodium lignin sulfonate to obtain composite carbon nanotubes; organic silicon polyurethane and the composite carbon nanotubes are blended as a protective coating, polytetrahydrofuran diol, isophorone diisocyanate and hydroxyl-terminated polydimethylsiloxane are used as raw materials, an organic silicon prepolymer is prepared under the action of a catalyst dibutyltin dilaurate, 2,2-bishydroxymethylpropionic acid and isosorbide are used as chain extenders, and 2-hydroxyethyl disulfide and quaternized sodium lignin sulfonate are used as end-capping agents to prepare the organic silicon polyurethane.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of PET release films, in particular to an antistatic PET release film and a preparation method thereof. Background Art

[0002] Release film generally refers to a film that has slight or no stickiness after contact with a specific material under limited conditions, and can play the role of isolation, filling, protection, easy peeling, etc. At present, PET release film has been widely used in packaging, printing, electronics, sealing, circuit boards, adhesive products, die-cutting and punching processing and other fields because of its excellent mechanical properties and good thermal stability.

[0003] Traditional PET release films have poor antistatic properties. In actual applications, static electricity accumulation can easily cause dust deposition and even damage to the protected parts. The existing method of enhancing the antistatic properties of release films is to spray an antistatic protective layer on the outside, which can easily cause the surface flatness to deteriorate and affect the release force of the release film. At the same time, the sprayed antistatic layer is prone to wear and aging and cannot provide long-term protection. In addition, the existing PET release film has average waterproof properties and is prone to corrosion and mildew in a humid environment, which reduces the service life of the release film. Summary of the invention

[0004] The object of the present invention is to provide an antistatic PET release film and a preparation method thereof, so as to solve the problems in the prior art.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0006] An antistatic PET release film comprises a composite polyester layer and a protective layer; the composite polyester layer is formed by co-extrusion of a polyester base layer and an antistatic polyester layer; the raw material composition of the antistatic polyester layer is, by weight, 70-100 parts of PET, 1-5 parts of a dispersant, 5-10 parts of a solvent, and 0.1-0.5 parts of composite carbon nanotubes; the raw material composition of the protective layer is, by weight, 18-21 parts of silicone polyurethane and 0.5-1 parts of composite carbon nanotubes.

[0007] Furthermore, the dispersant in the antistatic polyester layer is one of polyethylene glycol and polyvinyl pyrrolidone.

[0008] Furthermore, the solvent in the antistatic polyester layer is one of ethanol, N,N-dimethylformamide and N-methylpyrrolidone.

[0009] Furthermore, the preparation of the composite carbon nanotubes comprises the following steps:

[0010] 1) Mix 3-chloro-1,2-propylene glycol and 1-methylimidazole, heat to 68-72° C. and keep warm for 10-12 hours, cool, add methanol, wash with ether 3-5 times, and rotary evaporate to obtain a dihydroxy imidazole salt ionic liquid;

[0011] 2) Mix carbon nanotubes, quaternized sodium lignin sulfonate, dihydroxyimidazole salt ionic liquid, methanol and deionized water, grind, ultrasonically treat for 1-2 hours, filter, wash, dry and grind to obtain composite carbon nanotubes.

[0012] Further, the preparation of the silicone polyurethane comprises the following steps:

[0013] Under a nitrogen atmosphere, the temperature of polytetrahydrofuran diol is raised to 120°C and kept for 2 hours, isophorone diisocyanate, hydroxyl-terminated polydimethylsiloxane and dibutyltin dilaurate are added, the temperature is lowered to 78-82°C and kept for 1-2 hours, a mixed solution of 2,2-bis(hydroxymethyl)propionic acid and N-methylpyrrolidone is added, stirring is continued for 5-10 minutes, isosorbide and acetone are added, stirring is continued for 2-3 hours, the temperature is lowered to 58-62°C, 2-hydroxyethyl disulfide is added, stirring is continued for 1-2 hours, quaternized sodium lignin sulfonate is added, stirring is continued for 1-2 hours, cooling is carried out, deionized water is added for emulsification for 1-2 hours, rotary evaporation is performed, and the material is discharged to obtain silicone polyurethane.

[0014] Furthermore, the mass ratio of carbon nanotubes, quaternized sodium lignin sulfonate, and dihydroxyimidazole salt ionic liquid is 1:3:1.

[0015] Furthermore, the mass ratio of polytetramethylene glycol, isophorone diisocyanate, and hydroxyl-terminated polydimethylsiloxane is 7.4:4.4:0.6; the mass ratio of hydroxyl-terminated polydimethylsiloxane, 2,2-bis(hydroxymethyl)propionic acid, isosorbide, 2-hydroxyethyl disulfide, and quaternized sodium lignin sulfonate is 0.6:0.3:0.2:0.2:0.3.

[0016] Furthermore, the preparation of quaternized sodium lignin sulfonate includes the following steps: mixing sodium lignin sulfonate and sodium hydroxide, heating to 83-87° C., adding (3-chloro-2-hydroxypropyl)trimethylammonium chloride, and continuing to keep warm for 3-4 hours to obtain quaternized sodium lignin sulfonate.

[0017] Furthermore, a method for preparing an antistatic PET release film comprises the following steps:

[0018] S1: PET is used as the polyester base material;

[0019] S2: Put the dispersant, solvent and composite carbon nanotubes into a high-speed mixer, stir at 500-1000 r / min for 15-20 min, then put in PET, continue stirring for 15-20 min, and dry to obtain an antistatic polyester layer material;

[0020] S3: melt-extrude the polyester base material and the antistatic polyester layer material through a double-layer co-extrusion die, cool the cast sheet, biaxially stretch, heat-set, and cool to obtain a composite polyester layer;

[0021] S4: mixing the silicone polyurethane and the composite carbon nanotubes to obtain a protective coating;

[0022] S5: coating the protective coating on the surface of the composite polyester layer and drying it to obtain an antistatic PET release film.

[0023] Furthermore, the working conditions of the biaxial stretching are: temperature 108-110° C., stretching rate 100-110 mm / s, and transverse and longitudinal stretching ratio 2.5.

[0024] Beneficial effects of the present invention:

[0025] The invention provides an antistatic PET release film and a preparation method thereof. By limiting raw materials and processes, an antibacterial, water-resistant and antistatic PET release film with good mechanical strength and a self-repairing surface is prepared.

[0026] In the present invention, a polyester base material and an antistatic polyester layer material are co-extruded to improve the bonding strength between the antistatic layer and the base material layer and prevent delamination. In order to give the antistatic polyester layer excellent antistatic performance, carbon nanotubes and sodium lignin sulfonate are selected as antistatic agents and blended with the matrix resin polyethylene terephthalate. In order to improve the uniformity and antistatic property of the carbon nanotubes and sodium lignin sulfonate in the matrix resin, the sodium lignin sulfonate is first grafted and modified to obtain a quaternary ammonium containing both anions and cations in the molecular structure. Sodium lignin sulfonate, in order to improve the stability of quaternary ammonium sodium lignin sulfonate, the electrostatic interaction between the sulfonate group and the imidazole group is used to introduce a dihydroxy imidazole salt ionic liquid with high conductivity, high thermal stability, chemical stability and excellent water solubility. Together with the quaternary ammonium sodium lignin sulfonate, the carbon nanotubes are modified by a grinding method to obtain composite carbon nanotubes; the composite carbon nanotubes are introduced into the matrix resin polyethylene terephthalate, thereby greatly improving the antistatic and antibacterial properties of the release film, and greatly extending the service life of the PET release film.

[0027] In order to make the antistatic property of PET release film durable, silicone polyurethane and composite carbon nanotubes are blended as protective coating and coated on the surface of composite polyester layer to form a water-resistant, antibacterial and antistatic surface with self-repairing properties, thereby greatly improving the ability of PET release film to resist mechanical damage.

[0028] With polytetramethylene glycol, isophorone diisocyanate and hydroxyl-terminated polydimethylsiloxane as raw materials, silicone prepolymer was prepared under the action of dibutyltin dilaurate catalyst, 2,2-bis(hydroxymethyl)propionic acid and isosorbide were used as chain extenders, and 2-hydroxyethyl disulfide and quaternized sodium lignin sulfonate were used as end-capping agents to prepare silicone polyurethane, wherein hydroxyl-terminated polydimethylsiloxane effectively improved the water resistance of the protective layer, 2-hydroxyethyl disulfide provided dynamic disulfide bonds to give the silicone polyurethane a certain self-healing ability, and quaternized sodium lignin sulfonate gave the protective layer excellent antibacterial properties. On this basis, composite carbon nanotubes were added to improve the self-healing ability and mechanical strength of the protective layer. DETAILED DESCRIPTION

[0029] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] It should be noted that if the embodiments of the present invention involve directional indications such as up, down, left, right, front, and back, the directional indication is only used to explain a specific posture such as the relative position relationship between the components, the movement status, etc. If the specific posture changes, the directional indication will also change accordingly. In addition, the technical solutions between the various embodiments can be combined with each other, but it must be based on the ability of ordinary technicians in this field to implement. When the combination of technical solutions is contradictory or cannot be implemented, it should be considered that such a combination of technical solutions does not exist and is not within the protection scope required by the present invention.

[0031] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only used to explain the present invention, and are not used to limit the present invention.

[0032] Embodiment 1: A method for preparing an antistatic PET release film, comprising the following steps:

[0033] S1: PET is used as the polyester base material;

[0034] S2: Put the dispersant, solvent and composite carbon nanotubes into a high-speed mixer, stir at 500r / min for 20min, then put in PET, continue stirring for 15min, and dry to obtain an antistatic polyester layer material;

[0035] S3: melt-extrude the polyester base material and the antistatic polyester layer material through a double-layer co-extrusion die, cool the cast sheet, biaxially stretch, heat-set, and cool to obtain a composite polyester layer;

[0036] S4: mixing the silicone polyurethane and the composite carbon nanotubes to obtain a protective coating;

[0037] S5: coating the protective coating on the surface of the composite polyester layer and drying it to obtain an antistatic PET release film;

[0038] The working conditions of biaxial stretching are: temperature 108°C, stretching rate 100 mm / s, and transverse and longitudinal stretching ratio 2.5;

[0039] In terms of weight, the raw material composition of the antistatic polyester layer is: 70 parts of PET, 1 part of dispersant, 5 parts of solvent, and 0.1 parts of composite carbon nanotubes; the raw material composition of the protective layer is: 18 parts of silicone polyurethane and 0.5 parts of composite carbon nanotubes;

[0040] The dispersant in the antistatic polyester layer is polyethylene glycol; the solvent in the antistatic polyester layer is ethanol;

[0041] The preparation of the composite carbon nanotubes comprises the following steps:

[0042] 1) At 68°C, 4 g of 3-chloro-1,2-propylene glycol and 2 g of 1-methylimidazole were mixed, kept warm for 10 h, cooled, 2.5 mL of methanol was added, washed with ether for 3 times, and rotary evaporated to obtain a bishydroxyimidazole salt ionic liquid;

[0043] 2) 1 g of carbon nanotubes, 3 g of quaternized sodium lignin sulfonate, 1 g of dihydroxyimidazole salt ionic liquid, 3 mL of methanol, and 10 mL of deionized water were mixed, ground, and ultrasonically treated for 1 h, filtered, washed, dried, and ground to obtain composite carbon nanotubes;

[0044] The preparation of silicone polyurethane includes the following steps:

[0045] Under a nitrogen atmosphere, 7.4 g of polytetrahydrofuran diol was heated to 120° C. and kept warm for 2 h, 4.4 g of isophorone diisocyanate, 0.6 g of hydroxyl-terminated polydimethylsiloxane, and 2 drops of dibutyltin dilaurate were added, the temperature was lowered to 78° C. and kept warm for 2 h, 0.3 g of 2,2-bis(hydroxymethyl)propionic acid and a mixed solution of 1 g of N-methylpyrrolidone were added, stirring was continued for 5 min, 0.2 g of isosorbide and 15 mL of acetone were added, stirring was continued for 2 h, the temperature was lowered to 58° C., 0.2 g of 2-hydroxyethyl disulfide was added, stirring was continued for 1 h, 0.3 g of quaternized sodium lignin sulfonate was added, stirring was continued for 1 h, cooling was performed, 27 g of deionized water was added for emulsification for 1 h, rotary evaporation was performed, and the material was discharged to obtain silicone polyurethane;

[0046] The preparation of the quaternized sodium lignin sulfonate comprises the following steps: 5 g of sodium lignin sulfonate and 15 mL of a sodium hydroxide solution with a mass concentration of 15% are mixed, the temperature is raised to 83° C., 2 mL of (3-chloro-2-hydroxypropyl)trimethylammonium chloride is added, and the temperature is kept for 3 hours to obtain the quaternized sodium lignin sulfonate.

[0047] Embodiment 2: A method for preparing an antistatic PET release film, comprising the following steps:

[0048] S1: PET is used as the polyester base material;

[0049] S2: Put the dispersant, solvent and composite carbon nanotubes into a high-speed mixer, stir at 800 r / min for 18 min, then put in PET, continue stirring for 18 min, and dry to obtain an antistatic polyester layer material;

[0050] S3: melt-extrude the polyester base material and the antistatic polyester layer material through a double-layer co-extrusion die, cool the cast sheet, biaxially stretch, heat-set, and cool to obtain a composite polyester layer;

[0051] S4: mixing the silicone polyurethane and the composite carbon nanotubes to obtain a protective coating;

[0052] S5: coating the protective coating on the surface of the composite polyester layer and drying it to obtain an antistatic PET release film;

[0053] The working conditions of biaxial stretching are: temperature 109°C, stretching rate 105 mm / s, and transverse and longitudinal stretching ratio 2.5;

[0054] In terms of weight, the raw material composition of the antistatic polyester layer is: 95 parts of PET, 3 parts of dispersant, 7 parts of solvent, and 0.3 parts of composite carbon nanotubes; the raw material composition of the protective layer is: 20 parts of silicone polyurethane and 0.7 parts of composite carbon nanotubes;

[0055] The dispersant in the antistatic polyester layer is polyethylene glycol; the solvent in the antistatic polyester layer is ethanol;

[0056] The preparation of the composite carbon nanotubes comprises the following steps:

[0057] 1) At 70°C, 4 g of 3-chloro-1,2-propylene glycol and 2 g of 1-methylimidazole were mixed, kept warm for 11 h, cooled, 2.5 mL of methanol was added, washed with ether for 4 times, and rotary evaporated to obtain a bishydroxyimidazole salt ionic liquid;

[0058] 2) 1 g of carbon nanotubes, 3 g of quaternized sodium lignin sulfonate, 1 g of dihydroxyimidazole salt ionic liquid, 3 mL of methanol, and 10 mL of deionized water were mixed, ground, and ultrasonically treated for 1.5 h, filtered, washed, dried, and ground to obtain composite carbon nanotubes;

[0059] The preparation of silicone polyurethane includes the following steps:

[0060] Under a nitrogen atmosphere, 7.4 g of polytetrahydrofuran diol was heated to 120° C. and kept warm for 2 h, 4.4 g of isophorone diisocyanate, 0.6 g of hydroxyl-terminated polydimethylsiloxane, and 2 drops of dibutyltin dilaurate were added, the temperature was lowered to 80° C. and kept warm for 1.5 h, a mixed solution of 0.3 g of 2,2-bis(hydroxymethyl)propionic acid and 1 g of N-methylpyrrolidone was added, stirring was continued for 8 min, 0.2 g of isosorbide and 15 mL of acetone were added, stirring was continued for 2.5 h, the temperature was lowered to 60° C., 0.2 g of 2-hydroxyethyl disulfide was added, stirring was continued for 1.5 h, 0.3 g of quaternized sodium lignin sulfonate was added, stirring was continued for 1.5 h, cooling was performed, 27 g of deionized water was added for emulsification for 1 h, rotary evaporation was performed, and the material was discharged to obtain silicone polyurethane;

[0061] The preparation of the quaternized sodium lignin sulfonate comprises the following steps: 5 g of sodium lignin sulfonate and 15 mL of a sodium hydroxide solution with a mass concentration of 15% are mixed, the temperature is raised to 85° C., 2 mL of (3-chloro-2-hydroxypropyl)trimethylammonium chloride is added, and the temperature is kept for 3.5 hours to obtain the quaternized sodium lignin sulfonate.

[0062] Embodiment 3: A method for preparing an antistatic PET release film, comprising the following steps:

[0063] S1: PET is used as the polyester base material;

[0064] S2: Put the dispersant, solvent and composite carbon nanotubes into a high-speed mixer, stir at 1000r / min for 15min, then put in PET, continue stirring for 20min, and dry to obtain an antistatic polyester layer material;

[0065] S3: melt-extrude the polyester base material and the antistatic polyester layer material through a double-layer co-extrusion die, cool the cast sheet, biaxially stretch, heat-set, and cool to obtain a composite polyester layer;

[0066] S4: mixing the silicone polyurethane and the composite carbon nanotubes to obtain a protective coating;

[0067] S5: coating the protective coating on the surface of the composite polyester layer and drying it to obtain an antistatic PET release film;

[0068] The working conditions of biaxial stretching are: temperature 110°C, stretching rate 110 mm / s, and transverse and longitudinal stretching ratio 2.5;

[0069] In terms of weight, the raw material composition of the antistatic polyester layer is: 100 parts of PET, 5 parts of dispersant, 10 parts of solvent, and 0.5 parts of composite carbon nanotubes; the raw material composition of the protective layer is: 21 parts of silicone polyurethane and 1 part of composite carbon nanotubes;

[0070] The dispersant in the antistatic polyester layer is polyethylene glycol; the solvent in the antistatic polyester layer is ethanol;

[0071] The preparation of the composite carbon nanotubes comprises the following steps:

[0072] 1) At 72°C, 4 g of 3-chloro-1,2-propylene glycol and 2 g of 1-methylimidazole were mixed, kept warm for 12 h, cooled, 2.5 mL of methanol was added, washed with ether for 5 times, and rotary evaporated to obtain a bishydroxyimidazole salt ionic liquid;

[0073] 2) 1 g of carbon nanotubes, 3 g of quaternized sodium lignin sulfonate, 1 g of dihydroxyimidazole salt ionic liquid, 3 mL of methanol, and 10 mL of deionized water were mixed, ground, and ultrasonically treated for 2 h, filtered, washed, dried, and ground to obtain composite carbon nanotubes;

[0074] The preparation of silicone polyurethane includes the following steps:

[0075] Under a nitrogen atmosphere, 7.4 g of polytetrahydrofuran diol was heated to 120° C. and kept warm for 2 h, 4.4 g of isophorone diisocyanate, 0.6 g of hydroxyl-terminated polydimethylsiloxane, and 2 drops of dibutyltin dilaurate were added, the temperature was lowered to 82° C. and kept warm for 1 h, 0.3 g of 2,2-bis(hydroxymethyl)propionic acid and 1 g of N-methylpyrrolidone were added, stirring was continued for 10 min, 0.2 g of isosorbide and 15 mL of acetone were added, stirring was continued for 3 h, the temperature was lowered to 62° C., 0.2 g of 2-hydroxyethyl disulfide was added, stirring was continued for 2 h, 0.3 g of quaternized sodium lignin sulfonate was added, stirring was continued for 2 h, cooling was performed, 27 g of deionized water was added for emulsification for 1 h, rotary evaporation was performed, and the material was discharged to obtain silicone polyurethane;

[0076] The preparation of the quaternized sodium lignin sulfonate comprises the following steps: 5 g of sodium lignin sulfonate and 15 mL of a sodium hydroxide solution with a mass concentration of 15% are mixed, the temperature is raised to 87° C., 2 mL of (3-chloro-2-hydroxypropyl)trimethylammonium chloride is added, and the temperature is kept for 4 hours to obtain the quaternized sodium lignin sulfonate.

[0077] Comparative Example 1: Taking Example 3 as the control group, sodium lignin sulfonate was used to replace the quaternized sodium lignin sulfonate, and other processes were normal.

[0078] Comparative Example 2: Example 3 was used as a control group, in which no dihydroxyimidazole salt ionic liquid was prepared, and other processes were normal.

[0079] Comparative Example 3: Taking Example 3 as the control group, carbon nanotubes were used to replace the composite carbon nanotubes, and other processes were normal.

[0080] Comparative Example 4: Taking Example 3 as the control group, the silicone polyurethane was replaced by silicone coating (001: Langfang Wanteng Anticorrosion Materials Co., Ltd.), and the other processes were normal.

[0081] The mass ratio of the polyester base material to the antistatic polyester layer material in the examples and comparative examples is 1:1.5; the thickness of the composite polyester layer in the examples and comparative examples is 0.5 mm, and the thickness of the protective layer is 0.2 mm.

[0082] Source of raw materials (for demonstration only):

[0083] Polytetrahydrofurandiol 25190-06-1: Hubei Xinkang Pharmaceutical Chemical Co., Ltd.; PET 230BK-112: BASF; 3-chloro-1,2-propanediol 96-24-2: Merck reagent; polyethylene glycol P103723, 1-methylimidazole M109227, carbon nanotubes C434711, isophorone diisocyanate I109582, hydroxy-terminated polydimethylsiloxane P304442, dibutyltin dilaurate D100274, 2,2-bis(hydroxymethyl)propionic acid B104539, N-methylpyrrolidone M100589, isosorbide I157515, 2-hydroxyethyl disulfide B598951, (3-chloro-2-hydroxypropyl)trimethylammonium chloride C120679, sodium lignin sulfonate S140863: Aladdin reagent; ethanol, methanol, ether, acetone, sodium hydroxide, analytical grade: Sinopharm reagent.

[0084] Performance test: The PET release films in the embodiments and comparative examples were tested;

[0085] Tensile strength: The sample was cut into 120mm long and 15mm wide, and tested using a universal material testing machine with a tensile rate of 50mm / min; Surface resistivity: The test temperature was 25℃, the relative humidity was 25%, and the surface resistivity of the sample was tested using a surface resistance tester; Antibacterial property: Refer to GB / T 21866-2008 was tested, and Escherichia coli AS1.90 was selected as the test strain; Water resistance: the sample was cut into 1cm×1cm, the surface was wiped clean, dried for 4h, and the sample mass m0 was weighed. At 25°C, the sample was placed and soaked in 1L deionized water, taken out after 48h, and weighed after drying. The mass loss rate of the sample was (m0-m1) / m0×100%, and the mass loss rate of the sample was 0-1% (including 1%), indicating that the water resistance was excellent; Self-healing property: a scratch with a length of 100μm, a width of 4μm, and a depth of 0.2mm was drawn on the surface, and the initial scratch length L0 was recorded. It was kept at 70°C for 12h, and the scratch length L1 was observed under an electron microscope. The self-healing rate was calculated to be (L0-L1) / L1×100%; the test results are shown in Table 1 below;

[0086] Table 1

[0087]

[0088] The present invention provides an antistatic PET release film and a preparation method thereof. By limiting raw materials and processes, an antibacterial, water-resistant and antistatic PET release film with good mechanical strength and a self-repairing surface is prepared. In Table 1, / indicates that the item has not been tested.

[0089] Example 3 is compared with Comparative Examples 1, 2 and 3. Sodium lignin sulfonate is first grafted and modified to obtain a quaternized sodium lignin sulfonate containing both anions and cations in its molecular structure. In order to improve the stability of the quaternized sodium lignin sulfonate, the electrostatic interaction between the sulfonate group and the imidazole group is used to introduce a dihydroxy imidazole salt ionic liquid with high conductivity, high thermal stability, chemical stability and excellent water solubility. Together with the quaternized sodium lignin sulfonate, carbon nanotubes are modified by a grinding method to obtain composite carbon nanotubes. The composite carbon nanotubes are introduced into the matrix resin polyethylene terephthalate, thereby greatly improving the antistatic and antibacterial properties of the release film and greatly extending the service life of the PET release film.

[0090] Example 3 was compared with Comparative Examples 3 and 4. Polytetrahydrofuran diol, isophorone diisocyanate, and hydroxy-terminated polydimethylsiloxane were used as raw materials. Silicone prepolymer was prepared under the action of dibutyltin dilaurate as a catalyst. 2,2-Bis(hydroxymethyl)propionic acid and isosorbide were used as chain extenders. 2-Hydroxyethyl disulfide and quaternized sodium lignin sulfonate were used as end-capping agents to prepare silicone polyurethane. The hydroxy-terminated polydimethylsiloxane effectively improved the water resistance of the protective layer, and 2-Hydroxyethyl disulfide provided dynamic disulfide bonds to give the silicone polyurethane a certain self-repairing ability. The quaternized sodium lignin sulfonate gave the protective layer excellent antibacterial properties. On this basis, composite carbon nanotubes were added to improve the self-repairing ability and mechanical strength of the protective layer.

[0091] The above descriptions are only embodiments of the present invention and are not intended to limit the patent scope of the present invention. All equivalent structural changes made using the present invention specification under the inventive concept of the present invention, or direct / indirect applications in other related technical fields, are included in the patent protection scope of the present invention.

Claims

1. An antistatic PET release film, characterized in that: It comprises a composite polyester layer and a protective layer; the composite polyester layer is formed by co-extrusion of a polyester base layer and an antistatic polyester layer; the raw material composition of the antistatic polyester layer is, by weight, 70-100 parts of PET, 1-5 parts of a dispersant, 5-10 parts of a solvent, and 0.1-0.5 parts of composite carbon nanotubes; the raw material composition of the protective layer is, by weight, 18-21 parts of silicone polyurethane and 0.5-1 parts of composite carbon nanotubes; The preparation of the composite carbon nanotubes comprises the following steps: 1) Mix 3-chloro-1,2-propylene glycol and 1-methylimidazole, heat to 68-72°C and keep warm for 10-12 hours, cool, add methanol, wash with ether 3-5 times, and rotary evaporate to obtain a dihydroxy imidazole salt ionic liquid; 2) mixing carbon nanotubes, quaternized sodium lignin sulfonate, dihydroxyimidazole salt ionic liquid, methanol and deionized water, grinding, ultrasonic treatment for 1-2 hours, filtering, washing, drying and grinding to obtain composite carbon nanotubes; The preparation of the organosilicon polyurethane comprises the following steps: In a nitrogen atmosphere, the temperature of polytetrahydrofuran diol is raised to 120°C and kept for 2 hours, isophorone diisocyanate, hydroxyl-terminated polydimethylsiloxane and dibutyltin dilaurate are added, the temperature is lowered to 78-82°C and kept for 1-2 hours, a mixed solution of 2,2-bis(hydroxymethyl)propionic acid and N-methylpyrrolidone is added, stirring is continued for 5-10 minutes, isosorbide and acetone are added, stirring is continued for 2-3 hours, the temperature is lowered to 58-62°C, 2-hydroxyethyl disulfide is added, stirring is continued for 1-2 hours, quaternized sodium lignin sulfonate is added, stirring is continued for 1-2 hours, cooling is performed, deionized water is added for emulsification for 1-2 hours, rotary evaporation is performed, and the material is discharged to obtain silicone polyurethane; The preparation of the quaternized sodium lignin sulfonate comprises the following steps: mixing sodium lignin sulfonate and sodium hydroxide, heating to 83-87° C., adding (3-chloro-2-hydroxypropyl)trimethylammonium chloride, and continuing to keep the temperature for 3-4 hours to obtain the quaternized sodium lignin sulfonate.

2. An antistatic PET release film according to claim 1, characterized in that: The dispersant in the antistatic polyester layer is one of polyethylene glycol and polyvinyl pyrrolidone.

3. An antistatic PET release film according to claim 1, characterized in that: The solvent in the antistatic polyester layer is one of ethanol, N,N-dimethylformamide and N-methylpyrrolidone.

4. The antistatic PET release film according to claim 1, characterized in that: In the preparation of the composite carbon nanotubes, the mass ratio of the carbon nanotubes, the quaternized sodium lignin sulfonate, and the dihydroxyimidazole salt ionic liquid is 1:3:

1.

5. The antistatic PET release film according to claim 1, characterized in that: In the preparation of silicone polyurethane, the mass ratio of the polytetramethylene glycol, isophorone diisocyanate, and hydroxyl-terminated polydimethylsiloxane is 7.4:4.4:0.6; the mass ratio of the hydroxyl-terminated polydimethylsiloxane, 2,2-bis(hydroxymethyl)propionic acid, isosorbide, 2-hydroxyethyl disulfide, and quaternized sodium lignin sulfonate is 0.6:0.3:0.2:0.2:0.

3.

6. The method for preparing an antistatic PET release film according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1: PET is used as the polyester base material; S2: Put the dispersant, solvent and composite carbon nanotubes into a high-speed mixer, stir at 500-1000 r / min for 15-20 min, then put in PET, continue stirring for 15-20 min, and dry to obtain an antistatic polyester layer material; S3: melt-extrude the polyester base material and the antistatic polyester layer material through a double-layer co-extrusion die, cool the cast sheet, biaxially stretch, heat-set, and cool to obtain a composite polyester layer; S4: mixing the silicone polyurethane and the composite carbon nanotubes to obtain a protective coating; S5: coating the protective coating on the surface of the composite polyester layer and drying it to obtain an antistatic PET release film.

7. The method for preparing an antistatic PET release film according to claim 6, characterized in that: The working conditions of biaxial stretching are: temperature 108-110°C, stretching rate 100-110 mm / s, and transverse and longitudinal stretching ratio 2.5.