A thermal protection material and its preparation method and application
Through the thermal protection material of the laminated structure, combined with the design of buffer layer, heat insulation layer and ablation-resistant layer, the problem of poor ablation performance of existing materials in high temperature environments is solved, and the efficient thermal protection effect is achieved, which extends the The service life of the oil cylinder.
Patent Information
- Application Number
- CN202410974046.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-19
AI Technical Summary
The existing thermal protection materials are difficult to effectively resist the ablation of the oil cylinder under high temperature environments, and the preparation period is long and the curing process is slow, which limits its wide application.
Thermal protection materials with laminated structures include buffer layer, thermal insulation layer and ablation-resistant layer. The buffer layer consists of vinylphenyl polysiloxane, vinyl fluorosiloxane and flame retardant, and ablation-resistant layer By combining modified phenolic resin and modified carbon fiber, combined with silane and aluminate, a highly efficient ceramic layer is formed.
It achieves excellent oxidation and ablation performance in high temperature environments, with a linear ablation rate below 0.016mm/s, which can effectively protect the oil cylinder and extend its service life.
Abstract
Description
Technical Field
[0001] The present application relates to the field of polymer technology, and in particular to a thermal protection material and a preparation method and application thereof. Background Art
[0002] In the aerospace industry, hydraulic cylinders are crucial components, often costly to manufacture. They are primarily used to control the motion of actuators and serve as the actuating elements in hydraulic transmission and control systems. To ensure stable and sustainable operation in increasingly harsh operating environments during cylinder expansion and contraction, they require protection to isolate them from harsh environments, mitigate environmental damage, and enable reuse, thereby reducing operational costs.
[0003] When aerospace cylinders are working, they are constantly expanding and contracting, and the pistons are moving, which results in severe vibrations, internal oil pressure, and external heat flow impacts. Therefore, the external thermal protection material must be able to withstand the erosion of high heat flow and high temperature, and move with the cylinder to protect all parts without displacement or falling off.
[0004] Phenolic composites use a phenolic resin matrix reinforced with heat-resistant materials. Due to their low density, low thermal conductivity, high strength, and reliable ablation performance, they are widely used in oil cylinder linings. During the ablation process, phenolic composites not only produce penetrating pyrolysis gases, which release some heat into the atmosphere, but also form a thick carbonized layer. This carbonized layer effectively dissipates heat through radiation, preventing heat transfer to the interior. However, drawbacks such as a slow curing process, a long preparation cycle, and poor thermal protection have limited their widespread application. Summary of the Invention
[0005] The present application is made in view of the above problems, and its purpose is to provide a thermal protection material with excellent ablation resistance.
[0006] Specifically as follows, the first aspect of the present application provides a thermal protection material, comprising a buffer layer, a heat insulation layer and an ablation-resistant layer;
[0007] The buffer layer, the heat insulation layer and the ablation-resistant layer form a laminated structure;
[0008] The buffer layer includes component A, component B and component C;
[0009] The A component includes the following raw materials in parts by weight:
[0010] 50 parts of vinylphenyl polysiloxane, 5 to 10 parts of vinyl fluorosilicone, 15 to 20 parts of reinforcing agent, 20 to 25 parts of flame retardant and 15 to 25 parts of diluent;
[0011] The ablation-resistant layer includes the following raw materials in parts by weight:
[0012] 50 parts of modified phenolic resin, 5 to 10 parts of filler and 30 to 50 parts of modified carbon fiber;
[0013] The modified carbon fiber includes the following preparation raw materials:
[0014] 100 parts of carbon fiber, 10 to 20 parts of oxidant, 10 to 30 parts of silane, 10 to 20 parts of aluminate and 5 to 10 parts of tetrapropoxy zirconium.
[0015] According to some embodiments of the present application, the component B is silicone oil.
[0016] According to some embodiments of the present application, the silicone oil includes at least one of vinyl silicone oil and hydrogen-containing silicone oil.
[0017] According to some embodiments of the present application, the viscosity of the silicone oil is 100 mPa·s to 500 mPa·s.
[0018] According to some embodiments of the present application, the C component is an organometallic catalyst.
[0019] According to some embodiments of the present application, the mass ratio of component A to component B is 100:1~2.
[0020] According to some embodiments of the present application, the mass ratio of component A to component C is 100:0.1~0.4.
[0021] According to some embodiments of the present application, the reinforcing agent is fumed silica.
[0022] According to some embodiments of the present application, the flame retardant is at least one of ammonium polyphosphate, magnesium hydroxide, aluminum hydroxide, antimony trioxide and melamine;
[0023] According to some embodiments of the present application, the diluent is toluene or 200# solvent.
[0024] According to some embodiments of the present application, the thermal insulation layer includes the following raw materials in parts by weight:
[0025] 40 parts of modified phenolic resin, 10 to 20 parts of thermal insulation filler and 40 to 50 parts of reinforcing material.
[0026] According to some embodiments of the present application, the modified phenolic resin selected for the thermal insulation layer includes the following raw materials in parts by weight:
[0027] 30 parts of boric acid phenol ester, 40 parts to 50 parts of formaldehyde and 20 parts to 40 parts of cardanol.
[0028] According to some embodiments of the present application, the thermal insulation filler includes at least one of hollow glass microspheres, hollow ceramic microspheres, cork powder and vermiculite.
[0029] According to some embodiments of the present application, the reinforcing material includes glass fiber woven cloth.
[0030] According to some embodiments of the present application, the modified phenolic resin selected for the ablation-resistant layer includes the following raw materials in parts by weight:
[0031] 30 parts of boric acid phenol ester, 40 parts to 50 parts of formaldehyde and 20 parts to 40 parts of cardanol.
[0032] According to some embodiments of the present application, the filler includes at least one of silicon carbide and zirconium diboride.
[0033] According to some embodiments of the present application, the oxidant is nitric acid.
[0034] According to some embodiments of the present application, the silane is heptadecafluorodecyltriethoxysilane.
[0035] According to some embodiments of the present application, the aluminate is at least one of triisopropyl aluminate and tribenzyl aluminate.
[0036] According to some embodiments of the present application, the linear ablation rate of the thermal protection material is below 0.016 mm / s.
[0037] According to some embodiments of the present application, the vinylphenyl polysiloxane is a vinyl-terminated polyphenylsiloxane.
[0038] The second aspect of the present application discloses a method for preparing the thermal protection material of the first aspect of the present application, comprising the following steps:
[0039] The buffer layer, the heat insulation layer and the ablation-resistant layer are compounded.
[0040] According to some embodiments of the present application, the method for preparing the modified carbon fiber comprises the following steps:
[0041] The carbon fibers are oxidized by using an oxidant to obtain oxidized carbon fibers;
[0042] Oxidized carbon fibers, silane, aluminate and tetrapropoxy zirconium are mixed, dried and calcined.
[0043] According to some embodiments of the present application, the calcination temperature is 100°C to 200°C.
[0044] According to some embodiments of the present application, the calcination atmosphere is a protective gas.
[0045] The third aspect of the present application discloses the use of the above-mentioned thermal protection material in the preparation of thermal protection components.
[0046] According to one of the technical solutions of this application, at least the following beneficial effects are achieved:
[0047] The thermal protection material in the present application includes a buffer layer, a heat insulation layer and an ablation-resistant layer; the buffer layer is prepared using vinylphenyl polysiloxane and vinyl fluorosilicone as raw materials, and vinylphenyl polysiloxane and vinyl fluorosilicone form silicone rubber under certain conditions. Silicone rubber has excellent temperature resistance and maintains a flexible state within a certain temperature range, thus being able to play an excellent buffering role.
[0048] The buffer layer in this application is primarily based on phenyl silicone resin, combined with vinyl fluorosilicone, a reinforcing agent, a flame retardant, and a diluent. Due to the structural characteristics of silicone resin, it possesses high strength and excellent cushioning properties. The addition of component B adjusts the fluidity of the buffer layer, facilitating construction operations. The addition of the flame retardant imparts excellent flame retardancy to the buffer layer.
[0049] The ablation-resistant layer uses phenolic resin as the matrix material, which maintains its structural integrity and dimensional stability in a high-temperature environment, and has a high residual carbon rate after thermal decomposition; this application also uses modified carbon fiber and modified phenolic resin in combination, and uses silane, aluminate and tetrapropoxy zirconium to modify the carbon fiber, further improving the compatibility of the modified carbon fiber and modified phenolic resin, thereby forming a well-formed ablation-resistant layer.
[0050] The modified carbon fiber of the present application decomposes to form silicon oxide, zirconium oxide and aluminum oxide during the high-temperature ablation process, forming a uniform ceramic layer on the surface of the modified carbon fiber. At the same time, the melting and volatilization of silicon oxide effectively consumes heat, and the good oxygen barrier and heat insulation capabilities of zirconium oxide itself further improve the anti-oxidation and ablation performance of the modified carbon fiber material; and the aluminum oxide uniformly dispersed in the modified phenolic resin can also increase the heat resistance of the ablation-resistant layer to a certain extent; during the ablation process, the phenolic resin and silane ceramics are converted into dense SiC, which effectively increases the resistance of the ablation surface to high-temperature oxidation and high-temperature particle erosion, further improving the ablation resistance; therefore, the thermal protection material of the present application has excellent anti-oxidation and ablation performance, and can meet the ablation protection requirements under high-temperature and high-speed combustion service conditions. DETAILED DESCRIPTION
[0051] In order to make the purpose, technical solutions and advantages of this application more clearly understood, the present application is described and illustrated below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are merely used to explain this application and are not intended to limit this application. Based on the embodiments provided in this application, all other embodiments obtained by those of ordinary skill in the art without making any creative work are within the scope of protection of this application.
[0052] Obviously, the following descriptions are merely some examples or embodiments of the present application. Those skilled in the art can apply the present application to other similar scenarios without inventive effort. Furthermore, it is also understood that, although the effort involved in such a development process may be complex and lengthy, for those skilled in the art related to the content disclosed in the present application, changes in design, manufacturing, or production based on the technical content disclosed in the present application are merely conventional technical means and should not be construed as an insufficiency of the content disclosed in the present application.
[0053] However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters or repeated descriptions of substantially identical structures may be omitted. This is to avoid unnecessary redundancy in the following description and to facilitate understanding by those skilled in the art. Furthermore, the following description is provided to enable those skilled in the art to fully understand this application and is not intended to limit the subject matter recited in the claims.
[0054] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0055] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0056] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0057] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0058] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0059] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0060] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.
[0061] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0062] Specifically as follows, the first aspect of the present application provides a thermal protection material, comprising a buffer layer, a heat insulation layer and an ablation-resistant layer;
[0063] The buffer layer, the heat insulation layer and the ablation-resistant layer form a laminated structure;
[0064] The buffer layer includes component A, component B and component C;
[0065] The A component includes the following raw materials in parts by weight:
[0066] 50 parts of vinylphenyl polysiloxane, 5 to 10 parts of vinyl fluorosilicone, 15 to 20 parts of reinforcing agent, 20 to 25 parts of flame retardant and 15 to 25 parts of diluent;
[0067] The ablation-resistant layer includes the following raw materials in parts by weight:
[0068] 50 parts of modified phenolic resin, 5 to 10 parts of filler and 30 to 50 parts of modified carbon fiber;
[0069] The modified carbon fiber includes the following preparation raw materials:
[0070] 100 parts of carbon fiber, 10 to 20 parts of oxidant, 10 to 30 parts of silane, 10 to 20 parts of aluminate and 5 to 10 parts of tetrapropoxy zirconium.
[0071] According to some embodiments of the present application, the component B is silicone oil.
[0072] According to some embodiments of the present application, the silicone oil includes at least one of vinyl silicone oil and hydrogen-containing silicone oil.
[0073] According to some embodiments of the present application, the viscosity of the silicone oil is 100 mPa·s to 500 mPa·s.
[0074] According to some embodiments of the present application, the C component is an organometallic catalyst.
[0075] According to some embodiments of the present application, the mass ratio of component A to component B is 100:1~2.
[0076] According to some embodiments of the present application, the mass ratio of component A to component C is 100:0.1~0.4.
[0077] According to some embodiments of the present application, the reinforcing agent is fumed silica.
[0078] According to some embodiments of the present application, the flame retardant is at least one of ammonium polyphosphate, magnesium hydroxide, aluminum hydroxide, antimony trioxide and melamine;
[0079] According to some embodiments of the present application, the diluent is toluene or 200# solvent.
[0080] According to some embodiments of the present application, the thermal insulation layer includes the following raw materials in parts by weight:
[0081] 40 parts of modified phenolic resin, 10 to 20 parts of thermal insulation filler and 40 to 50 parts of reinforcing material.
[0082] According to some embodiments of the present application, the modified phenolic resin selected for the thermal insulation layer includes the following raw materials in parts by weight:
[0083] 30 parts of boric acid phenol ester, 40 parts to 50 parts of formaldehyde and 20 parts to 40 parts of cardanol.
[0084] According to some embodiments of the present application, the thermal insulation filler includes at least one of hollow glass microspheres, hollow ceramic microspheres, cork powder and vermiculite.
[0085] According to some embodiments of the present application, the reinforcing material includes glass fiber woven cloth.
[0086] According to some embodiments of the present application, the modified phenolic resin selected for the ablation-resistant layer includes the following raw materials in parts by weight:
[0087] 30 parts of boric acid phenol ester, 40 parts to 50 parts of formaldehyde and 20 parts to 40 parts of cardanol.
[0088] According to some embodiments of the present application, the filler includes at least one of silicon carbide and zirconium diboride.
[0089] According to some embodiments of the present application, the oxidant is nitric acid.
[0090] According to some embodiments of the present application, the silane is heptadecafluorodecyltriethoxysilane.
[0091] According to some embodiments of the present application, the aluminate is at least one of triisopropyl aluminate and tribenzyl aluminate.
[0092] According to some embodiments of the present application, the linear ablation rate of the thermal protection material is below 0.016 mm / s.
[0093] The second aspect of the present application discloses a method for preparing the thermal protection material of the first aspect of the present application, comprising the following steps:
[0094] The buffer layer, the heat insulation layer and the ablation-resistant layer are compounded.
[0095] According to some embodiments of the present application, the method for preparing the modified carbon fiber comprises the following steps:
[0096] The carbon fibers are oxidized by using an oxidant to obtain oxidized carbon fibers;
[0097] Oxidized carbon fibers, silane, aluminate and tetrapropoxy zirconium are mixed, dried and calcined.
[0098] According to some embodiments of the present application, the calcination temperature is 100°C to 200°C.
[0099] According to some embodiments of the present application, the calcination atmosphere is a protective gas.
[0100] The third aspect of the present application discloses the use of the above-mentioned thermal protection material in the preparation of thermal protection components.
[0101] According to one of the technical solutions of this application, at least the following beneficial effects are achieved:
[0102] Vinylphenyl polysiloxane and vinyl fluorosilicone are used as raw materials for preparation, and vinylphenyl polysiloxane and vinyl fluorosilicone form silicone rubber under certain conditions. Silicone rubber has excellent temperature resistance and maintains a flexible state within a certain temperature range, so it can play an excellent buffering role.
[0103] The buffer layer in this application is primarily based on phenyl silicone resin, combined with vinyl fluorosilicone, a reinforcing agent, a flame retardant, and a diluent. Due to the structural characteristics of silicone resin, it possesses high strength and excellent cushioning properties. The addition of component B adjusts the fluidity of the buffer layer, facilitating construction operations. The addition of the flame retardant imparts excellent flame retardancy to the buffer layer.
[0104] The ablation-resistant layer uses phenolic resin as the matrix material, which maintains its structural integrity and dimensional stability in a high-temperature environment, and has a high residual carbon rate after thermal decomposition; this application also uses modified carbon fiber and modified phenolic resin in combination, and uses silane, aluminate and tetrapropoxy zirconium to modify the carbon fiber, further improving the compatibility of the modified carbon fiber and modified phenolic resin, thereby forming a well-formed ablation-resistant layer.
[0105] The modified carbon fiber of the present application decomposes to form silicon oxide, zirconium oxide and aluminum oxide during the high-temperature ablation process, forming a uniform ceramic layer on the surface of the modified carbon fiber. At the same time, the melting and volatilization of silicon oxide effectively consumes heat, and the good oxygen barrier and heat insulation capabilities of zirconium oxide itself further improve the anti-oxidation and ablation performance of the modified carbon fiber material; and the aluminum oxide uniformly dispersed in the modified phenolic resin can also increase the heat resistance of the ablation-resistant layer to a certain extent; during the ablation process, the phenolic resin and silane ceramics are converted into dense SiC, which effectively increases the resistance of the ablation surface to high-temperature oxidation and high-temperature particle erosion, further improving the ablation resistance; therefore, the thermal protection material of the present application has excellent anti-oxidation and ablation performance, and can meet the ablation protection requirements under high-temperature and high-speed combustion service conditions.
[0106] The following is a further detailed description of the thermal protection material and preparation method of the present application, with reference to specific examples. The present application can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to facilitate a more thorough and comprehensive understanding of the present disclosure.
[0107] The manufacturers and models of some of the raw materials used in the examples and comparative examples of this application are as follows:
[0108] Vinylphenyl polysiloxane: vinyl terminated polyphenylsiloxane (CAS No.: 225927-21-9);
[0109] Vinyl fluorosilicone: Vinyl-terminated fluorinated polysiloxane, Shanghai Guishan Polymer Materials Co., Ltd. (model FSY-780);
[0110] Fumed silica: Cabot TS-720;
[0111] Silicone oil: hydrogen-terminated silicone oil, Jiangsu Keqi Polymer Materials Co., Ltd., product model: D-100, viscosity 160 mPa·s;
[0112] Organometallic catalyst: divinyltetramethyldisiloxane platinum complex (platinum catalyst) (CAS No.: 68478-92-2);
[0113] Glass hollow microspheres: Zhengzhou Shenglait Hollow Microsphere New Materials Co., Ltd., hollow glass microspheres HL20.
[0114] Cork powder: Lingshou County Shengxiang Mineral Products Co., Ltd. (average particle size 200 μm);
[0115] Glass fiber cloth: Hejian Yuanchuang Insulation Materials Co., Ltd., anti-deformation glass fiber cloth, thickness 2mm;
[0116] Oxidant: nitric acid solution (60% by mass).
[0117] Carbon fiber: Japan Toray T300B-1000.
[0118] Example 1
[0119] This embodiment is a thermal protection material, which consists of a buffer layer, a heat insulation layer and an ablation-resistant layer;
[0120] The buffer layer, the heat insulation layer and the ablation-resistant layer form a laminated structure;
[0121] The buffer layer consists of component A, component B (silicone oil) and component C (organic metal catalyst);
[0122] The mass ratio of component A, component B and component C is 100:1:0.3;
[0123] Component A is composed of the following raw materials in parts by mass:
[0124] 50 parts of vinylphenyl polysiloxane, 8 parts of vinyl fluorosilicone, 15 parts of reinforcing agent (fumed silica), 23 parts of flame retardant (8 parts of magnesium hydroxide, 3 parts of antimony trioxide, 12 parts of aluminum hydroxide) and 25 parts of diluent (200# gasoline, i.e. 200# solvent gasoline);
[0125] The preparation method of the buffer layer in this embodiment comprises the following steps:
[0126] The raw materials for preparing component A were mixed and stirred at 1200 rpm / min for 1.5 h to prepare component A;
[0127] Components A, B and C are then mixed and coated to prepare a buffer layer.
[0128] The heat-insulating layer is composed of the following raw materials in parts by weight:
[0129] 40 parts of modified phenolic resin, 15 parts of thermal insulation filler (7 parts of hollow glass microspheres and 8 parts of cork powder thermal insulation filler) and 45 parts of reinforcing material (glass fiber cloth).
[0130] The modified phenolic resin comprises the following raw materials in parts by weight:
[0131] 30 parts of boric acid phenol ester, 40 parts of formaldehyde and 30 parts of cardanol.
[0132] The preparation method of the modified phenolic resin in the thermal insulation layer of this embodiment comprises the following steps:
[0133] 40 parts of p-phenol, 5 parts of boric acid, 45 parts of toluene and 2 parts of oxalic acid were mixed, heated to 120°C, refluxed to remove water, reacted for 5 hours, and then cooled to below 60°C to obtain boric acid phenol ester.
[0134] Then, 30 parts of boric acid phenol ester, 40 parts of formaldehyde (added in the form of a 37% formaldehyde aqueous solution by mass) and 30 parts of cardanol were mixed, heated to 120°C, refluxed to separate water, and refluxed at a constant temperature for 3 hours to obtain a modified phenolic resin.
[0135] The ablation-resistant layer is composed of the following raw materials in parts by weight:
[0136] 50 parts of modified phenolic resin, 10 parts of filler (5 parts of silicon carbide (D50 is 3 μm) and 5 parts of zirconium diboride (D50 is 3 μm)) and 40 parts of modified carbon fiber;
[0137] The preparation method of the modified phenolic resin in the ablation-resistant layer in this embodiment comprises the following steps:
[0138] 40 parts of p-phenol, 5 parts of boric acid, 45 parts of toluene and 2 parts of oxalic acid were mixed, heated to 120°C, refluxed to remove water, reacted for 5 hours, and then cooled to below 60°C to obtain boric acid phenol ester.
[0139] Then, 30 parts of boric acid phenol ester, 45 parts of formaldehyde (added in the formaldehyde aqueous solution with a mass fraction of 37%, the actual mass fraction of formaldehyde added is 45 parts) and 35 parts of cardanol were mixed and heated to 120°C, refluxed to separate water, and refluxed at a constant temperature for 3 hours to obtain a modified phenolic resin.
[0140] The modified carbon fiber includes the following raw materials in parts by weight:
[0141] 100 parts of carbon fiber, 20 parts of oxidant, 20 parts of silane (heptadecafluorodecyltriethoxysilane), 15 parts of aluminate (the mass ratio of triisopropyl aluminate and tribenzyl aluminate is 1:1) and 8 parts of tetrapropoxy zirconium.
[0142] The preparation method of modified carbon fiber consists of the following steps:
[0143] S1. Silane, aluminate, tetrapropoxy zirconium and anhydrous ethanol (the mass ratio of silane to anhydrous ethanol is 1:1) are mixed, refluxed at 110°C for 20 hours, and then aged for 5 hours to obtain a modified solution;
[0144] S2, mixing carbon fiber and nitric acid solution (mass fraction 60%) and treating at 80°C for 2h, washing, and drying to obtain oxidized carbon fiber;
[0145] S3. Coating the modified liquid on the surface of the oxidized carbon fiber to obtain modified carbon fiber.
[0146] The method for preparing the heat-insulating layer and the ablation-resistant layer in this embodiment comprises the following steps:
[0147] The thermal insulation filler and the cardanol-modified phenolic resin were mixed, coated on the surface of the reinforcement material, and dried at 80° C. for 5 hours to obtain a thermal insulation material.
[0148] The filler, modified carbon fiber and modified resin were mixed and dried at 80° C. for 5 hours to obtain an ablation-resistant material.
[0149] After the buffer layer, thermal insulation material and ablation-resistant material are stacked, they are preheated at 95°C for 30 minutes, slowly pressurized and heated (heating rate is 5°C / min), and kept warm and pressurized at 25Mpa and 175°C for 2 hours to obtain a thermal protection material.
[0150] Example 2
[0151] This embodiment is a heat protection material and a preparation method thereof, which differs from Example 1 in that:
[0152] Component A is composed of the following raw materials in parts by mass:
[0153] 50 parts of vinylphenyl polysiloxane, 8 parts of vinyl fluorosilicone, 15 parts of reinforcing agent (fumed silica), 21 parts of flame retardant (8 parts of ammonium polyphosphate, 3 parts of antimony trioxide, 10 parts of aluminum hydroxide) and 25 parts of diluent (200# gasoline);
[0154] The modified carbon fiber includes the following raw materials in parts by weight:
[0155] 100 parts of carbon fiber, 15 parts of oxidant, 10 parts of silane (heptadecafluorodecyltriethoxysilane), 20 parts of aluminate (the mass ratio of triisopropyl aluminate and tribenzyl aluminate is 1:1) and 5 parts of tetrapropoxy zirconium.
[0156] The preparation method of modified carbon fiber consists of the following steps:
[0157] S1. Silane, aluminate, tetrapropoxy zirconium and anhydrous ethanol (the mass ratio of silane to anhydrous ethanol is 1:1) are mixed, refluxed at 110°C for 20 hours, and then aged for 5 hours to obtain a modified solution;
[0158] S2, mixing carbon fiber and nitric acid solution (mass fraction 60%) and treating at 80°C for 2h, washing, and drying to obtain oxidized carbon fiber;
[0159] S3. Coating the modified liquid on the surface of the oxidized carbon fiber to obtain modified carbon fiber.
[0160] Example 3
[0161] This embodiment is a heat protection material and a preparation method thereof, which differs from Example 1 in that:
[0162] Component A is composed of the following raw materials in parts by mass:
[0163] 50 parts of vinylphenyl polysiloxane, 10 parts of vinyl fluorosilicone, 15 parts of reinforcing agent (fumed silica), 23 parts of flame retardant (8 parts of magnesium hydroxide, 3 parts of antimony trioxide, 12 parts of aluminum hydroxide) and 25 parts of diluent (200# gasoline);
[0164] The modified carbon fiber includes the following raw materials in parts by weight:
[0165] 100 parts of carbon fiber, 10 parts of oxidant, 30 parts of silane (heptadecafluorodecyltriethoxysilane), 10 parts of aluminate (the mass ratio of triisopropyl aluminate and tribenzyl aluminate is 1:1) and 5 parts of tetrapropoxy zirconium.
[0166] The preparation method of modified carbon fiber consists of the following steps:
[0167] S1. Silane, aluminate, tetrapropoxy zirconium and anhydrous ethanol (the mass ratio of silane to anhydrous ethanol is 1:1) are mixed, refluxed at 110°C for 20 hours, and then aged for 5 hours to obtain a modified solution;
[0168] S2, mixing carbon fiber and nitric acid solution (mass fraction 60%) and treating at 80°C for 2h, washing, and drying to obtain oxidized carbon fiber;
[0169] S3. Coating the modified liquid on the surface of the oxidized carbon fiber to obtain modified carbon fiber.
[0170] Example 4
[0171] This embodiment is a heat protection material and a preparation method thereof, which differs from Example 1 in that:
[0172] Modified carbon fiber includes the following preparation raw materials:
[0173] 100 parts of carbon fiber, 12 parts of oxidant, 28 parts of silane (heptadecafluorodecyltriethoxysilane), 15 parts of aluminate (triisopropyl aluminate) and 6 parts of tetrapropoxy zirconium.
[0174] The preparation method of modified carbon fiber consists of the following steps:
[0175] S1. Silane, aluminate, tetrapropoxy zirconium and anhydrous ethanol (the mass ratio of silane to anhydrous ethanol is 1:1) are mixed, refluxed at 110°C for 20 hours, and then aged for 5 hours to obtain a modified solution;
[0176] S2, mixing carbon fiber and nitric acid solution (mass fraction 60%) and treating at 80°C for 2h, washing, and drying to obtain oxidized carbon fiber;
[0177] S3. Coating the modified liquid on the surface of the oxidized carbon fiber to obtain modified carbon fiber.
[0178] Example 5
[0179] This embodiment is a heat protection material and a preparation method thereof, which differs from Example 1 in that:
[0180] Modified carbon fiber includes the following preparation raw materials:
[0181] 100 parts of carbon fiber, 12 parts of oxidant, 28 parts of silane (heptadecafluorodecyltriethoxysilane), 15 parts of aluminate (tribenzyl aluminate) and 6 parts of tetrapropoxyzirconium.
[0182] The preparation method of modified carbon fiber consists of the following steps:
[0183] S1. Silane, aluminate, tetrapropoxy zirconium and anhydrous ethanol (the mass ratio of silane to anhydrous ethanol is 1:1) are mixed, refluxed at 110°C for 20 hours, and then aged for 5 hours to obtain a modified solution;
[0184] S2, mixing carbon fiber and nitric acid solution (mass fraction 60%) and treating at 80°C for 2h, washing, and drying to obtain oxidized carbon fiber;
[0185] S3. Coating the modified liquid on the surface of the oxidized carbon fiber to obtain modified carbon fiber.
[0186] Comparative Example 1
[0187] This comparative example is a heat protection material and its preparation method, which differs from Example 1 in that:
[0188] The ablation-resistant layer is composed of the following raw materials in parts by weight:
[0189] 50 parts of modified phenolic resin, 10 parts of filler (5 parts of silicon carbide (D50 is 3 μm) and 5 parts of zirconium diboride (D50 is 3 μm)) and 40 parts of carbon fiber.
[0190] Comparative Example 2
[0191] This comparative example is a heat protection material and its preparation method, which differs from Example 1 in that:
[0192] The modified carbon fiber includes the following raw materials in parts by weight:
[0193] 100 parts of carbon fiber and 20 parts of oxidant.
[0194] The preparation method of modified carbon fiber consists of the following steps:
[0195] The carbon fibers were mixed with a nitric acid solution (60% by mass) and treated at 80°C for 2 hours, followed by washing and drying to obtain modified carbon fibers.
[0196] Comparative Example 3
[0197] This comparative example is a heat protection material and its preparation method, which differs from Example 1 in that:
[0198] The modified carbon fiber includes the following raw materials in parts by weight:
[0199] 100 parts of carbon fibers, 20 parts of oxidant, 20 parts of silane (heptadecafluorodecyltriethoxysilane) and 8 parts of tetrapropoxyzirconium.
[0200] The preparation method of modified carbon fiber consists of the following steps:
[0201] S1. Mix silane, tetrapropoxy zirconium and anhydrous ethanol (the mass ratio of silane to anhydrous ethanol is 1:1), reflux at 110°C for 20 hours, and then allow to stand for 5 hours to obtain a modified solution;
[0202] S2, mixing carbon fiber and nitric acid solution (mass fraction 60%) and treating at 80°C for 2h, washing, and drying to obtain oxidized carbon fiber;
[0203] S3. Coating the modified liquid on the surface of the oxidized carbon fiber to obtain modified carbon fiber.
[0204] Comparative Example 4
[0205] This comparative example is a heat protection material and its preparation method, which differs from Example 1 in that:
[0206] The modified carbon fiber includes the following raw materials in parts by weight:
[0207] 100 parts of carbon fiber, 20 parts of oxidant, 15 parts of aluminate (the mass ratio of triisopropyl aluminate and tribenzyl aluminate is 1:1) and 8 parts of tetrapropoxy zirconium.
[0208] The preparation method of modified carbon fiber consists of the following steps:
[0209] S1. Aluminate, tetrapropoxy zirconium and anhydrous ethanol (the mass ratio of aluminate to anhydrous ethanol is 1:1) are mixed, refluxed at 110°C for 20 hours, and then aged for 5 hours to obtain a modified solution;
[0210] S2, mixing carbon fiber and nitric acid solution (mass fraction 60%) and treating at 80°C for 2h, washing, and drying to obtain oxidized carbon fiber;
[0211] S3. Coating the modified liquid on the surface of the oxidized carbon fiber to obtain modified carbon fiber.
[0212] Comparative Example 5
[0213] This comparative example is a heat protection material and its preparation method, which differs from Example 1 in that:
[0214] The modified carbon fiber includes the following raw materials in parts by weight:
[0215] 100 parts of carbon fiber, 20 parts of oxidant and 20 parts of silane (heptadecafluorodecyltriethoxysilane).
[0216] The preparation method of modified carbon fiber consists of the following steps:
[0217] S1. Mix silane and anhydrous ethanol (the mass ratio of silane to anhydrous ethanol is 1:1), reflux at 110°C for 20 hours, and then allow to stand for 5 hours to obtain a modified solution;
[0218] S2, mixing carbon fiber and nitric acid solution (mass fraction 60%) and treating at 80°C for 2h, washing, and drying to obtain oxidized carbon fiber;
[0219] S3. Coating the modified liquid on the surface of the oxidized carbon fiber to obtain modified carbon fiber.
[0220] The present application performs the following performance tests on the embodiments and comparative examples:
[0221] Thermal protection component (buffer layer in direct contact with the cylinder) performance test, operating conditions: 12Mw / m 2 , lasting 3s-5s, while the high-speed movement of the cylinder piston brings vibration and impact to the thermal protection material, and the linear ablation rate and the surface temperature of the cylinder are tested. The test results are shown in Table 1;
[0222] .
[0223] The difference between Comparative Example 1 and Example 1 is that the carbon fibers are not modified, and silicon oxide, zirconium oxide, aluminum oxide and silicon carbide cannot be introduced; therefore, the ablation resistance is poor.
[0224] The difference between Comparative Example 2 and Example 1 is that the carbon fibers are only subjected to oxidation treatment, which can improve the compatibility of the carbon fibers with the phenolic resin; thus, the performance is slightly improved compared to Comparative Example 1.
[0225] The difference between Comparative Example 3 and Example 1 is that the carbon fibers are not modified with aluminate and thus cannot form aluminum oxide, thereby affecting the ablation resistance.
[0226] The difference between Comparative Example 4 and Example 1 is that the carbon fibers are not modified with silicate, which results in the inability to form silicon oxide and silicon carbide, resulting in poor ablation resistance.
[0227] The difference between Comparative Example 1 and Example 1 is that the carbon fiber is not modified with tetrapropoxy zirconium and cannot form zirconium oxide, resulting in poor ablation resistance.
[0228] From the data in the above table, it can be seen that the thermal protection material in the embodiment has excellent ablation resistance. The thermal protection material in the embodiment of the present application can make the cylinder operate safely and stably in a harsh and demanding environment, while extending its service life; the thermal protection material of the present application is composed of three functional layers - a buffer layer, a heat insulation layer, and an ablation-resistant layer, which integrates the characteristics of multiple materials to jointly provide thermal protection for aerospace cylinders; the silicone rubber of the buffer layer of the present application has good flexibility and elasticity, which offsets the extrusion force of the outer rigid structure due to heat deformation on the aviation cylinder. At the same time, it can withstand temperatures for a long time, and has good toughness and ductility at both low and high temperatures; the ablation-resistant layer has good ablation resistance, and at 12Mw / m 2 Under the heat flow condition, the linear ablation rate is ≤0.016mm / s.
[0229] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and any embodiments having substantially the same structure and effect as the technical concept within the scope of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the present application, any other embodiments that can be conceived by those skilled in the art and that combine some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A thermal protection material, characterized in that: It includes a buffer layer, a heat insulation layer and an ablation-resistant layer; The buffer layer, the heat insulation layer and the ablation-resistant layer form a laminated structure; The buffer layer includes component A, component B and component C; The A component includes the following raw materials in parts by weight: 50 parts of vinyl phenyl polysiloxane, 5 to 10 parts of vinyl fluorosilicone, 15 to 20 parts of reinforcing agent, 20 to 25 parts of flame retardant and 15 to 25 parts of diluent; The B component is silicone oil; The C component is an organic metal catalyst; The thermal insulation layer comprises the following raw materials in parts by weight: 40 parts of modified phenolic resin, 10 to 20 parts of thermal insulation filler and 40 to 50 parts of reinforcing material; The modified phenolic resin used in the thermal insulation layer includes the following raw materials in parts by weight: 30 parts of boric acid phenol ester, 40 parts to 50 parts of formaldehyde and 20 parts to 40 parts of cardanol; The ablation-resistant layer comprises the following raw materials in parts by weight: 50 parts of modified phenolic resin, 5 parts of silicon carbide, 5 parts of zirconium diboride and 40 parts of modified carbon fiber; The modified phenolic resin selected for the ablation-resistant layer includes the following raw materials in parts by weight: 30 parts of boric acid phenol ester, 40 to 50 parts of formaldehyde and 20 to 40 parts of cardanol; The modified carbon fiber comprises the following preparation raw materials: 100 parts of carbon fiber, 10 to 20 parts of oxidant, 10 to 30 parts of silane, 10 to 20 parts of aluminate and 5 to 10 parts of tetrapropoxy zirconium; The aluminate is at least one of triisopropyl aluminate and tribenzyl aluminate; The silane is heptadecafluorodecyltriethoxysilane; The vinylphenyl polysiloxane is a vinyl terminated polyphenyl siloxane; The method for preparing the modified carbon fiber comprises the following steps: The carbon fiber is oxidized by using an oxidant to obtain an oxidized carbon fiber; The oxidized carbon fiber, silane, aluminate and tetrapropoxy zirconium are mixed, dried and calcined; The calcination temperature is 100°C to 200°C; The calcination atmosphere is protective gas.
2. The heat protection material according to claim 1, characterized in that: The silicone oil comprises at least one of vinyl silicone oil and hydrogen-containing silicone oil; And / or, the viscosity of the silicone oil is 100 mPa·s to 500 mPa·s; And / or, the mass ratio of component A to component B is 100:1-2; And / or, the mass ratio of component A to component C is 100:0.1-0.
4.
3. The heat protection material according to claim 1, characterized in that: The reinforcing agent is fumed silica; and / or, the flame retardant is at least one of ammonium polyphosphate, magnesium hydroxide, aluminum hydroxide, antimony trioxide and melamine; And / or, the diluent is toluene or 200# gasoline.
4. The heat protection material according to claim 1, characterized in that: The heat-insulating filler comprises at least one of hollow glass microspheres, hollow ceramic microspheres, cork powder and vermiculite; And / or, the reinforcing material comprises glass fiber woven cloth.
5. The heat protection material according to claim 1, characterized in that: The oxidant is nitric acid.
6. The heat protection material according to claim 1, characterized in that: The linear ablation rate of the thermal protection material is below 0.016 mm / s.
7. A method for preparing a heat protection material according to any one of claims 1 to 6, characterized in that: The following steps are involved: The buffer layer, the heat insulation layer and the ablation-resistant layer are compounded.