A high-performance polyetheretherketone (PEEK) fine synthesis process

Through the acylation and hydrolysis reaction of high-purity 4,4'-difluorobenzophenone, combined with finely controlled polymerization process and nitrogen replacement, the problems of unstable performance and impurities of PEEK materials are solved, and the high polymerization of high Purity and narrow molecular weight distribution meet the performance requirements of high-end applications.

CN118515863BActive Publication Date: 2024-11-19JIANGSU HENGFENGLONG NEW MATERIALS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410985421.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-19
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

Existing polyether ether ketone (PEEK) materials have problems of performance instability and impurities in high-end applications, especially performance fluctuations and increased conductivity caused by wide molecular weight distribution and impurities residues, which affect their aerospace, medical devices and Applications in the electrical field.

Method used

High-purity 4,4'-difluorobenzophenone is used as polymerized monomer to generate high-purity polymerized monomers through the acylation and hydrolysis reaction of non-metallic catalysts, and the temperature and pressure are finely controlled during the polymerization process, and nitrogen replacement is used. Remove oxygen impurities, combine the torque sensor to determine the polymerization end point and supercritical carbon dioxide extraction for purification, avoiding the use of additional capping agents and molecular weight regulators.

Benefits of technology

It significantly improves the thermal stability, mechanical properties and purity of PEEK materials, narrows the molecular weight distribution range, enhances its reliability and performance stability in high-end applications, reduces the impact of impurities, and meets the aerospace, medical devices and electrical fields. high-end design requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118515863B_ABST
    Figure CN118515863B_ABST
Patent Text Reader

Abstract

The invention discloses a high-performance polyetheretherketone (PEEK) fine synthesis process. Starting from a polymerization raw material, a high-purity polymerization monomer 4,4'-difluorobenzophenone (4,4'-DFBP) is prepared by using a non-metallic catalyst, so as to ensure the stable performance of the synthesized polyetheretherketone molecules from the source; and the influence of pressure on the molecular weight of the polymer during the polymerization process is paid attention to, the temperature increase program is more carefully controlled, and the pressure is increased with the gradient temperature increase, so as to control the growth rate of the polymer chain and the distribution of the molecular weight, balance the material-liquid ratio of 4,4'-difluorobenzophenone and diphenyl sulfone in the polymerization stage, so as to make the polymerization reaction more uniform and controllable, ensure the regularity of the polymer molecular chain, realize the narrowing of the molecular weight distribution range, make the polymer have more consistent physical and chemical properties, improve the product quality, meet the high-end design requirements in the fields of aerospace, medical equipment and electrical applications, and have good economic value and application value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of high molecular polymer synthesis, and specifically relates to a high-performance polyetheretherketone (PEEK) fine synthesis process. Background Art

[0002] Polyetheretherketone (PEEK) is a high-performance special engineering plastic whose main chain structure consists of repeating units of one ketone bond and two ether bonds. This structure gives PEEK excellent physical and chemical properties. The long-term use temperature of PEEK can reach 250-260°C, and the short-term use temperature can even reach 300°C. In addition, PEEK also has good self-lubricity and excellent processing properties, which makes it have broad application prospects in aerospace, medical equipment, electrical applications and other fields. However, the existing PEEK materials still have the problem of unstable performance in some high-end applications. This is mainly attributed to the wide molecular weight distribution of the material, which leads to fluctuations in mechanical properties, and the molecular chains of the low molecular weight part are susceptible to chemical attacks, affecting the chemical resistance of the material.

[0003] In order to solve these problems, researchers have tried to control the molecular weight distribution by end-capping agents or adding molecular weight regulators to improve the performance stability and reliability of PEEK. For example, the polyetheretherketone and its preparation method disclosed in Chinese patent document CN102250299B use 2,5-di-tert-butylhydroquinone as an end-capping agent, which can effectively control the end point of the polymerization reaction and improve the quality of the final product. Another Chinese patent document CN103467681B discloses a method for synthesizing a high thermal stability polyetheretherketone resin, which suppresses phenoxy branching and ensures the regularity of the molecular chain of the polymer by adding a molecular weight regulator 4,4'-dihydroxybenzophenone, thereby improving the thermal stability and mechanical properties of PEEK.

[0004] However, impurities in 4,4'-DFBP, a key monomer for synthesizing PEEK, especially non-metallic impurities and metal residues, have a significant impact on the performance of PEEK materials. Non-metallic impurities will introduce defects during the polymerization of PEEK chains, affecting the stability of the molecular chains, while metal residues will cause cross-linking of PEEK chains, resulting in oversized chain segments, affecting the stability of product performance. At the same time, metal residues may also increase the conductivity of PEEK, affecting its application in the electrical field. Therefore, in order to obtain high-quality PEEK, in addition to controlling the molecular weight distribution, it is also necessary to ensure the high purity of the polymerized monomers.

[0005] In addition, there are some potential defects in controlling the molecular weight distribution by using additional end-capping agents or adding molecular weight regulators. End-capping agents may reduce the end group activity of the polymer, affect its reactivity with other materials, or introduce unstable factors. For example, using 2,5-di-tert-butylhydroquinone as an end-capping agent can effectively react with the active end groups at the end of the PEEK molecular chain to form a stable structure, thereby sealing the end groups; however, 2,5-di-tert-butylhydroquinone will decompose or volatilize at high temperatures to produce unstable by-products, which will not only affect the thermal stability and processing properties of PEEK, but also increase safety risks and cause pollution to the reactor. The amount of molecular weight regulator added and the reaction conditions are difficult to control accurately. For example, if 4,4'-dihydroxybenzophenone is added as a molecular weight regulator, if the addition ratio is too large, the molecular weight of the oligomer generated in the initial stage of the reaction is too small, and the molecular weight of the polymer cannot be accurately controlled; if the addition ratio is too small, it will not inhibit phenoxy branching, and the molecular weight of the polymer cannot be accurately controlled. In addition, the end-capping agent and molecular weight regulator may have residues in the polymer, and these residues will also affect the purity and performance of the polymer.

[0006] It is worth noting that in the existing synthesis process of polyetheretherketone, it is considered to be a solid-phase polycondensation reaction, which is mainly controlled by temperature. Therefore, most studies usually focus more on temperature control and usually do not pay attention to specific "pressure" conditions. However, studies have shown that as the reaction proceeds, the pressure in the reactor will change due to the evaporation of the solvent and the gas produced by the reaction, which makes the polymerization environment uncontrollable and the regularity of the polymerization chain will also be affected. Therefore, the pressure during the polymerization process is also an important link to ensure the molecular weight distribution of the polymer.

[0007] Therefore, how to obtain high-purity monomers, how to optimize the synthesis process of polyetheretherketone, effectively narrow the molecular weight distribution range of PEEK materials, obtain polyetheretherketone products with stable and reliable performance, and broaden the scope of use of PEEK in high-end application fields are still problems that need to be solved urgently. Summary of the invention

[0008] In view of the above problems and in order to achieve the above objectives, the present invention provides a high-performance polyetheretherketone (PEEK) fine synthesis process, starting from the polymerization raw materials, using non-metallic catalysts to prepare high-purity polymerization monomer 4,4'-difluorobenzophenone (4,4'-DFBP), ensuring the stability of the molecular performance of the synthesized polyetheretherketone from the source; and by precisely and finely controlling each link in the polymerization process, achieving PEEK materials with a narrow molecular weight distribution range, meeting high-end design requirements in the fields of aerospace, medical equipment and electrical applications. The specific technical scheme is as follows:

[0009] A high-performance polyetheretherketone fine synthesis process comprises the following steps:

[0010] 1) Synthesis and purification of high-purity 4,4'-difluorobenzophenone:

[0011] Using para-fluorotrichlorotoluene and fluorobenzene as starting materials, in the presence of a mixture of trifluoromethanesulfonic acid and N,N-dimethyl-4-pyridinamine as a catalyst, an acylation reaction is carried out in an inert atmosphere to generate 4,4'-difluorophenyldichloromethane, and then a hydrolysis reaction is carried out to generate 4,4'-difluorobenzophenone; then purification is carried out to remove the catalyst, unreacted starting materials and by-products, and 4,4'-difluorobenzophenone with a purity of ≥99.99% is obtained for standby use;

[0012] 2) Nitrogen replacement to control oxygen concentration:

[0013] The prepared 4,4'-difluorobenzophenone, hydroquinone, sodium carbonate and diphenyl sulfone are gas-displaced with nitrogen having a purity greater than 99.9995%, and the melting tank is replaced at the same time; the qualified materials of gas replacement are added into the corresponding melting tank after gas replacement by a single screw conveying and metering device after accurate metering in batches, and nitrogen replacement is continued to be introduced to control the oxygen concentration to be less than 5ppm;

[0014] 3) Material melting:

[0015] After the oxygen concentration in the melting tank reaches the standard, heating is started to melt 4,4'-difluorobenzophenone, hydroquinone, and diphenyl sulfone respectively, and sodium carbonate is added to the melted diphenyl sulfone for standby use;

[0016] 4) Synthesis of PEEK:

[0017] The molten materials are added to the pre-substituted reactor in order, the molar ratio of the polymerization raw material monomer 4,4'-difluorobenzophenone and hydroquinone is controlled, the amount of sodium carbonate and diphenyl sulfone and the oxygen concentration in the reactor are controlled, stirring is started, and polymerization reaction is carried out to synthesize PEEK;

[0018] During the reaction, the temperature and pressure gradients are precisely controlled, while the residence time of the reaction materials at each temperature gradient is controlled, and the material-liquid ratio of 4,4'-difluorobenzophenone and diphenyl sulfone is balanced;

[0019] The gradient temperature increase and pressure increase is:

[0020] The first gradient temperature is 150-180°C, the pressure is 0.1-0.5Mpa, and the reaction material residence time is 1-5 hours;

[0021] The second gradient temperature is 250-280°C, the pressure is 0.3-0.8Mpa, and the reaction material residence time is 1-3 hours;

[0022] The third gradient temperature is 300-320°C, the pressure is 1-1.5Mpa, and the reaction material residence time is 1-2 hours;

[0023] 5) Determine the end point of the polymerization reaction:

[0024] The torque force generated by the melt stirring in the reactor is detected by a torque sensor, thereby judging the polymerization reaction end point and controlling the melt index of polyetheretherketone;

[0025] 6) End-capping refining:

[0026] After the polymerization reaction reaches the end point, 4,4'-difluorobenzophenone is added as a capping agent to perform capping to complete the polymerization reaction; and then the reaction is refined to obtain high-performance polyetheretherketone.

[0027] In the above-mentioned high-performance polyetheretherketone fine synthesis process, in step 1), the specific process of synthesis and purification of high-purity 4,4'-difluorobenzophenone includes the following sub-steps:

[0028] 1-1) Acylation reaction:

[0029] In a nitrogen atmosphere, p-fluorotrichlorotoluene and fluorobenzene are mixed, cooled to 0-25° C., and then a mixture of trifluoromethanesulfonic acid and N,N-dimethyl-4-pyridinamine is added as a catalyst, and the reaction is carried out for 10-30 minutes to complete the acylation reaction to generate 4,4'-difluorophenyldichloromethane;

[0030] 1-2) Hydrolysis reaction: 4,4'-difluorophenyl dichloromethane is mixed with water, heated to 100-110°C for azeotropic reaction, and hydrolyzed for 4-6 hours to obtain crude 4,4'-difluorobenzophenone;

[0031] 1-3) Purification: After the hydrolysis reaction is completed, the material is purified by extraction, filtration, distillation and recrystallization to remove the catalyst, unreacted starting materials and by-products to obtain 4,4'-difluorobenzophenone with a purity of ≥99.99%.

[0032] As a preferred technical solution, in the above-mentioned high-performance polyetheretherketone fine synthesis process, in step 1-1), the molar ratio of p-fluorotrichlorotoluene to fluorobenzene is 1:3-5; the amount of the catalyst, trifluoromethanesulfonic acid, is 0.1-0.3 equivalents of the total molar amount of p-fluorotrichlorotoluene and fluorobenzene, and the amount of N,N-dimethyl-4-pyridinamine is 1-10% of the mass of trifluoromethanesulfonic acid.

[0033] As a preferred technical solution, the above-mentioned high-performance polyetheretherketone fine synthesis process, the specific process of the purification treatment in step 1-3) is:

[0034] A. Extracting the catalyst: After the hydrolysis reaction is completed, the material is cooled to room temperature, and sodium carbonate with a weight of 2 to 3 times the total mass of the catalyst is added, and the catalyst is extracted by stirring at 200 to 500 rpm for 5 to 10 minutes;

[0035] B. Distillation: Then centrifuge at 3000-5000 rpm for 2 min, take the middle organic phase for distillation, the distillation temperature is 275-280°C, and obtain 4,4'-difluorobenzophenone distillate;

[0036] C. Recrystallization: Add 95% ethanol in an amount of 10 times the volume of 4,4'-difluorobenzophenone distillate, and stir for 5-10 minutes in a water bath at 80°C; then filter while hot, transfer the filtered hot solution to a crystallizer and gradually cool it at room temperature to crystallize 4,4'-difluorobenzophenone;

[0037] D. Washing: After crystallization is completed, centrifuge at 2000-3000 rpm for 2 minutes, take the precipitate and add 95% ethanol to wash the crystals three times. The amount of 95% ethanol added each time is 1.5-2 times the volume of 4,4'-difluorobenzophenone crystals;

[0038] E. Drying: After washing, place the 4,4'-difluorobenzophenone crystals in a vacuum drying oven at 60-80°C for more than 6 hours to ensure complete drying;

[0039] F. Purity test: Check the purity of 4,4'-difluorobenzophenone after recrystallization, and the purity is qualified if it is ≥ 99.99%.

[0040] As a preferred technical solution, in the above-mentioned high-performance polyetheretherketone fine synthesis process, in step 4),

[0041] In the synthesis of the PEEK precursor, the order of adding the molten materials into the reactor is: first adding the molten diphenyl sulfone and sodium carbonate into the reactor, and then adding the polymerization raw material monomers 4,4'-difluorobenzophenone and hydroquinone into the reactor at the same time;

[0042] The molar ratio of the polymerization raw material monomers 4,4'-difluorobenzophenone and hydroquinone is 1:1 to 1.2;

[0043] The molar ratio of the amount of sodium carbonate to hydroquinone is: hydroquinone: sodium carbonate = 1:2.3-2.5;

[0044] The amount of diphenyl sulfone used is 2 to 4 times the volume of 4,4'-difluorobenzophenone;

[0045] The concentration of reactive oxygen in the reactor is controlled to be less than 5 ppm;

[0046] The precise control of the gradient temperature and pressure is:

[0047] The first gradient temperature is 150-180°C, the pressure is 0.1-0.5Mpa, and the reaction material residence time is 1-5 hours;

[0048] The second gradient temperature is 250-280°C, the pressure is 0.3-0.8Mpa, and the reaction material residence time is 1-3 hours;

[0049] The third gradient temperature is 300-320° C., the pressure is 1-1.5 MPa, and the residence time of the reaction materials is 1-2 hours.

[0050] As a further preferred technical solution, in the above-mentioned high-performance polyetheretherketone fine synthesis process, the gradient temperature increase and pressure increase is:

[0051] First gradient: 150℃±5℃, 0.2Mpa, the reaction mass is retained for 1h; 160℃±5℃, 0.3Mpa, the reaction mass is retained for 0.5h; 170℃±5℃, 0.4Mpa, the reaction mass is retained for 0.5h; 180℃±5℃, 0.5Mpa, the reaction mass is retained for 1h;

[0052] Second gradient: 250℃±5℃, 0.6Mpa, the reaction mass is retained for 1h; 260℃±5℃, 0.7Mpa, the reaction mass is retained for 0.5h; 270℃±5℃, 0.8Mpa, the reaction mass is retained for 0.5h;

[0053] The third gradient: 300°C±2°C, 1 MPa, the reaction material is retained for 0.5 h; 310°C±2°C, 1.2 MPa, the reaction material is retained for 1 h.

[0054] As a preferred technical solution, in the above-mentioned high-performance polyetheretherketone fine synthesis process, in step 4), the balanced material-liquid ratio of 4,4'-difluorobenzophenone and diphenyl sulfone is specifically as follows: in the synthesis stage of the PEEK precursor, 8 to 10 wt% of 4,4'-difluorobenzophenone, one of the polymerization monomer raw materials, is reserved, and in the second gradient stage of the gradient heating, when the temperature reaches 250°C, it is added in at least three batches to ensure the balance of the reaction material-liquid ratio and to make the prepolymerization reaction stable.

[0055] As a preferred technical solution, in the above-mentioned high-performance polyetheretherketone fine synthesis process, in step 5), at the end point of the polymerization reaction, the melt index of the polymerized polyetheretherketone is controlled to be 8 to 90 g / 10 min.

[0056] As a preferred technical solution, in the above-mentioned high-performance polyetheretherketone fine synthesis process, in step 6), the amount of the end-capping agent 4,4'-difluorobenzophenone added is 2% to 3% of the mass of the polymerized monomer 4,4'-difluorobenzophenone;

[0057] The refining process is to directly introduce the polyetheretherketone melt into a supercritical carbon dioxide extraction device for extraction. The specific parameters of the extraction are:

[0058] The carbon dioxide flow rate is 50-60 kg / h·kg PEEK, the extraction pressure is 25-35 MPa, and the temperature is 345-365°C;

[0059] The separation column pressure is 15-20 MPa, and the temperatures from bottom to top are 350°C, 355°C, 360°C, and 365°C;

[0060] The first decomposition kettle has a pressure of 5.5-6.5 MPa and a temperature of 305°C;

[0061] The second analysis kettle has a pressure of 4.5-5.5 MPa and a temperature of 275°C.

[0062] The extraction time was set at 180 min, and the polyetheretherketone extraction melt was taken out from the bottom of the separation column every 20 min for cooling and solidification to obtain high-performance polyetheretherketone.

[0063] Beneficial effects of the present invention:

[0064] 1) The synthesis process of the present invention starts with the polymerization raw materials, improves the purity of the polymerization monomer 4,4'-difluorobenzophenone, and adopts a mixture of non-metallic trifluoromethanesulfonic acid and N,N-dimethyl-4-pyridinamine as a catalyst, wherein the trifluoromethanesulfonic acid can protonate fluorobenzene to make it more electron-deficient, thereby increasing the nucleophilic attack ability of para-fluorotrichlorotoluene, and the protonation effect helps to form an intermediate, thereby promoting the acylation reaction; N,N-dimethyl-4-pyridinamine can form a complex with the carbonyl oxygen atom in para-fluorotrichlorotoluene, reduce the bond order of the C=O bond of the carbonyl group, make the carbonyl carbon atom more electron-deficient, and increase its attraction to the nucleophilic reagent; in addition, N,N-dimethyl-4-pyridinamine can further stabilize the generated intermediate through its protonation effect, thereby improving the selectivity and yield of the reaction. The synergistic effect of the two can not only significantly increase the reaction rate, allowing the reaction to be completed in a shorter time, but most importantly, it can be removed from the product through subsequent purification steps, essentially reducing the metal and non-metal impurities in 4,4'-difluorobenzophenone. The effect of impurities in 4,4'-DFBP on the performance of PEEK materials is solved from the source, ensuring the stability of the synthesized polyetheretherketone polymer chain, thereby improving the thermal stability and mechanical properties of PEEK, so that the obtained 4,4'-difluorobenzophenone material can be adapted to the application of high-end designs in the electrical field.

[0065] 2) The synthesis process of the present invention increases the purity of nitrogen to greater than 99.9995% or even greater than 99.9999% by making a homemade molecular sieve, which fundamentally controls the oxygen concentration in the reaction system and further prevents the oxygen component from affecting the polymer, so that the obtained polyetheretherketone product has a lighter color and higher quality.

[0066] 3) The synthesis process of the present invention pays attention to the influence of pressure on the molecular weight of the polymer during the polymerization process for the first time. It not only controls the temperature increase program more carefully, but also controls the pressure of the entire polymerization process in coordination. It increases the pressure as the temperature increases, controls the growth rate of the polymer chain more finely, controls the distribution of molecular weight, and reduces the occurrence of various side reactions (such as cross-linking or chain transfer) that may occur during the polymer synthesis process by gradually increasing the pressure, which helps to obtain PEEK with a narrow molecular weight distribution. In addition, as the pressure increases, the concentration of the reactants is increased, the selectivity of the reaction is improved, and the purity of the final PEEK product is improved. At the same time, increasing the pressure can make the small molecules generated by the reaction, including (water and carbon dioxide), fully discharged without affecting subsequent reactions. In addition, in the process of the present invention, the material-liquid ratio of 4,4'-difluorobenzophenone and diphenyl sulfone is balanced in the gradient temperature increase and pressure increase stage, so that the polymerization reaction is more uniform and controllable, and the occurrence of this side reaction is further reduced, and the regularity of the polymer molecular chain is further guaranteed, so that the polymer has more consistent physical and chemical properties, and the product quality is improved.

[0067] 4) The synthesis process of the present invention uses a torque sensor to detect the torque force generated by the melt stirring in the reactor to determine the end point of the polymerization reaction, and control the melt index of the synthesized polymer melt, avoiding the use of molecular weight regulators and the introduction of unstable factors, while better controlling the polymer molecular weight. After the polymerization is completed, the polyetheretherketone melt is directly introduced into the carbon dioxide supercritical equipment for extraction, which further ensures the purity and performance of the polyetheretherketone.

[0068] 5) The synthesis process of the present invention uses 4,4'-difluorobenzophenone, one of the polymerization monomers, as a capping agent, which not only avoids the introduction of unstable factors by selecting an additional capping agent, but also facilitates the later refining of the polymerization product; and 4,4'-difluorobenzophenone is used as a capping agent, and its molecular chain after capping contains a fluorine end group, which has a higher bond energy, so that the polymer chain end has better thermal stability, and the bonding force between the fluorine atom and the carbon atom is strong, which helps to maintain the integrity of the polymer chain and enhance the mechanical properties of the PEEK polymer. At the same time, the high electronegativity of the fluorine atom makes it difficult for the polymer chain end to react with other chemical substances, thereby enhancing the chemical stability of PEEK and making it more resistant to chemical corrosion, further ensuring the application of polyetheretherketone materials in high-end products in the fields of aerospace, medical equipment, and electrical. BRIEF DESCRIPTION OF THE DRAWINGS

[0069] Figure 1The liquid chromatography test result of 4,4'-difluorobenzophenone synthesized by the preparation method of the present invention;

[0070] Figure 2 The polyetheretherketone product synthesized by the present invention is real;

[0071] Figure 3 This is a chromaticity comparison of the polyetheretherketone product of the embodiment of the present invention;

[0072] Figure 4 The figures are the acid and alkali resistance test and results of the polyetheretherketone product according to the embodiment of the present invention. DETAILED DESCRIPTION

[0073] In order to make the purpose, technical solution and advantages of the present invention more clear, the technical solution of the present invention will be clearly and completely described below in conjunction with embodiments.

[0074] Example 1

[0075] The present embodiment is a method for preparing high-purity nitrogen. The purity of existing commercially available nitrogen is mostly 99.9%, high-purity is 99.99%, and a few can reach 99.999%. As for polyetheretherketone, as a high-performance special engineering plastic, the environment in which it is used has very high requirements for its own structural performance, especially high-end designs in the fields of aerospace, medical equipment, electrical applications, etc., which have more stringent requirements on the performance of polyetheretherketone materials. During the polymerization process, the oxygen content in the atmosphere will not only cause the color of the polyetheretherketone product to deepen, but also oxidatively damage its chain segments, burying the hidden danger of instability for subsequent applications. In order to solve this problem, this embodiment provides a measure to prepare nitrogen with a purity greater than 99.9995%, or even greater than 99.9999%, for use. The specific process is as follows:

[0076] The nitrogen gas with a purity of 99.99% purchased from the market is compressed and pre-treated to a pressure of 0.5-1.3Mpa, and then passed into a prefabricated purification adsorption tower for pressure swing adsorption treatment. The prefabricated purification adsorption tower includes three levels of molecular sieves, two of which are 3A zeolite molecular sieves, and one is a carbon molecular sieve with a pore size between 0.3 and 1nm; the distribution structure of each molecular sieve is: 3A zeolite molecular sieve-carbon molecular sieve-3A zeolite molecular sieve; the parameters of pressure swing adsorption are:

[0077] Adsorption stage: pressure 2.5Mpa, adsorption time 10min;

[0078] Desorption stage: pressure 0.8Mpa, desorption time 3min;

[0079] The cycle of the adsorption-desorption process is to detect that the purity of nitrogen is greater than 99.9999%. In the following examples, the nitrogen used is prepared by the method of this example.

[0080] Example 2

[0081] This embodiment is a method for synthesizing high-purity 4,4'-difluorobenzophenone. 4,4'-difluorobenzophenone is a key monomer for synthesizing PEEK. The impurities therein, especially non-metallic impurities and metal residues, have a significant effect on the performance of PEEK materials. Among them, non-metallic impurities will introduce defects in the polymerization process of PEEK chains, affecting the stability of the molecular chains, while metal residues will cause the PEEK chains to be cross-linked, resulting in oversized chain segments, affecting the stability of product performance. At the same time, metal residues may also increase the conductivity of PEEK, affecting its application in the electrical field.

[0082] In this embodiment, in order to obtain high-quality PEEK, para-fluorotrichlorotoluene and fluorobenzene are used as starting materials, and a mixture of trifluoromethanesulfonic acid and N,N-dimethyl-4-pyridinamine is used instead of a metal compound as a catalyst, and an acylation reaction is carried out in an inert atmosphere to generate 4,4'-difluorophenyldichloromethane, and a hydrolysis reaction is carried out to obtain 4,4'-difluorobenzophenone; and a double purification by distillation + recrystallization is carried out to completely remove the catalyst, unreacted starting materials and by-products, and 4,4'-difluorobenzophenone with a purity of ≥99.99% is obtained. The details are as follows:

[0083] First, 2 kg of p-fluorobenzotrichloride and 4 kg of fluorobenzene were weighed, and p-fluorobenzotrichloride and fluorobenzene were mixed in the nitrogen atmosphere prepared in Example 1, and then cooled to 4°C, and then 1.8 kg of trifluoromethanesulfonic acid and 0.2 kg of N,N-dimethyl-4-pyridinamine mixture were added, stirred and mixed evenly, and the temperature was raised to 16°C, and the acylation reaction was carried out for 30 minutes to generate 4,4'-difluorophenyl dichloromethane. Then, the reactant was mixed with purified water, heated to the azeotropic temperature of 110°C, and hydrolyzed for 5 hours to obtain 4,4'-difluorobenzophenone.

[0084] The material after the hydrolysis reaction was completed was cooled to room temperature, 5 kg of sodium carbonate was added, and the mixture was stirred at 300 rpm for 10 minutes to extract the catalyst; then centrifuged at 4000 rpm for 2 minutes, and the organic phase in the middle was distilled at a distillation temperature of 137°C to obtain 4,4'-difluorobenzophenone distillate; 95% ethanol in an amount 10 times its volume was added to the 4,4'-difluorobenzophenone distillate, and stirred for 10 minutes under 80°C water bath conditions; filtered while hot, the filtered hot solution was transferred to a crystallizer and gradually cooled at room temperature to crystallize 4,4'-difluorobenzophenone; after crystallization, the mixture was centrifuged at 2500 rpm for 2 minutes, the precipitate was taken and 95% ethanol was added to wash the crystals 3 times, and the amount of 95% ethanol added each time was 2 times the volume of the 4,4'-difluorobenzophenone crystals. After washing, the 4,4'-difluorobenzophenone crystals were placed in a vacuum drying oven and dried at 75°C for 10 hours to ensure complete drying. The purity of 4,4'-difluorobenzophenone after recrystallization was tested by liquid chromatography. Figure 1 As shown, the purity of the prepared 4,4'-difluorobenzophenone reaches 99.99%, which is qualified and ready for use.

[0085] Example 3

[0086] This embodiment is to synthesize a polyetheretherketone (PEEK).

[0087] Take 900 kg of high-purity 4,4'-difluorobenzophenone synthesized in Example 2, 423 kg of hydroquinone, 1142 kg of sodium carbonate, and 3000 kg of diphenyl sulfone, and replace them with the nitrogen prepared in Example 1, respectively, and replace three melting kettles at the same time; the qualified materials are added to the corresponding replaced melting tanks in batches after accurate measurement through a single screw conveying and metering device, and nitrogen is continued to be introduced for replacement until the oxygen concentration is less than 5 ppm, and then heated to melt them respectively. After the materials are completely melted, sodium carbonate is added to diphenyl sulfone, and stirred and mixed evenly for standby use.

[0088] At the same time, the nitrogen prepared in Example 1 was used to replace the polymerization reactor, and the oxygen concentration was also controlled to be less than 5 ppm. Sodium carbonate and diphenyl sulfone were first input into the polymerization reactor, and then molten 4,4'-difluorobenzophenone and hydroquinone were added to the reactor, wherein 100 kg of 4,4'-difluorobenzophenone was left for subsequent material ratio balancing and end-capping. The temperature and pressure in the reactor were carefully controlled, and the temperature and pressure were increased gradually, specifically:

[0089] The first gradient: temperature 150℃, pressure 0.2Mpa, reaction 1h; temperature increased to 160℃, pressure 0.3Mpa, reaction 0.5h; temperature increased to 170℃, pressure 0.4Mpa, reaction 0.5h; temperature increased to 180℃, pressure 0.5Mpa, reaction 1h; to ensure that small molecule water and carbon dioxide are fully and thoroughly discharged; no effect on the second gradient.

[0090] Second gradient: temperature raised to 250℃, pressure 0.6Mpa, reaction 1h; at this stage, the remaining 87kg 4,4'-difluorobenzophenone was added to the reactor in five times, with an interval of 10min, 18kg was added each time from the first to the fourth time, and 15kg was added for the last time. Then the temperature was raised to 260℃, pressure 0.7Mpa, reaction 0.5h; temperature raised to 270℃, pressure 0.8Mpa, reaction 0.5h; ensure that the prepolymerization is stable, the molecular chain formed is uniform and average; there is no obviously too large or too small segment.

[0091] The third gradient: the temperature rises to 300°C, the pressure is 1.0Mpa, and the reaction is carried out for 0.5h; the temperature rises to 310°C, the pressure is 1.2Mpa, and the reaction is carried out for 1h; ensure that the polymerization stage is smooth, the formed molecular chains are uniform and average; and there are no obviously too large or too small chain segments; it is conducive to improving the fluidity and mechanical strength of the polymer.

[0092] Observe the torque sensor until the torque value displayed reaches the predetermined range and the torque value changes less than 0.5Nm within 20 minutes, and judge that the polymerization reaction has reached the end point. Then add the remaining 22kg of molten 4,4'-difluorobenzophenone as a capping agent into the reactor, continue stirring, react for 10 minutes, and complete the polymerization reaction. Then introduce the melt into the supercritical carbon dioxide extraction equipment for refining. The extraction conditions are:

[0093] The carbon dioxide flow rate is 50-60 kg / h·kg PEEK, the extraction pressure is 25-35 MPa, and the temperature is 345-365°C;

[0094] The separation column pressure is 15-20 MPa, and the temperatures from bottom to top are 350°C, 355°C, 360°C, and 365°C;

[0095] The first decomposition kettle has a pressure of 5.5-6.5 MPa and a temperature of 305°C;

[0096] The second analysis kettle has a pressure of 4.5-5.5 MPa and a temperature of 275°C.

[0097] The extraction time was set to 180 min, and the polyetheretherketone extraction melt was taken out from the bottom of the separation column every 20 min for cooling and solidification to obtain polyetheretherketone product 1 (PEEK1). Figure 2 shown.

[0098] Example 4

[0099] This example also synthesizes a polyetheretherketone (PEEK). The amount of each material used in this example is consistent with that in Example 3. The synthesis method does not perform gradient pressure control during the gradient heating stage. The pressure in the reactor during the reaction is 0.1-0.2Mpa. The remaining steps and parameters are also consistent with those in Example 3. The details are as follows:

[0100] Take 900 kg of high-purity 4,4'-difluorobenzophenone synthesized in Example 2, 423 kg of hydroquinone, 1142 kg of sodium carbonate, and 3000 kg of diphenyl sulfone, and replace them with the nitrogen prepared in Example 1, respectively, and replace three melting kettles at the same time; the qualified materials are added to the corresponding replaced melting tanks in batches after accurate measurement through a single screw conveying and metering device, and nitrogen is continued to be introduced for replacement until the oxygen concentration is less than 5 ppm, and then heated to melt them respectively. After the materials are completely melted, sodium carbonate is added to diphenyl sulfone, and stirred and mixed evenly for standby use.

[0101] At the same time, the polymerization reactor was replaced with the nitrogen prepared in Example 1, and the oxygen concentration was also controlled to be less than 5 ppm. Sodium carbonate and diphenyl sulfone were first introduced into the polymerization reactor, and then molten 4,4'-difluorobenzophenone and hydroquinone were added to the reactor, wherein 100 kg of 4,4'-difluorobenzophenone was left for subsequent material ratio balancing and end-capping. The temperature in the reactor was controlled as follows:

[0102] First gradient: temperature 150℃, reaction for 3h; temperature increased to 160℃, reaction for 0.5h; temperature increased to 170℃, reaction for 0.5h; temperature increased to 180℃, reaction for 1h;

[0103] Second gradient: Raise the temperature to 250℃ and react for 1h. At this stage, add the remaining 87kg of 4,4'-difluorobenzophenone into the reactor in five times, with an interval of 10min. From the first to the fourth time, 18kg is added each time, and the last time is 15kg. Then raise the temperature to 260℃ and react for 0.5h; raise the temperature to 270℃ and react for 0.5h.

[0104] The third gradient: the temperature was raised to 300°C and the reaction was continued for 0.5 h; the temperature was raised to 310°C and the reaction was continued for 1 h.

[0105] Observe the torque sensor until the torque value displayed reaches the predetermined range and the torque value changes less than 0.5Nm within 20 minutes, and judge that the polymerization reaction has reached the end point. Then add the remaining 22kg of molten 4,4'-difluorobenzophenone as a capping agent into the reactor, continue stirring, react for 10 minutes, and complete the polymerization reaction. Then introduce the melt into the supercritical carbon dioxide extraction equipment for refining. The extraction conditions are:

[0106] The carbon dioxide flow rate is 50-60 kg / h·kg PEEK, the extraction pressure is 25-35 MPa, and the temperature is 345-365°C;

[0107] The separation column pressure is 15-20 MPa, and the temperatures from bottom to top are 350°C, 355°C, 360°C, and 365°C;

[0108] The first decomposition kettle has a pressure of 5.5-6.5 MPa and a temperature of 305°C;

[0109] The second analysis kettle has a pressure of 4.5-5.5 MPa and a temperature of 275°C.

[0110] The extraction time was set at 180 min, and the polyetheretherketone extraction melt was taken out from the bottom of the separation column every 20 min for cooling and solidification to obtain polyetheretherketone product 2 (PEEK2).

[0111] Example 5

[0112] This example also synthesizes a polyetheretherketone (PEEK). The amount of each material of the polyetheretherketone in this example is consistent with that in Example 3. Except that the material ratio is not balanced in the gradient heating stage, the other steps and parameters of the synthesis method are also consistent with those in Example 3. The details are as follows:

[0113] Take 900 kg of high-purity 4,4'-difluorobenzophenone synthesized in Example 2, 423 kg of hydroquinone, 1142 kg of sodium carbonate, and 3000 kg of diphenyl sulfone, and replace them with the nitrogen prepared in Example 1, respectively, and replace three melting kettles at the same time; the qualified materials are added to the corresponding replaced melting tanks in batches after accurate measurement through a single screw conveying and metering device, and nitrogen is continued to be introduced for replacement until the oxygen concentration is less than 5 ppm, and then heated to melt them respectively. After the materials are completely melted, sodium carbonate is added to diphenyl sulfone, and stirred and mixed evenly for standby use.

[0114] At the same time, the nitrogen prepared in Example 1 was used to replace the polymerization reactor, and the oxygen concentration was also controlled to be less than 5 ppm. Sodium carbonate and diphenyl sulfone were first input into the polymerization reactor, and then molten 4,4'-difluorobenzophenone and hydroquinone were added to the reactor, wherein 22 kg of 4,4'-difluorobenzophenone was left for subsequent end-capping. The temperature and pressure in the reactor were carefully controlled, and the temperature and pressure were increased gradually, specifically:

[0115] The first gradient: temperature 150°C, pressure 0.2Mpa, reaction 1h; temperature increased to 160°C, pressure 0.3Mpa, reaction 0.5h; temperature increased to 170°C, pressure 0.4Mpa, reaction 0.5h; temperature increased to 180°C, pressure 0.5Mpa, reaction 1h.

[0116] The second gradient: the temperature was raised to 250°C, the pressure was 0.6 MPa, and the reaction lasted for 1 hour; then the temperature was raised to 260°C, the pressure was 0.7 MPa, and the reaction lasted for 0.5 hour; the temperature was raised to 270°C, the pressure was 0.8 MPa, and the reaction lasted for 0.5 hour.

[0117] The third gradient: the temperature was raised to 300°C, the pressure was 1.0 MPa, and the reaction was carried out for 0.5 h; the temperature was raised to 310°C, the pressure was 1.2 MPa, and the reaction was carried out for 1 h.

[0118] Observe the torque sensor until the torque value displayed reaches the predetermined range and the torque value changes less than 0.5Nm within 20 minutes, and judge that the polymerization reaction has reached the end point. Then add the remaining 22kg of molten 4,4'-difluorobenzophenone as a capping agent into the reactor, continue stirring, react for 10 minutes, and complete the polymerization reaction. Then introduce the melt into the supercritical carbon dioxide extraction equipment for refining. The extraction conditions are:

[0119] The carbon dioxide flow rate is 50-60 kg / h·kg PEEK, the extraction pressure is 25-35 MPa, and the temperature is 345-365°C;

[0120] The separation column pressure is 15-20 MPa, and the temperatures from bottom to top are 350°C, 355°C, 360°C, and 365°C;

[0121] The first decomposition kettle has a pressure of 5.5-6.5 MPa and a temperature of 305°C;

[0122] The second analysis kettle has a pressure of 4.5-5.5 MPa and a temperature of 275°C.

[0123] The extraction time was set to 180 min, and the polyetheretherketone extraction melt was taken out from the bottom of the separation column every 20 min for cooling and solidification to obtain polyetheretherketone product 3 (PEEK3).

[0124] Example 6

[0125] This example also synthesizes a polyetheretherketone (PEEK). The amount of each material used in this example is consistent with that in Example 3. The synthesis method is that the temperature is not finely controlled during the gradient heating stage, and the remaining steps and parameters are also consistent with those in Example 3. The details are as follows:

[0126] Take 900 kg of high-purity 4,4'-difluorobenzophenone synthesized in Example 2, 423 kg of hydroquinone, 1142 kg of sodium carbonate, and 3000 kg of diphenyl sulfone, and replace them with the nitrogen prepared in Example 1, respectively, and replace three melting kettles at the same time; the qualified materials are added to the corresponding replaced melting tanks in batches after accurate measurement through a single screw conveying and metering device, and nitrogen is continued to be introduced for replacement until the oxygen concentration is less than 5 ppm, and then heated to melt them respectively. After the materials are completely melted, sodium carbonate is added to diphenyl sulfone, and stirred and mixed evenly for standby use.

[0127] At the same time, the nitrogen prepared in Example 1 was used to replace the polymerization reactor, and the oxygen concentration was also controlled to be less than 5 ppm. Sodium carbonate and diphenyl sulfone were first input into the polymerization reactor, and then molten 4,4'-difluorobenzophenone and hydroquinone were added to the reactor, wherein 100 kg of 4,4'-difluorobenzophenone was left for subsequent material ratio balancing and end-capping. The temperature and pressure in the reactor were carefully controlled, and the temperature and pressure were increased gradually, specifically:

[0128] The first gradient: temperature 150°C, reaction time 3h.

[0129] Second gradient: raise the temperature to 250°C and react for 2h; at this stage, add the remaining 87kg of 4,4'-difluorobenzophenone into the reactor in five times, with an interval of 10min. From the first to the fourth time, 18kg is added each time, and the last time is 15kg.

[0130] The third gradient: the temperature was raised to 300°C and the reaction was continued for 1.5 hours.

[0131] Observe the torque sensor until the torque value displayed reaches the predetermined range and the torque value changes less than 0.5Nm within 20 minutes, and judge that the polymerization reaction has reached the end point. Then add the remaining 22kg of molten 4,4'-difluorobenzophenone as a capping agent into the reactor, continue stirring, react for 10 minutes, and complete the polymerization reaction. Then introduce the melt into the supercritical carbon dioxide extraction equipment for refining. The extraction conditions are:

[0132] The carbon dioxide flow rate is 50-60 kg / h·kg PEEK, the extraction pressure is 25-35 MPa, and the temperature is 345-365°C;

[0133] The separation column pressure is 15-20 MPa, and the temperatures from bottom to top are 350°C, 355°C, 360°C, and 365°C;

[0134] The first decomposition kettle has a pressure of 5.5-6.5 MPa and a temperature of 305°C;

[0135] The second analysis kettle has a pressure of 4.5-5.5 MPa and a temperature of 275°C.

[0136] The extraction time was set at 180 min, and the polyetheretherketone extraction melt was taken out from the bottom of the separation column every 20 min for cooling and solidification to obtain polyetheretherketone product 4 (PEEK4).

[0137] Example 7

[0138] This example also synthesizes a polyetheretherketone (PEEK). The amount of each material used in the polyetheretherketone in this example is consistent with that in Example 3. The synthesis method is that the temperature is not finely controlled during the gradient heating stage, and the material ratio is not balanced. The remaining steps and parameters are also consistent with those in Example 3. The details are as follows:

[0139] Take 900 kg of high-purity 4,4'-difluorobenzophenone synthesized in Example 2, 423 kg of hydroquinone, 1142 kg of sodium carbonate, and 3000 kg of diphenyl sulfone, and replace them with the nitrogen prepared in Example 1, respectively, and replace three melting kettles at the same time; the qualified materials are added to the corresponding replaced melting tanks in batches after accurate measurement through a single screw conveying and metering device, and nitrogen is continued to be introduced for replacement until the oxygen concentration is less than 5 ppm, and then heated to melt them respectively. After the materials are completely melted, sodium carbonate is added to diphenyl sulfone, and stirred and mixed evenly for standby use.

[0140] At the same time, the nitrogen prepared in Example 1 was used to replace the polymerization reactor, and the oxygen concentration was also controlled to be less than 5 ppm. Sodium carbonate and diphenyl sulfone were first input into the polymerization reactor, and then molten 4,4'-difluorobenzophenone and hydroquinone were added to the reactor, wherein 22 kg of 4,4'-difluorobenzophenone was left for subsequent end-capping. The temperature and pressure in the reactor were carefully controlled, and the temperature and pressure were increased gradually, specifically:

[0141] The first gradient: temperature 150°C, reaction time 3h.

[0142] Second gradient: raise the temperature to 250°C and react for 2h.

[0143] The third gradient: the temperature was raised to 300°C and the reaction was continued for 1.5 hours.

[0144] Observe the torque sensor until the torque value displayed reaches the predetermined range and the torque value changes less than 0.5Nm within 20 minutes, and judge that the polymerization reaction has reached the end point. Then add the remaining 22kg of molten 4,4'-difluorobenzophenone as a capping agent into the reactor, continue stirring, react for 10 minutes, and complete the polymerization reaction. Then introduce the melt into the supercritical carbon dioxide extraction equipment for refining. The extraction conditions are:

[0145] The carbon dioxide flow rate is 50-60 kg / h·kg PEEK, the extraction pressure is 25-35 MPa, and the temperature is 345-365°C;

[0146] The separation column pressure is 15-20 MPa, and the temperatures from bottom to top are 350°C, 355°C, 360°C, and 365°C;

[0147] The first decomposition kettle has a pressure of 5.5-6.5 MPa and a temperature of 305°C;

[0148] The second analysis kettle has a pressure of 4.5-5.5 MPa and a temperature of 275°C.

[0149] The extraction time was set to 180 min, and the polyetheretherketone extraction melt was taken out from the bottom of the separation column every 20 min for cooling and solidification to obtain polyetheretherketone product 5 (PEEK5).

[0150] Example 8

[0151] This example also synthesizes a polyetheretherketone (PEEK). The synthesis method of this example is the same as that of Example 3, except that the 4,4'-difluorobenzophenone used is purchased from the market (Shanghai Siyan Biotechnology Co., Ltd.) with a purity of 98%. Polyetheretherketone product 6 (PEEK6) is obtained.

[0152] Example 9

[0153] This example also synthesizes a polyetheretherketone (PEEK). The synthesis method of this example is consistent with that of Example 3, except that the nitrogen used is purchased from the market (Hangzhou Best Gas Co., Ltd.) with a purity of 99.999%. Since the oxygen purity of the nitrogen purchased from the market is not high, the oxygen concentration in the materials, melting kettle, reactor and reaction process in this example is relatively high, generally greater than 15ppm, or even greater than 20ppm. Polyetheretherketone product 7 (PEEK7) is obtained.

[0154] Example 10

[0155] This embodiment is to test the quality and performance of the polyetheretherketone products prepared in Examples 3 to 9.

[0156] 1) Test the viscosity, molecular weight distribution and conductivity of each PEEK product.

[0157] (1) Viscosity detection: In the embodiment, after supercritical extraction for 60 min, the polyetheretherketone extracted melt was taken out from the bottom of the separation column for viscosity detection. The specific detection method is: the flow index of the polyetheretherketone extracted melt is measured by CEAST melt flow meter MF30 (g / 10min).

[0158] (2) Molecular weight distribution range detection: The average molecular weight (Da) and molecular weight distribution (PDI) of each polyetheretherketone product are detected by the method specified in the national standard "Determination of the average molecular weight and molecular weight distribution of polymers by size exclusion chromatography of plastics Part 1: General rules" (GB / T 36214.1-2018).

[0159] (3) Conductivity test: Weigh 5 g of each refined polyetheretherketone product, add 10 ml of high-purity water (conductivity <1 μs / cm, 60°C) and stir and wash for 10 min. Then filter while hot and use a conductivity meter to test the conductivity of the aqueous solution.

[0160] The test results are shown in Table 1.

[0161] Table 1. Viscosity and molecular weight distribution of various polyetheretherketone products

[0162]

[0163] It can be seen from the test results in Table 1 that the use of more purified 4,4'-difluorobenzophenone as a monomer, the use of higher purity nitrogen for atmosphere protection, and the precise control of temperature and pressure can make the prepared polyetheretherketone have a narrower molecular weight distribution range and lower conductivity, making the polymerized polyetheretherketone molecular chain more regular and uniform, thereby ensuring the stability of product quality and performance.

[0164] 2) Test the physical and chemical properties of each polyetheretherketone product. Take each polyetheretherketone product and use a small injection molding machine to prepare standard specimens. Perform performance comparison tests under the same conditions and test the color value, physical properties and chemical properties according to relevant standards. The specific test preparation and method are as follows:

[0165] (1) Chromaticity value: spectrophotometer (UltraScan VIS), spectral range, 360 ~ 780nm, ensure that the surface of the PEEK sample is clean, without scratches or unevenness;

[0166] (2) Glass transition temperature and melting point: Differential scanning calorimetry (DSC) was used under the following conditions: nitrogen atmosphere, heating rate 10 °C / min, and secondary heating.

[0167] (3) 5% thermal weight loss: thermogravimetric analyzer (TGA), nitrogen atmosphere, heating rate 10°C / min;

[0168] (4) Melt viscosity change: rotational rheometer, 400°C, 1000 rpm / min, 30 min;

[0169] (5) Impact strength: carried out in accordance with the method specified in GB / T 1843, with the notch type being type A;

[0170] (6) Load deformation temperature: in accordance with the provisions of GB / T 1634.2, bending load is 1.80MPa, lying flat;

[0171] (7) Corrosion resistance: 50g / L NaOH and 50g / L H2SO4 solutions, immersed in water for 25 days at room temperature.

[0172] The test results are shown in Table 2 and Figure 3 and Figure 4 shown.

[0173] Table 2. Chromaticity, physical properties and chemical properties of each polyetheretherketone product

[0174]

[0175] It can be seen from the test results in Table 2 that the use of more purified 4,4'-difluorobenzophenone as a monomer, nitrogen with higher purity for atmosphere protection, and fine control of temperature and pressure can make the prepared polyetheretherketone have good chromaticity, its glass transition temperature and melting point are improved, and the 5% thermal weight loss temperature is significantly increased, the thermal stability is improved, the melt viscosity change is smaller, the load deformation temperature is increased, and there is no change after long-term immersion in strong acid and strong alkali, which fully proves that it has good product quality and stable physical and chemical properties, and can meet the use requirements of high-end products in the fields of aerospace, medical equipment, and electrical.

[0176] It is obvious to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be regarded as exemplary and non-restrictive from any point of view. In addition, it should be understood that although this specification is described in accordance with the implementation mode, it does not include only one technical solution. This narrative mode of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole, and the technical solutions in the embodiments can also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A high-performance polyetheretherketone fine synthesis process, Features: The steps include: 1) Synthesis and purification of high-purity 4,4'-difluorobenzophenone: Using para-fluorotrichlorotoluene and fluorobenzene as starting materials, in the presence of a mixture of trifluoromethanesulfonic acid and N,N-dimethyl-4-pyridinamine as a catalyst, an acylation reaction is carried out in an inert atmosphere to generate 4,4'-difluorophenyldichloromethane; then a hydrolysis reaction is carried out to generate 4,4'-difluorobenzophenone; then purification is carried out to remove the catalyst, unreacted starting materials and by-products, and 4,4'-difluorobenzophenone with a purity of ≥99.99% is obtained for standby use; 2) Nitrogen replacement to control oxygen concentration: The prepared 4,4'-difluorobenzophenone, hydroquinone, sodium carbonate and diphenyl sulfone are gas-displaced with nitrogen having a purity greater than 99.9995%, and the gas in the melting tank is replaced at the same time; the qualified materials are added to the corresponding melting tank after gas replacement in batches after accurate measurement through a single screw conveying and metering device, and nitrogen is continuously introduced for replacement to control the oxygen concentration to be less than 5ppm; 3) Material melting: After the oxygen concentration in the melting tank reaches the standard, heating is started to melt 4,4'-difluorobenzophenone, hydroquinone, and diphenyl sulfone respectively, and sodium carbonate is added to the melted diphenyl sulfone for standby use; 4) Synthesis of PEEK: The molten materials are added to the pre-substituted reactor in order, the molar ratio of the polymerization raw material monomer 4,4'-difluorobenzophenone and hydroquinone is controlled, the amount of sodium carbonate and diphenyl sulfone and the oxygen concentration in the reactor are controlled, stirring is started, and polymerization reaction is carried out to synthesize PEEK; During the reaction, the temperature and pressure gradients are precisely controlled, while the residence time of the reaction materials at each temperature gradient is controlled, and the material-liquid ratio of 4,4'-difluorobenzophenone and diphenyl sulfone is balanced; The gradient temperature increase and pressure increase is: The first gradient temperature is 150-180°C, the pressure is 0.1-0.5Mpa, and the reaction material residence time is 1-5 hours; The second gradient temperature is 250-280°C, the pressure is 0.3-0.8Mpa, and the reaction material residence time is 1-3 hours; The third gradient temperature is 300-320°C, the pressure is 1-1.5Mpa, and the reaction material residence time is 1-2 hours; 5) Determine the end point of the polymerization reaction: The torque force generated by the melt stirring in the reactor is detected by a torque sensor, thereby judging whether the polymerization reaction has reached the desired end point, thereby controlling the melt index of the synthesized polyetheretherketone; 6) End-capping refining: After the polymerization reaction reaches the desired end point, 4,4'-difluorobenzophenone is added as a capping agent to perform capping to complete the polymerization reaction; and then the reaction is refined to obtain high-performance polyetheretherketone.

2. The high-performance polyetheretherketone fine synthesis process according to claim 1, Features: In step 1), the specific process of synthesis and purification of high-purity 4,4'-difluorobenzophenone includes the following sub-steps: 1-1) Acylation reaction: In a nitrogen atmosphere, p-fluorotrichlorotoluene and fluorobenzene are mixed, cooled to 0-25° C., and then a mixture of trifluoromethanesulfonic acid and N,N-dimethyl-4-pyridinamine is added as a catalyst, and the reaction is carried out for 10-30 minutes to complete the acylation reaction to generate 4,4'-difluorophenyldichloromethane; 1-2) Hydrolysis reaction: 4,4'-difluorophenyl dichloromethane is mixed with water, heated to 100-110°C for azeotropic reaction, and hydrolyzed for 4-6 hours to obtain crude 4,4'-difluorobenzophenone; 1-3) Purification: After the hydrolysis reaction is completed, the crude 4,4'-difluorobenzophenone is purified by extraction, filtration, distillation and recrystallization to remove the catalyst, unreacted starting materials and by-products to obtain 4,4'-difluorobenzophenone with a purity of ≥99.99%.

3. The high-performance polyetheretherketone fine synthesis process according to claim 2, Features: In step 1-1), the molar ratio of p-fluorotrichlorotoluene to fluorobenzene is 1:3-5; the amount of the catalyst, trifluoromethanesulfonic acid, is 0.1-0.3 equivalents of the total molar amount of p-fluorotrichlorotoluene and fluorobenzene, and the amount of N,N-dimethyl-4-pyridinamine is 1-10% of the mass of trifluoromethanesulfonic acid.

4. The high-performance polyetheretherketone fine synthesis process according to claim 2, Features: 1-3) The specific process of the purification treatment is as follows: A. Extracting the catalyst: After the hydrolysis reaction is completed, the material is cooled to room temperature, and sodium carbonate with a weight of 2 to 3 times the total mass of the catalyst is added, and the catalyst is extracted by stirring at 200 to 500 rpm for 5 to 10 minutes; B. Distillation: Then centrifuge at 3000-5000 rpm for 2 min, take the middle organic phase for distillation, the distillation temperature is 275-280°C, and obtain 4,4'-difluorobenzophenone distillate; C. Recrystallization: Add 95% ethanol in an amount of 10 times the volume of 4,4'-difluorobenzophenone distillate, and stir for 5-10 minutes in a water bath at 80°C; then filter while hot, transfer the filtered hot solution to a crystallizer and gradually cool it at room temperature to crystallize 4,4'-difluorobenzophenone; D. Washing: After crystallization is completed, centrifuge at 2000-3000 rpm for 2 minutes, take the precipitate and add 95% ethanol to wash the crystals three times. The amount of 95% ethanol added each time is 1.5-2 times the volume of 4,4'-difluorobenzophenone crystals; E. Drying: After washing, place the 4,4'-difluorobenzophenone crystals in a vacuum drying oven at 60-80°C for more than 6 hours to ensure complete drying; F. Purity test: Check the purity of 4,4'-difluorobenzophenone after recrystallization, and the purity is qualified if it is ≥99.99%.

5. The high-performance polyetheretherketone fine synthesis process according to claim 1, Features: In step 4), the synthesis of PEEK, The order of adding the molten materials into the reactor is: first add the molten diphenyl sulfone and sodium carbonate into the reactor, and then add the polymerization raw material monomers 4,4'-difluorobenzophenone and hydroquinone into the reactor at the same time; The oxygen concentration is controlled to be less than 5 ppm; The molar ratio of the polymerization raw material monomers 4,4'-difluorobenzophenone and hydroquinone is 1:1 to 1.2; The sodium carbonate is used in a molar ratio of hydroquinone to sodium carbonate: hydroquinone: sodium carbonate = 1:2.3-2.5; The amount of diphenyl sulfone used is 2 to 4 times the volume of 4,4'-difluorobenzophenone.

6. The high-performance polyetheretherketone fine synthesis process according to claim 1, Features: In step 4), the gradient temperature increase and pressure increase is: First gradient: 150℃±5℃, 0.2Mpa, the reaction mass is retained for 1h; 160℃±5℃, 0.3Mpa, the reaction mass is retained for 0.5h; 170℃±5℃, 0.4Mpa, the reaction mass is retained for 0.5h; 180℃±5℃, 0.5Mpa, the reaction mass is retained for 1h; Second gradient: 250℃±5℃, 0.6Mpa, the reaction mass is retained for 1h; 260℃±5℃, 0.7Mpa, the reaction mass is retained for 0.5h; 270℃±5℃, 0.8Mpa, the reaction mass is retained for 0.5h; The third gradient: 300°C±2°C, 1 MPa, the reaction material is retained for 0.5 h; 310°C±2°C, 1.2 MPa, the reaction material is retained for 1 h.

7. The high-performance polyetheretherketone fine synthesis process according to claim 1, Features: In step 4), the balanced material-liquid ratio of 4,4'-difluorobenzophenone and diphenyl sulfone is specifically as follows: in the synthesis stage of the PEEK precursor, 8-10wt% of 4,4'-difluorobenzophenone, one of the polymerization monomer raw materials, is reserved, and in the second gradient stage of the gradient heating, when the temperature reaches 250°C, it is added in at least three batches to ensure the balance of the reaction material-liquid ratio and make the prepolymerization reaction stable.

8. The high-performance polyetheretherketone fine synthesis process according to claim 1, Features: In step 5), at the end point of the polymerization reaction, the melt index of polyetheretherketone is controlled to be 8 to 90 g / 10 min.

9. The high-performance polyetheretherketone fine synthesis process according to claim 1, Features: In step 6), the amount of the end-capping agent 4,4'-difluorobenzophenone added is 2% to 3% of the mass of the polymerized monomer 4,4'-difluorobenzophenone; The refining step is to directly introduce the polyetheretherketone melt into a supercritical carbon dioxide extraction device for extraction, and the specific extraction parameters are: The carbon dioxide flow rate is 50-60 kg / h·kg PEEK, the extraction pressure is 25-35 MPa, and the temperature is 345-365°C; The separation column pressure is 15-20 MPa, and the temperatures from bottom to top are 350°C, 355°C, 360°C, and 365°C; The first decomposition kettle has a pressure of 5.5-6.5 MPa and a temperature of 305°C; The second decomposition kettle has a pressure of 4.5-5.5 MPa and a temperature of 275°C; The extraction time was set at 180 min, and the polyetheretherketone extraction melt was taken out from the bottom of the separation column every 20 min for cooling and solidification to obtain high-performance polyetheretherketone.

Citation Information

Cited By

  • Process and equipment for synthesizing high-wear-resistance polyether-ether-ketone

    CN119708379A