A Mg 17 Al 12 Phase-reinforced magnesium-based composite material and preparation method thereof

Through the technology of nano-Zn powder coating micron Ti particles, the size and distribution of the Mg17Al12 precipitated phase are controlled, which solves the problems of precipitated phase brittleness and casting defects in Mg-9Al-1Zn alloy, and improves the strength and plasticity of magnesium-based composite materials.

CN118516594BActive Publication Date: 2024-10-01GUANGDONG INST OF NEW MATERIALS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410979003.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-10-01
Estimated Expiration
2044-07-22

AI Technical Summary

Technical Problem

The presence of coarse, network-distributed Mg17Al12 precipitates in Mg-9Al-1Zn alloy leads to brittleness and casting defects, affecting compactness and mechanical properties, and high Al content reduces elongation.

Method used

Micron Ti particles coated with nano-Zn powder are used as reinforcing particles, which are uniformly deposited through electric explosion deposition. Combined with low-energy ball milling, sintering and hot extrusion deformation processing, the size and distribution of the Mg17Al12 precipitated phase are controlled to form a high volume fraction of sub-micron particles. Grade precipitation phase to achieve dispersion precipitation strengthening and solid solution strengthening.

Benefits of technology

Significantly improve the tensile strength, yield strength and elongation of Mg17Al12 phase-reinforced magnesium-based composite materials, avoid the occurrence of cracks and defects, and improve the toughness and mechanical properties of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118516594B_ABST
    Figure CN118516594B_ABST
Patent Text Reader

Abstract

The invention discloses a Mg 17 Al 12 The invention discloses a phase-reinforced magnesium-based composite material and a preparation method thereof, belonging to the technical field of magnesium-based composite materials. The raw materials for preparing the magnesium-based composite material include reinforcing particles and a magnesium-aluminum-zinc alloy matrix, wherein the reinforcing particles are micron Ti particles coated with nano Zn powder; the magnesium-based composite material has long strips of Mg 17 Al 12 Precipitation phase; Mg 17 Al 12 The length of the precipitated phase is 0.1μm~1.5μm, and the width is 100nm~500nm; Mg 17 Al 12 The volume fraction of the precipitated phase in the magnesium-based composite material is 20% to 30%. The magnesium-based composite material can have high strength and plasticity at the same time. The preparation method comprises: subjecting a mixture of reinforcing particles and magnesium-aluminum-zinc alloy powder to low-energy ball milling, sintering, rapid cooling, homogenization heat treatment and hot extrusion deformation treatment. The method is simple, easy to operate and can be industrialized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of magnesium-based composite materials, and in particular to a magnesium-based composite material. 17 Al 12 Phase-reinforced magnesium-based composite material and preparation method thereof. Background Art

[0002] Mg-9Al-1Zn alloy is often used as a cast magnesium alloy. However, the cast Mg-9Al-1Zn alloy often has coarse and network-like Mg 17 Al 12 Precipitated phases, which are obviously brittle, are prone to crack initiation and expansion, and eventually lead to the fracture failure of magnesium alloy. In addition, a large number of casting defects, such as segregation, porosity, shrinkage, etc., will also affect the compactness and mechanical properties of Mg-9Al-1Zn alloy. Moreover, the higher Al content in Mg-9Al-1Zn alloy usually leads to a significant decrease in the elongation of the alloy.

[0003] Therefore, how to simultaneously improve the strength and plasticity of Mg-9Al-1Zn alloy has been a major research hotspot in recent years.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The object of the present invention is to provide a Mg 17 Al 12 Phase-reinforced magnesium-based composite materials and preparation methods thereof are provided to solve or improve the above technical problems.

[0006] The present invention can be implemented like this:

[0007] In a first aspect, the present invention provides a Mg 17 Al 12 Phase reinforced magnesium matrix composites, Mg 17 Al 12 The raw materials for preparing the phase-reinforced magnesium-based composite material include reinforcing particles and a magnesium-aluminum-zinc alloy matrix, wherein the reinforcing particles are micron Ti particles coated with nano Zn powder;

[0008] Mg 17 Al 12 Phase-reinforced magnesium matrix composites have long strips of Mg 17 Al 12 Precipitation phase; Mg 17 Al 12 The length of the precipitated phase is 0.1μm~1.5μm, and the width is 100nm~500nm; Mg 17 Al 12 The precipitate phase is Mg 17 Al 12The volume fraction of phase-reinforced magnesium-based composites is 20%~30%.

[0009] In an optional embodiment, in the preparation raw material, the amount of reinforcing particles is 0.5wt%~3wt%, and the balance is a magnesium-aluminum-zinc alloy matrix; the Al content in the magnesium-aluminum-zinc alloy matrix is ​​not less than 9wt%, and the Zn content is not less than 1wt%.

[0010] In an optional embodiment, the average particle size of the reinforcement particles is 10 μm to 20 μm; the magnesium-aluminum-zinc alloy matrix is ​​in powder form, and the average particle size of the magnesium-aluminum-zinc alloy matrix is ​​50 μm to 80 μm.

[0011] In an alternative embodiment, Mg 17 Al 12 The phase-reinforced magnesium matrix composite material has at least one of the following characteristics:

[0012] Feature 1: Mg 17 Al 12 The phase-reinforced magnesium-based composite material has a bimodal heterogeneous structure including a coarse-grained deformed grain region and a fine-grained dynamic recrystallization region;

[0013] Feature 2: Micron Ti particles are distributed on the interface of the magnesium-aluminum-zinc alloy matrix, and Zn element is solid-dissolved in the magnesium-aluminum-zinc alloy matrix;

[0014] Feature 3: Mg 17 Al 12 The tensile strength of the phase-reinforced magnesium-based composite material is not less than 355MPa;

[0015] Feature 4: Mg 17 Al 12 The yield strength of the phase-reinforced magnesium-based composite material is not less than 225MPa;

[0016] Feature 5: Mg 17 Al 12 The elongation of the phase-reinforced magnesium-based composite material is not less than 10%;

[0017] Feature 6: Mg 17 Al 12 The grain size of the phase-reinforced magnesium-based composite material is not higher than 6.2 μm.

[0018] In a second aspect, the present invention provides a Mg as in any one of the foregoing embodiments. 17 Al 12 The preparation method of phase-reinforced magnesium-based composite material comprises the following steps: subjecting a mixture of reinforcing particles and magnesium-aluminum-zinc alloy powder to low-energy ball milling to obtain composite powder; sintering the composite powder and rapidly cooling it to obtain a sintered body; subjecting the sintered body to homogenization treatment and hot extrusion deformation treatment to obtain Mg 17 Al12 Phase reinforced magnesium matrix composites.

[0019] In an optional embodiment, the preparation of the reinforced particles includes: depositing nano Zn powder on the surface of micron Ti particles by electric explosion deposition;

[0020] The mass of Zn powder is 5wt%~15wt% of Ti particles; the average particle size of Ti particles is 10μm~20μm, and the average particle size of Zn powder is 30nm~100nm;

[0021] The conditions for electric explosion deposition include: deposition voltage of 5Kev~8Kev and deposition distance of 25mm~30mm.

[0022] In an optional embodiment, the reinforced particles are mixed with the magnesium-aluminum-zinc alloy powder at a rotation speed of 50 r / min to 150 r / min for 3 h to 6 h to obtain a mixture.

[0023] In an optional embodiment, the conditions for low-energy ball milling include: a rotation speed of 120 r / min to 150 r / min, a ball-to-material ratio of 20:1 to 25:1, and a time of 1 h to 2 h.

[0024] In an optional embodiment, the sintering conditions include: a sintering temperature of 480° C. to 500° C., a sintering pressure of 40 MPa to 50 MPa, and a sintering time of 20 min to 30 min;

[0025] The rapid cooling after sintering is carried out under liquid nitrogen conditions, with a cooling rate of 100°C / min~200°C / min.

[0026] In an optional embodiment, the temperature of the homogenization treatment is 350°C~400°C, and the time is 30min~60min; the conditions of the hot extrusion deformation treatment include: the hot extrusion temperature is 360°C~400°C, the extrusion ratio is 15:1 to 25:1, and the extrusion speed is 0.3m / min~0.5m / min.

[0027] The beneficial effects of the present invention include:

[0028] The Mg provided by the present invention 17 Al 12 Phase-reinforced magnesium matrix composites have long strips of Mg 17 Al 12 Precipitation phase; Mg 17 Al 12 The length of the precipitated phase is 0.1μm~1.5μm, and the width is 100nm~500nm; Mg 17 Al 12 The precipitate phase is Mg 17 Al 12The volume fraction of the reinforced magnesium matrix composite material is 20%~30%. 17 Al 12 The size and content of the precipitated phase are controlled within the above range, so that Mg 17 Al 12 The precipitated phase is elongated and dispersed in the magnesium matrix composite with a high volume fraction, which avoids the Mg 17 Al 12 The precipitated phase is often coarse and distributed in a network pattern, which helps to avoid and reduce the occurrence of cracks and defects.

[0029] In addition, the present invention uses micron Ti particles coated with nano Zn powder as reinforcing particles, which can avoid the uneven distribution of Zn elements in the magnesium-aluminum-zinc alloy matrix, resulting in local segregation and forming hot brittle Mg. 51 Zn 20 , which seriously affects the toughness of the composite material. Zn element solid solution enters the magnesium aluminum zinc alloy matrix, which can reduce the solid solubility of Al element in the matrix and promote Mg 17 Al 12 Phase precipitation. After hot extrusion, Mg 17 Al 12 The phase is broken into submicron precipitate phase with high volume fraction, which can improve the strength and plasticity of the composite material simultaneously through dispersion precipitation strengthening, solid solution strengthening and fine grain strengthening.

[0030] Therefore, the Mg provided by the present invention 17 Al 12 Phase-reinforced magnesium-based composites can simultaneously have high tensile strength, yield strength and elongation. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0032] Figure 1 This is a longitudinal cross-sectional morphology diagram of the magnesium-based composite material prepared in Example 1;

[0033] Figure 2 This is a cross-sectional morphology diagram of the magnesium-based composite material prepared in Example 1;

[0034] Figure 3 This is a longitudinal cross-sectional morphology diagram of the magnesium-based composite material prepared in Comparative Example 1;

[0035] Figure 4 This is a longitudinal cross-sectional morphology diagram of the magnesium-based composite material prepared in Comparative Example 2;

[0036] Figure 5 This is a morphology of the submicron precipitate phase in the magnesium-based composite material prepared in Example 1;

[0037] Figure 6 for Figure 5 Medium Mg 17 Al 12 A magnified view of the coherent structure of the phase interface;

[0038] Figure 7 This is a morphology diagram of the precipitated phase in the magnesium-based composite material prepared in Comparative Example 2;

[0039] Figure 8 for Figure 7 Medium Mg 17 Al 12 A magnified view of the coherent structure of the phase interface;

[0040] Fig. 9 Tensile curves of the magnesium-based composite materials prepared in Example 1, Comparative Example 1 and Comparative Example 2. DETAILED DESCRIPTION

[0041] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0042] The Mg provided by the present invention is as follows 17 Al 12 The phase-reinforced magnesium-based composite material and its preparation method are specifically described.

[0043] The present invention proposes a Mg 17 Al 12 The invention discloses a phase-reinforced magnesium-based composite material, wherein the raw materials for preparing the composite material include reinforcing particles and a magnesium-aluminum-zinc alloy matrix. In the raw materials for preparing the composite material, the amount of the reinforcing particles is 0.5wt% to 3wt%, and the balance is the magnesium-aluminum-zinc alloy matrix.

[0044] Illustratively, the content of the reinforcing particles in the raw material can be 0.5wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt% or 3wt%, etc., or other values ​​within the range of 0.5wt% to 3wt%.

[0045] If the content of reinforcing particles in the raw material is higher than 3wt%, the stress concentration between the reinforcing particles may increase the brittleness of the material. At this time, too high a content of reinforcing particles may also cause the material to crack and break easily, thus affecting the hardness. Most importantly, the stress concentration between the reinforcing particles will accelerate the crack propagation, resulting in a shortened life of the material. Too high a content of reinforcing particles will reduce the plastic deformation capacity of the material, making it more prone to fracture.

[0046] The above-mentioned reinforcement particles are micron Ti particles coated with nano Zn powder.

[0047] It should be noted that the Zn element is prone to uneven distribution in the magnesium-aluminum-zinc alloy matrix, and local segregation forms hot brittle Mg 51 Zn 20 The present invention uses nano Zn to coat micron Ti particles to strengthen the magnesium-aluminum-zinc alloy matrix. The Zn is evenly distributed on the surface of the Ti particles, and the evenly distributed Zn element is then dissolved into the magnesium-aluminum-zinc alloy matrix, which can reduce the solid solubility of the Al element in the matrix and promote the Mg 17 Al 12 Phase precipitation. After hot extrusion, Mg 17 Al 12 The phase is broken into a submicron precipitate phase with a high volume fraction, which can simultaneously improve the strength and plasticity of the composite material through dispersion precipitation strengthening, solid solution strengthening and grain refinement strengthening.

[0048] The average particle size of the reinforcing particles is 10 μm to 20 μm, such as 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm or 20 μm, etc., and can also be other values ​​within the range of 10 μm to 20 μm.

[0049] If the average particle size of the reinforcement particles is less than 10 μm, it is not conducive to uniform surface coating of nano Zn powder; if the average particle size of the reinforcement particles is greater than 20 μm, the stress distribution between the particles may be uneven, resulting in some areas being subjected to higher stress and prone to fracture. When the particle size is larger, the interface between the particles and the matrix material may not be completely tightly bonded, which can easily form cracks and promote crack propagation.

[0050] In the reinforced particles, the mass of Zn powder is 5wt%~15wt% of the Ti particles, such as 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, 13wt%, 14wt% or 15wt%, etc., and can also be other values ​​within the range of 5wt%~15wt%.

[0051] If the mass of Zn powder in the reinforcement particles is less than 5wt%, the content of Zn element solid solution entering the magnesium-aluminum-zinc alloy matrix is ​​reduced, which is not conducive to the submicron Mg 17 Al 12 If the weight of Zn powder in the reinforcement particles is higher than 15wt%, it is not conducive to the uniform dispersion of Zn powder, and it is easy to aggregate and form hot brittle Mg 51 Zn 20 phase, which seriously affects the toughness of the composite material.

[0052] The average particle size of the Ti particles can be 10μm to 20μm, such as 10μm, 11μm, 12μm, 13μm, 14μm, 15μm, 16μm, 17μm, 18μm, 19μm or 20μm, or other values ​​within the range of 10μm to 20μm.

[0053] The average particle size of the Zn powder can be 30nm to 100nm, such as 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm or 100nm, etc., or other values ​​within the range of 30nm to 100nm. Of course, the average particle size of the Ti particles is smaller than the average particle size of the reinforcing particles.

[0054] In the present invention, the content of Al in the magnesium-aluminum-zinc alloy matrix is ​​not less than 9wt%, such as 9wt%, 10wt%, 12wt% or higher. The content of Zn in the magnesium-aluminum-zinc alloy matrix is ​​not less than 1wt%, such as 1wt%, 2wt% or higher.

[0055] In some typical implementations, the Al content in the magnesium-aluminum-zinc alloy matrix is ​​9wt%, the Zn content is 1wt%, and the balance is mainly Mg.

[0056] In some embodiments, the magnesium-aluminum-zinc alloy matrix is ​​in powder form, and the average particle size of the magnesium-aluminum-zinc alloy matrix can be 50μm~80μm, such as 50μm, 55μm, 60μm, 65μm, 70μm, 75μm or 80μm, etc., or other values ​​within the range of 50μm~80μm.

[0057] The Mg provided by the present invention 17 Al 12 Phase-reinforced magnesium matrix composites have long strips of Mg 17 Al 12 The Mg 17 Al 12The length of the precipitated phase is 0.1μm~1.5μm (such as 0.1μm, 0.2μm, 0.5μm, 0.8μm, 1.0μm, 1.2μm or 1.5μm, etc.), and the width is 100nm~500nm (such as 100nm, 200nm, 300nm, 400nm or 500nm, etc.); the Mg 17 Al 12 The precipitate phase is Mg 17 Al 12 The volume fraction of the phase-reinforced magnesium-based composite material is 20%~30%, such as 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29% or 30%.

[0058] By adding Mg 17 Al 12 The size and content of the precipitated phase are controlled within the above range, so that Mg 17 Al 12 The precipitated phase is elongated and dispersed in the magnesium matrix composite with a high volume fraction, which avoids the Mg 17 Al 12 The precipitated phase is often coarse and distributed in a network pattern, which helps to avoid and reduce the occurrence of cracks and defects.

[0059] The Mg provided by the present invention 17 Al 12 The phase-reinforced magnesium-based composite material has a bimodal isomorphous structure including a coarse-grained deformed grain region and a fine-grained dynamic recrystallization region. Micron Ti particles are distributed on the interface of the magnesium-aluminum-zinc alloy matrix, and Zn elements are solid-dissolved in the magnesium-aluminum-zinc alloy matrix.

[0060] In the present invention, micron Ti particles are distributed on the interface of Mg-Al matrix powder, and the nano Zn element on the surface is dissolved into the magnesium-aluminum-zinc alloy matrix, which reduces the solid solubility of Al element and promotes the submicron Mg 17 Al 12 The phase precipitates with Ti particles as nucleation sites, and a high volume fraction of submicron-sized Mg 17 Al 12 The precipitated phase and micronized Ti particles hinder the movement of dislocations, thereby improving the strength of the composite material. 17 Al 12 The precipitated phase promotes the occurrence of dynamic recrystallization, hinders the migration and growth of grain boundaries, refines the grains, and significantly improves the toughness of the composite material.

[0061] In some embodiments, the Mg 17 Al 12 The tensile strength of the phase-reinforced magnesium-based composite material is not less than 355 MPa, such as 355 MPa to 380 MPa.

[0062] In some embodiments, the Mg 17 Al 12 The yield strength of the phase-reinforced magnesium-based composite material is not less than 225 MPa, such as 226 MPa~250 MPa.

[0063] In some embodiments, the Mg 17 Al 12 The elongation of the phase-reinforced magnesium-based composite material is not less than 10%, for example, it can be 10% to 16%.

[0064] In some embodiments, the Mg 17 Al 12 The grain size of the phase-reinforced magnesium-based composite material is not higher than 6.2 μm, for example, it can be 3.5 μm to 6.2 μm.

[0065] As above, the Mg 17 Al 12 Phase-reinforced magnesium-based composites can simultaneously have high tensile strength, yield strength and elongation.

[0066] The composite material has a high volume fraction dispersed submicron Mg 17 Al 12 , and the grains of the composite material are also significantly refined. Compared with micron Ti particle reinforced Mg-Al-Zn and original Mg-Al-Zn alloy, the mechanical properties are significantly improved. The strength of the composite material is improved by precipitation strengthening, solid solution strengthening and grain refinement. The formation of bimodal isomerization increases the storage energy of the grains, and the submicron Mg 17 Al 12 The precipitated phase hinders the crack propagation and helps to improve the toughness.

[0067] Accordingly, the present invention also provides a kind of above-mentioned Mg 17 Al 12 The preparation method of the phase-reinforced magnesium-based composite material comprises the following steps: subjecting a mixture of reinforcing particles and magnesium-aluminum-zinc alloy powder to low-energy ball milling to obtain composite powder; subjecting the composite powder to sintering and rapid cooling to obtain a sintered body; subjecting the sintered body to homogenization and hot extrusion deformation to obtain a submicron Mg 17 Al 12 Phase reinforced magnesium matrix composites.

[0068] In some embodiments, the preparation of the reinforced particles may include: depositing nano Zn powder on the surface of micron Ti particles by electric explosion deposition.

[0069] The conditions for electric explosion deposition include: deposition voltage of 5Kev~8Kev and deposition distance of 25mm~30mm.

[0070] The deposition voltage may be 5 Kev, 5.5 Kev, 6 Kev, 6.5 Kev, 7 Kev, 7.5 Kev or 8 Kev, or other values ​​within the range of 5 Kev to 8 Kev.

[0071] The deposition distance may be 25 mm, 26 mm, 27 mm, 28 mm, 29 mm or 30 mm, or other values ​​within the range of 25 mm to 30 mm.

[0072] The present invention adopts the method of electric explosion deposition to prepare the reinforced particles, and controls the deposition voltage and deposition distance within the above range, so that the nano Zn powder with the size and amount specified in the present invention can be uniformly deposited and coated on the surface of the micron Ti particles, effectively avoiding the uneven distribution of Zn that will cause local segregation to form hot brittle Mg 51 Zn 20 And affect the toughness of the composite material.

[0073] In some embodiments, the reinforcing particles and the magnesium-aluminum-zinc alloy powder may be mixed at a rotation speed of 50 r / min to 150 r / min for 3 h to 6 h to obtain a mixture.

[0074] The mixing speed may be 50 r / min, 80 r / min, 100 r / min, 120 r / min or 150 r / min, or other values ​​within the range of 50 r / min to 150 r / min.

[0075] The mixing time can be 3 h, 3.5 h, 4 h, 4.5 h, 5 h, 5.5 h or 6 h, etc., or other values ​​within the range of 3 h to 6 h.

[0076] In some embodiments, the conditions of low-energy ball milling include: a rotation speed of 120 r / min to 150 r / min, a ball-to-material ratio of 20:1 to 25:1, and a time of 1 h to 2 h.

[0077] Among them, the rotation speed of the low-energy ball mill can be 120r / min, 125r / min, 130r / min, 135r / min, 140r / min, 145r / min or 150r / min, etc., or other values ​​within the range of 120r / min~150r / min.

[0078] The ball-to-material ratio can be 20:1, 21:1, 22:1, 23:1, 24:1 or 25:1, etc., or other values ​​within the range of 20:1 to 25:1.

[0079] The low-energy ball milling time can be 1 h, 1.5 h or 2 h, etc., or other values ​​within the range of 1 h to 2 h.

[0080] The present invention adopts low-energy ball milling, which is conducive to the uniform distribution of Zn element on the surface of the matrix powder, solid solution into the magnesium alloy, reducing the content of aluminum element, and promoting the submicron Mg 17 Al 12 If high-energy ball milling is used, the powder will be flattened by the grinding balls, and the prepared composite material will easily lead to high porosity, which is not conducive to the close bonding between powders. High-energy ball milling will introduce mechanical stress, which may cause microcracks and dislocations inside the material, affecting the mechanical properties and stability of the material.

[0081] In some embodiments, the sintering conditions include: a sintering temperature of 480° C. to 500° C., a sintering pressure of 40 MPa to 50 MPa, and a sintering time of 20 min to 30 min.

[0082] The sintering temperature may be 480°C, 485°C, 490°C, 495°C or 500°C, or other values ​​within the range of 480°C to 500°C.

[0083] The sintering pressure may be 40 MPa, 42 MPa, 45 MPa, 48 MPa or 50 MPa, etc., or other values ​​within the range of 40 MPa to 50 MPa.

[0084] The sintering time can be 20 min, 25 min or 30 min, etc., or other values ​​within the range of 20 min to 30 min.

[0085] The rapid cooling after sintering is carried out under liquid nitrogen conditions, and the cooling rate can be 100°C / min~200°C / min, such as 100°C / min, 120°C / min, 140°C / min, 160°C / min, 180°C / min or 200°C / min, or other values ​​within the range of 100°C / min~200°C / min.

[0086] If the cooling speed after sintering is too slow, the dissolved Al and Zn elements will not be able to precipitate to form fine Mg 17 Al 12 In some embodiments, the temperature of the homogenization treatment is 350°C to 400°C, such as 350°C, 360°C, 370°C, 380°C, 390°C or 400°C, or other values ​​within the range of 350°C to 400°C.

[0087] The homogenization treatment time may be 30 min to 60 min, such as 30 min, 40 min, 50 min or 60 min, etc., or may be other values ​​within the range of 30 min to 60 min.

[0088] If homogenization treatment is not performed before hot extrusion deformation treatment, it is easy to cause the following problems: ① Internal stress accumulation: The hot extrusion process will cause internal stress accumulation, which will affect the performance and stability of the composite material. ② Non-uniform distribution of grains: The grains of metal materials that have not been homogenized may be uneven, which may cause grain distortion and instability during hot extrusion. ③ Poor surface quality: Materials that have not been homogenized may have defects such as inclusions, which may be aggravated during hot extrusion, resulting in poor surface quality of the product.

[0089] In some embodiments, the conditions of the hot extrusion deformation treatment include: a hot extrusion temperature of 360° C. to 400° C., an extrusion ratio of 15:1 to 25:1, and an extrusion speed of 0.3 m / min to 0.5 m / min.

[0090] The hot extrusion temperature may be 360°C, 370°C, 380°C, 390°C or 400°C, or other values ​​within the range of 360°C to 400°C.

[0091] If the hot extrusion temperature is higher than 400℃, the excessively high hot extrusion temperature may cause the material to overheat. Overheating will cause the grains of the metal material to grow and the grain boundaries to become unclear. Excessively high hot extrusion temperatures may also cause the local temperature of the material to be too high, resulting in excessive thermal stress in the material, which in turn leads to thermal cracks. Excessively high hot extrusion temperatures will also cause abnormal metallographic structures of metal materials, grain growth, and decreased grain boundary clarity, thereby reducing the hardness and strength of the material.

[0092] The extrusion ratio may be 15:1, 18:1, 20:1, 22:1 or 25:1, etc., or other values ​​within the range of 15:1 to 25:1.

[0093] The extrusion speed may be 0.3 m / min, 0.35 m / min, 0.4 m / min, 0.45 m / min or 0.5 m / min, etc., or other values ​​within the range of 0.3 m / min to 0.5 m / min.

[0094] As mentioned above, Zn diffuses into the Mg-Al-Zn alloy matrix during hot pressing and sintering to produce solid solution strengthening. During the cooling process, Mg 17 Al 12 The phase forms a precipitate and then is deformed by hot extrusion to form a fine size.

[0095] It should be noted that in the extruded Mg-9Al-1Zn alloy, the main precipitates are Mg 17 Al 12 and Al8Mn5. The size, distribution and grain size of these precipitated phases have a great influence on the mechanical properties of the composite material. 17 Al 12 The Ti / Mg-9Al-1Zn composites have the effect of Al8Mn5 precipitation phase, but the grain size of the Ti / Mg-9Al-1Zn composites increases, resulting in a significant decrease in yield strength and hardness. Therefore, Ti particles cannot absolutely improve the comprehensive properties of magnesium-based composites.

[0096] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0097] Example 1

[0098] This embodiment provides a high volume fraction dispersed submicron Mg 17 Al 12 Phase-reinforced magnesium-based composite material, the preparation method of which comprises:

[0099] S1: Nano Zn powder was deposited on the surface of micron Ti particles by electric explosion deposition to obtain reinforced particles with an average particle size of 10.12 μm.

[0100] The mass of the nano Zn powder is 10wt% of the Ti particles; the average particle size of the Ti particles is 10μm, and the average particle size of the Zn powder is 30nm. The deposition voltage of the electric explosion deposition is 8Kev, and the deposition distance is 25mm.

[0101] S2: The reinforced particles and Mg-9Al-1Zn alloy powder with an average particle size of 50 μm were mixed in a double cone mixer at a mass ratio of 2:98 at a rotation speed of 100 r / min for 3 hours to obtain a mixture.

[0102] S3: The mixture was subjected to low-energy ball milling for 2 h at a ball-to-material ratio of 20:1 and a rotation speed of 150 r / min to obtain a composite powder.

[0103] S4: hot-pressing and sintering the composite powder, and rapidly cooling the composite powder to room temperature under liquid nitrogen conditions to obtain a sintered body.

[0104] The hot pressing sintering temperature is 500° C., the hot pressing sintering pressure is 50 MPa, and a sintered part is obtained. The hot pressing sintering time is 30 min, and the cooling rate is 200° C. / min.

[0105] S5: The sintered part is homogenized at a temperature of 350°C for 30 minutes; then it is subjected to hot extrusion deformation at a temperature of 400°C, an extrusion ratio of 20:1, and an extrusion speed of 0.5 m / min to obtain a high volume fraction dispersed submicron Mg 17 Al 12 Phase reinforced magnesium matrix composites.

[0106] Example 2

[0107] The difference between this embodiment and embodiment 1 is that the mass of the nano Zn powder is 15wt% of the Ti particles.

[0108] Example 3

[0109] The difference between this embodiment and embodiment 1 is that the average particle size of the nano Zn powder is 80 nm.

[0110] Example 4

[0111] The difference between this embodiment and embodiment 1 is that the average particle size of the micron Ti particles is 15 μm.

[0112] Example 5

[0113] The difference between this embodiment and embodiment 1 is that the cooling rate of hot pressing sintering is 150° C. / min.

[0114] Example 6

[0115] The difference between this embodiment and embodiment 1 is that the hot extrusion temperature is 380°C.

[0116] Example 7

[0117] This embodiment provides a high volume fraction dispersed submicron Mg 17 Al 12 Phase-reinforced magnesium-based composite material, the preparation method of which comprises:

[0118] S1: Nano Zn powder was deposited on the surface of micron Ti particles by electric explosion deposition to obtain reinforced particles with an average particle size of 15.10.

[0119] The mass of the nano Zn powder is 5wt% of the Ti particles; the average particle size of the Ti particles is 15μm, and the average particle size of the Zn powder is 50nm. The deposition voltage of the electric explosion deposition is 7Kev, and the deposition distance is 28mm.

[0120] S2: The reinforced particles and Mg-9Al-1Zn alloy powder with an average particle size of 50 μm were mixed in a double cone mixer at a mass ratio of 0.5:99.5 at a rotation speed of 50 r / min for 6 hours to obtain a mixture.

[0121] S3: The mixture was subjected to low-energy ball milling for 1.5 h at a ball-to-material ratio of 25:1 and a rotation speed of 120 r / min to obtain a composite powder.

[0122] S4: hot-pressing and sintering the composite powder, and rapidly cooling the composite powder to room temperature under liquid nitrogen conditions to obtain a sintered body.

[0123] The hot pressing sintering temperature is 480° C., the hot pressing sintering pressure is 40 MPa, and a sintered part is obtained. The hot pressing sintering time is 25 min, and the cooling rate is 150° C. / min.

[0124] S5: The sintered part is homogenized at a temperature of 370°C for 60 minutes; then it is subjected to hot extrusion deformation at a temperature of 360°C, an extrusion ratio of 15:1, and an extrusion speed of 0.3 m / min to obtain a high volume fraction dispersed submicron Mg 17 Al 12 Phase reinforced magnesium matrix composites.

[0125] Example 8

[0126] This embodiment provides a high volume fraction dispersed submicron Mg 17 Al 12 Phase-reinforced magnesium-based composite material, the preparation method of which comprises:

[0127] S1: Nano Zn powder was deposited on the surface of micron Ti particles by electric explosion deposition to obtain reinforced particles with an average particle size of 19.2.

[0128] The mass of the nano Zn powder is 10wt% of the Ti particles; the average particle size of the Ti particles is 19μm, and the average particle size of the Zn powder is 100nm. The deposition voltage of the electric explosion deposition is 6Kev, and the deposition distance is 30mm.

[0129] S2: The reinforced particles and Mg-9Al-1Zn alloy powder with an average particle size of 60 μm were mixed in a double cone mixer at a mass ratio of 3:97 at a rotation speed of 150 r / min for 4 hours to obtain a mixture.

[0130] S3: The mixture was subjected to low-energy ball milling for 1 h at a ball-to-material ratio of 20:1 and a rotation speed of 140 r / min to obtain a composite powder.

[0131] S4: hot-pressing and sintering the composite powder, and rapidly cooling the composite powder to room temperature under liquid nitrogen conditions to obtain a sintered body.

[0132] The hot pressing sintering temperature is 500° C., the hot pressing sintering pressure is 45 MPa, and a sintered part is obtained. The hot pressing sintering time is 20 min, and the cooling rate is 100° C. / min.

[0133] S5: The sintered part is homogenized at a temperature of 400°C for 40 minutes; then hot extrusion deformation is performed at a temperature of 400°C, an extrusion ratio of 25:1, and an extrusion speed of 0.4 m / min to obtain a high volume fraction dispersed submicron Mg 17 Al 12 Phase reinforced magnesium matrix composites.

[0134] Comparative Example 1

[0135] The difference between this comparative example and Example 1 is that pure Mg-9Al-1Zn alloy powder is selected for ball milling, hot pressing sintering, rapid cooling, homogenization treatment and hot extrusion deformation treatment.

[0136] That is, the preparation raw material is only a magnesium-aluminum-zinc alloy matrix, and no reinforcing particles are used.

[0137] Comparative Example 2

[0138] The difference between this comparative example and Example 1 is that the Mg-9Al-1Zn alloy is reinforced with micron Ti particles.

[0139] That is, the preparation raw materials include reinforcement particles and a magnesium-aluminum-zinc alloy matrix, but the reinforcement particles are only micron Ti particles, and the surfaces of the micron Ti particles are not coated with nano Zn powder.

[0140] Comparative Example 3

[0141] The difference between this comparative example and Example 1 is that the average particle size of the Zn powder is 1 μm.

[0142] Comparative Example 4

[0143] The difference between this comparative example and Example 1 is that the average particle size of the Ti particles is 25 μm.

[0144] Comparative Example 5

[0145] The difference between this comparative example and Example 1 is that the mass of Zn powder is 3wt% of the Ti particles.

[0146] Comparative Example 6

[0147] The difference between this comparative example and Example 1 is that the mass of Zn powder is 20wt% of the Ti particles.

[0148] Comparative Example 7

[0149] The difference between this comparative example and Example 1 is that the average particle size of the reinforcing particles is 5 μm.

[0150] Comparative Example 8

[0151] The difference between this comparative example and Example 1 is that the content of the reinforcing particles in the preparation raw material is 5wt%.

[0152] Comparative Example 9

[0153] The difference between this comparative example and Example 1 is that: the nano Zn powder is deposited on the surface of the micron Ti particles by gas phase spraying, and the spraying conditions include: the spraying temperature is 500°C.

[0154] Comparative Example 10

[0155] The difference between this comparative example and Example 1 is that the ball milling speed is 600 r / min.

[0156] Comparative Example 11

[0157] The difference between this comparative example and Example 1 is that the cooling rate after hot pressing sintering is 10° C. / min.

[0158] Comparative Example 12

[0159] The difference between this comparative example and Example 1 is that the hot extrusion temperature is 500°C.

[0160] Comparative Example 13

[0161] The difference between this comparative example and Example 1 is that no homogenization treatment is performed before the hot extrusion deformation treatment.

[0162] Comparative Example 14

[0163] The difference between this comparative example and Example 1 is that the Al content in the magnesium-aluminum-zinc alloy matrix is ​​less than 9wt%, and the Zn content is less than 1wt%, specifically, the magnesium-aluminum-zinc alloy matrix is ​​Mg-3Al-1Zn.

[0164] Test example

[0165] ① Taking Examples 1 to 8 as an example, the obtained magnesium-based composite material was subjected to SEM and TEM tests to obtain the size and volume fraction of the precipitated phase for statistical analysis. The results showed that the magnesium-based composite material had long strips of Mg 17 Al 12 Precipitation phase; Mg 17 Al 12 The length of the precipitated phase is 0.1μm~1.5μm, and the width is 100nm~500nm; Mg 17 Al 12 The precipitate phase is Mg 17 Al 12 The volume fraction of reinforced magnesium-based composites is 20%~30%.

[0166] ②. The grain size statistics and mechanical property tests of the magnesium-based composite materials obtained in Examples 1 to 8 and Comparative Examples 1 to 14 were performed. The results are shown in Table 1.

[0167] Among them, the tensile strength, yield strength and elongation are tested in accordance with "GB / T 228.1-2021".

[0168] Table 1 Mechanical properties test results

[0169]

[0170] It can be seen from Table 1 that the magnesium-based composite material provided by the present invention can simultaneously have high tensile strength, yield strength and elongation.

[0171] ③. Taking the magnesium-based composite materials prepared in Example 1, Comparative Example 1 and Comparative Example 2 as examples, they are respectively denoted as Zn@Ti / Mg-9Al-1Zn, Ti / Mg-9Al-1Zn and Mg-9Al-1Zn. The morphology of the magnesium-based composite material of Example 1 is shown in FIG. Figure 1 and Figure 2 As shown, the morphology of the magnesium-based composite material of Comparative Example 1 is as shown Figure 3 As shown, the morphology of the magnesium-based composite material of Comparative Example 2 is as follows Figure 4 shown.

[0172] Depend on Figures 1 to 4 It can be seen that the Mg precipitated in Mg-9Al-1Zn and Ti / Mg-9Al-1Zn 17 Al 12 The phase is relatively coarse, and the Mg precipitated in Zn@Ti / Mg-9Al-1Zn 17 Al 12 The phase is at submicron level and is distributed relatively evenly.

[0173] The morphology of the submicron precipitate phase in the magnesium-based composite material of Example 1 is as follows: Figure 5 and Figure 6 As shown, the morphology of the submicron precipitate phase in the magnesium-based composite material of Comparative Example 2 is as follows Figures 7 and 8 shown.

[0174] Depend on Figures 5 to 8 It can be seen that the Mg of Ti / Mg-9Al-1Zn composite material 17 Al 12 The size of the precipitated phase is micrometer level, the interface between the precipitated phase and the magnesium alloy matrix is ​​not smooth, and there is no obvious orientation relationship. 17 Al 12Phase, the size is nanometer level, the precipitation phase interface has a good coherent relationship with the magnesium alloy matrix, the interface is tightly bonded, and there is only one layer of dislocation on the interface, which is conducive to the transfer of load on the interface.

[0175] The tensile curves of the magnesium-based composite materials prepared in Example 1, Comparative Example 1 and Comparative Example 2 are shown in FIG. Fig. 9 shown.

[0176] Depend on Fig. 9 It can be seen that compared with Mg-9Al-1Zn and Ti / Mg-9Al-1Zn, the strength and plasticity of Zn@Ti / Mg-9Al-1Zn composite materials are improved simultaneously.

[0177] In summary, the present invention adopts nano Zn surface coated with micron Ti particles to strengthen Mg-9Al-1Zn, and the uniformly distributed Zn element solid dissolves into the Mg-9Al-1Zn matrix, which reduces the solid solubility of Al element in the matrix and promotes Mg 17 Al 12 Phase precipitation. After hot extrusion, Mg 17 Al 12 Phase fragmentation is called submicron precipitation phase with high volume fraction. Dispersion precipitation strengthening, solid solution strengthening and fine grain strengthening can improve the strength and plasticity of composite materials at the same time.

[0178] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A kind of Mg 17 Al 12 Phase-reinforced magnesium-based composite material, characterized in that: The Mg 17 Al 12 The raw materials for preparing the phase-reinforced magnesium-based composite material include reinforcing particles and a magnesium-aluminum-zinc alloy matrix, wherein the reinforcing particles are micron Ti particles coated with nano Zn powder; In the raw materials, the amount of the reinforcing particles is 0.5wt%~3wt%, and the balance is the magnesium-aluminum-zinc alloy matrix; the content of Al in the magnesium-aluminum-zinc alloy matrix is ​​not less than 9wt%, and the content of Zn is not less than 1wt%; the mass of the Zn powder is 5wt%~15wt% of the Ti particles; the Mg 17 Al 12 Phase-reinforced magnesium matrix composites have long strips of Mg 17 Al 12 Precipitation phase; the Mg 17 Al 12 The length of the precipitated phase is 0.1 μm to 1.5 μm, and the width is 100 nm to 500 nm; the Mg 17 Al 12 The precipitated phase 17 Al 12 The volume fraction of phase-reinforced magnesium-based composites is 20%~30%.

2. Mg according to claim 1 17 Al 12 Phase-reinforced magnesium-based composite material, characterized in that: The average particle size of the reinforcement particles is 10 μm to 20 μm; the magnesium-aluminum-zinc alloy matrix is ​​in powder form, and the average particle size of the magnesium-aluminum-zinc alloy matrix is ​​50 μm to 80 μm.

3. Mg according to claim 1 or 2 17 Al 12 Phase-reinforced magnesium-based composite material, characterized in that: The Mg 17 Al 12 The phase-reinforced magnesium matrix composite material has at least one of the following characteristics: Feature 1: The Mg 17 Al 12 The phase-reinforced magnesium-based composite material has a bimodal heterogeneous structure including a coarse-grained deformed grain region and a fine-grained dynamic recrystallization region; Feature 2: Micron Ti particles are distributed on the interface of the magnesium-aluminum-zinc alloy matrix, and Zn element is solid-dissolved in the magnesium-aluminum-zinc alloy matrix; Feature 3: The Mg 17 Al 12 The tensile strength of the phase-reinforced magnesium-based composite material is not less than 355MPa; Feature 4: The Mg 17 Al 12 The yield strength of the phase-reinforced magnesium-based composite material is not less than 225MPa; Feature 5: The Mg 17 Al 12 The elongation of the phase-reinforced magnesium-based composite material is not less than 10%; Feature 6: The Mg 17 Al 12 The grain size of the phase-reinforced magnesium-based composite material is not higher than 6.2 μm.

4. A Mg as described in any one of claims 1 to 3 17 Al 12 A method for preparing a phase-reinforced magnesium-based composite material, characterized in that: The following steps are involved: The mixture of the reinforcing particles and the magnesium-aluminum-zinc alloy powder is subjected to low-energy ball milling to obtain a composite powder; the composite powder is sintered and rapidly cooled to obtain a sintered body; the sintered body is subjected to homogenization treatment and hot extrusion deformation treatment to obtain Mg 17 Al 12 Phase reinforced magnesium matrix composites; The preparation of the enhanced particles comprises: depositing nano Zn powder on the surface of micron Ti particles by electric explosion deposition; Wherein, the average particle size of the Ti particles is 10 μm to 20 μm, and the average particle size of the Zn powder is 30 nm to 100 nm; The conditions of electric explosion deposition include: deposition voltage of 5Kev~8Kev, deposition distance of 25mm~30mm; The rapid cooling after sintering is carried out under liquid nitrogen conditions, with a cooling rate of 100℃ / min~200℃ / min; The hot extrusion temperature is 360℃~400℃.

5. The preparation method according to claim 4, characterized in that: The reinforcing particles and the magnesium-aluminum-zinc alloy powder are mixed at a rotation speed of 50 r / min to 150 r / min for 3 h to 6 h to obtain the mixture.

6. The preparation method according to claim 4, characterized in that: The conditions for low-energy ball milling include: rotation speed of 120r / min~150r / min, ball-to-material ratio of 20:1 to 25:1, and time of 1h~2h.

7. The preparation method according to claim 4, characterized in that: The sintering conditions include: sintering temperature of 480°C to 500°C, sintering pressure of 40MPa to 50MPa, and sintering time of 20min to 30min.

8. The preparation method according to claim 4, characterized in that: The temperature of homogenization treatment is 350℃~400℃, and the time is 30min~60min; The conditions of the hot extrusion deformation treatment include: an extrusion ratio of 15:1 to 25:1, and an extrusion speed of 0.3 m / min to 0.5 m / min.