A high-uniformity lignin nanobottle and its preparation method and application

Through the method of ultrasonic dissolution and heating and stirring self-assembly in γ-valerolactone, lignin nanobottles with uniform size are prepared, which solves the problem of poor size uniformity in the existing technology and realizes the efficient preparation of nanobottles and biomedicine. Application functionality improvements.

CN118530473BActive Publication Date: 2024-10-01QILU UNIVERSITY OF TECHNOLOGY (SHANDONG ACADEMY OF SCIENCES)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411010641.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-10-01
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

It is difficult to prepare lignin nanobottles with uniform size using existing technology, which affects their functionality and effectiveness in biomedical applications.

Method used

The lignin raw material is dissolved in γ-valerolactone by ultrasonic, and is added dropwise to the γ-valerolactone aqueous solution under heating and stirring conditions at a constant speed for self-assembly. The ultrasonic power, time, heating temperature and stirring speed are adjusted, combined with dialysis. Steps to prepare lignin nanobottles with uniform sizes.

Benefits of technology

The size uniformity of the lignin nanobottle is achieved. The particle size is between 50 and 500 nm. The bottle mouth size is adjustable between 10 and 200 nm. The polydispersity coefficient is less than 0.1. It is suitable for high-end applications such as bioengineering and drug carriers. Improved economic efficiency and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118530473B_ABST
    Figure CN118530473B_ABST
Patent Text Reader

Abstract

The present invention discloses a high-uniformity lignin nanobottle and its preparation method and application, belonging to the technical field of natural polymer nanomaterial preparation. The preparation method provided by the present invention comprises the following steps: mixing γ-valerolactone and water in a volume ratio of 4: (4~10) to form a γ-valerolactone aqueous solution; ultrasonically dissolving the lignin raw material in γ-valerolactone, filtering to obtain a γ-valerolactone solution of lignin; adding the γ-valerolactone solution of lignin to the γ-valerolactone aqueous solution at a uniform speed under heating and stirring conditions for self-assembly, that is. The self-assembly process of the lignin nanobottle of the present invention is simple, and there is no need to grade, modify or purify the starting lignin solution. The prepared nanobottle can be used as a nanocarrier, and its size uniformity is very high, and the polydispersity coefficient is less than 0.1, and it has good application prospects in high-end application fields such as bioengineering, drug carriers, intelligent phase change materials, and selective catalytic reactions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of natural polymer nanomaterial preparation, and in particular to a high-uniformity lignin nanobottle and a preparation method and application thereof. Background Art

[0002] The information disclosed in the background of the invention is only intended to enhance the understanding of the overall background of the invention and should not be necessarily regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] Lignin is the only renewable natural aromatic polymer in nature, and it is widely available, green, non-toxic and harmless. At present, industrial lignin is mainly produced in the pulp and papermaking process and the bioethanol refining industry. These lignins are currently mainly burned to provide heat. Micro-nano processing of lignin can achieve high-value utilization of lignin. The π-π stacking and hydrogen bonding between lignin molecules lead to the formation of micro-nanospheres. In the process of preparing nano-lignin using the solvent replacement method, due to the intermolecular interaction between the good solvent and the bad solvent, the lignin molecules will aggregate into nanospheres. Therefore, different solvents affect the formation of micro-nanoparticles with different structures by the solvent exchange method. For example, when nano-lignin is prepared using lignin and ethylene glycol solution, regular nanospheres cannot be obtained. In addition, most of the nano-lignin prepared using industrial lignin as raw materials are irregular nanoparticles or isotropic lignin nanospheres.

[0004] Nanobottles refer to colloidal particles that are hollow inside and have only one opening on the wall. Their unique morphological characteristics make them ideal carriers for loading, encapsulating, releasing and delivering various types of therapeutic diagnostic agents in a series of biomedical applications. Currently, only the patent with publication number CN117843991A reports the preparation method of lignin nanobottles. However, the size uniformity of lignin nanobottles prepared by the method provided by the patent is not ideal, and the sizes of the prepared nanobottles vary greatly. In practical applications, the size uniformity of nanobottles may have a great impact on their application effects. Obtaining nanobottles with controllable and uniform sizes is a necessary condition for improving their functional applications. Therefore, how to provide a preparation method for lignin nanobottles with high uniformity is an urgent problem to be solved. Summary of the invention

[0005] In view of this, the present invention provides a high-uniformity lignin nanobottle and a preparation method and application thereof, which solves the problem of poor size uniformity of nanobottles prepared by existing preparation methods.

[0006] In a first aspect, the present invention provides a method for preparing a high-uniformity lignin nanobottle, comprising the following steps:

[0007] Mixing γ-valerolactone and water in a volume ratio of 4:(4-10) to form a γ-valerolactone aqueous solution;

[0008] dissolving the lignin raw material in γ-valerolactone by ultrasonication, and filtering to obtain a γ-valerolactone solution of lignin;

[0009] Under heating and stirring conditions, the γ-valerolactone solution of lignin is uniformly added dropwise to the γ-valerolactone aqueous solution for self-assembly, thereby obtaining;

[0010] The ultrasonic power is 10-40 kHz, the ultrasonic time is 5-30 min, the volume ratio of the γ-valerolactone solution of lignin to the γ-valerolactone aqueous solution is 1:(9-15), the heating and stirring conditions are: the temperature is 40-60°C, the stirring speed is 300-800 rpm, the self-assembly time is 0.4-1h, and the uniform dripping speed is 0.5-10 mL / min.

[0011] Preferably, the lignin raw material is selected from bioethanol refining lignin, kraft lignin or deep eutectic solvent lignin.

[0012] Preferably, in the γ-valerolactone solution of lignin, the concentration of the lignin raw material in γ-valerolactone is 2-50 mg / mL.

[0013] Preferably, the volume ratio of the γ-valerolactone solution of lignin to the γ-valerolactone aqueous solution is 1:(9~14); the heating and stirring conditions are: temperature of 45~55°C, stirring speed of 400~800 rpm; the self-assembly time is 0.4~0.6h; the uniform dripping speed is 0.5~2 mL / min.

[0014] Preferably, after the self-assembly step is completed, the method further comprises dialyzing the self-assembled solution in water to obtain a lignin nanobottle water suspension.

[0015] Furthermore, the lignin nanobottle water suspension is freeze-dried to obtain lignin nanobottle powder.

[0016] Furthermore, the molecular weight of the dialysis bag used in the dialysis step is 500-3000 Da, and the dialysis time is 24-96 h.

[0017] In a second aspect, the present invention provides a high-uniformity lignin nanobottle prepared by the above preparation method.

[0018] In a third aspect, the present invention provides an application of the above-mentioned high-uniformity lignin nanobottle, wherein the application is to use the high-uniformity lignin nanobottle as a nanocarrier.

[0019] Compared with the prior art, the present invention has achieved the following beneficial effects:

[0020] (1) The self-assembly process of the lignin nanobottle of the present invention is simple. There is no need to grade the starting lignin solution, and there is no need to modify and purify the lignin. The size of the nanobottle and the size of the bottle mouth can be adjusted by adjusting the self-assembly process parameters. The size of the nanobottle is adjustable between 50 and 500 nm, and the size of the bottle mouth is adjustable between 10 and 200 nm. The size uniformity is very high, and the polydispersity index (PDI) is less than 0.1, which makes it competitive in high-end application fields such as bioengineering, drug carriers, intelligent phase change materials, and selective catalytic reactions.

[0021] (2) The preparation method of the present invention has little restriction on the source of lignin raw materials. For example, the kraft lignin produced by the current mainstream pulping method, kraft pulping, can be selected, or the lignin can be selected from bioethanol refined lignin and lignin separated from biomass components by low eutectic solvents. The preparation method of the present invention can achieve high-value utilization of existing industrial lignin and improve economic benefits.

[0022] (3) The good solvent for lignin selected in the present invention is γ-valerolactone, which, as a relatively mild solvent, retains the intramolecular stacking of lignin molecules and helps to form a spherical core as the nucleus for the uniform and stable growth of lignin nanobottles. γ-valerolactone also helps to stabilize the functionalization of lignin nanobottles because its hydrolyzate has a strong chelating ability. In addition, as a green solvent, γ-valerolactone is not only widely available, but also greatly ensures the safety of the preparation process. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] The drawings constituting part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their description are used to explain the present invention and do not constitute an improper limitation of the present invention. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative work.

[0024] Figure 1 is a scanning electron microscope image of the lignin nanobottle obtained in Example 2 of the present invention;

[0025] Figure 2 is a scanning electron microscope image of the lignin nanobottle obtained in Example 6 of the present invention;

[0026] Figure 3 This is a scanning electron microscope image of the lignin nanospheres obtained in Comparative Example 1 of the present invention;

[0027] Figure 4 is a scanning electron microscope image of lignin nanoparticles obtained in Comparative Example 2 of the present invention;

[0028] Figure 5 is a scanning electron microscope image of lignin nanoparticles obtained in Comparative Example 3 of the present invention;

[0029] Figure 6 This is a scanning electron microscope image of the lignin nanobottle obtained in Comparative Example 5 of the present invention;

[0030] Figure 7 It is a UV-visible spectrum of the lignin nanobottle water suspension in the application example of the present invention and a UV-visible spectrum of the lignin nanobottle water suspension encapsulated with lauric acid and R6G;

[0031] Figure 8 It is a comparison chart of R6G encapsulation amount of 1g of uniform-sized lignin nanobottle (LNBs-PCM-R6G) prepared in Example 2 and uniform-sized lignin nanobottle (LNBs2-PCM-R6G) prepared in Comparative Example 5 in the application example of the present invention;

[0032] Fig. 9 It is a curve diagram of the cumulative release rate of R6G released from the LNBs-PCM-R6G nanobottle at different times in the application example of the present invention. DETAILED DESCRIPTION

[0033] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0034] The present invention provides a method for preparing a high-uniformity lignin nanobottle, comprising the following steps:

[0035] Mixing γ-valerolactone and water in a volume ratio of 4:(4-10) to form a γ-valerolactone aqueous solution;

[0036] dissolving the lignin raw material in γ-valerolactone by ultrasonication, and filtering to obtain a γ-valerolactone solution of lignin;

[0037] Under heating and stirring conditions, the γ-valerolactone solution of lignin is uniformly added dropwise to the γ-valerolactone aqueous solution for self-assembly to obtain the product.

[0038] The present invention firstly ultrasonically dissolves the lignin raw material in the good solvent γ-valerolactone, and filters to obtain the γ-valerolactone solution of lignin. γ-valerolactone is a good solvent for lignin, and water is a poor solvent for lignin. Under appropriate conditions, when the γ-valerolactone solution of lignin is uniformly added dropwise to the γ-valerolactone aqueous solution, the lignin molecules will aggregate into nanobottles due to the intermolecular interaction between the good solvent and the poor solvent.

[0039] Different good solvents for lignin have different interaction forces with poor solvent water and lignin molecules, which significantly affects the morphology of the final nanoparticles. The good solvent for lignin, γ-valerolactone of the present invention, has a good solubility effect on lignin and good miscibility with water. At the same time, it retains the intramolecular stacking of lignin molecules, which helps to form a spherical core as a uniform and stable nucleus for the growth of lignin nanobottles, and finally obtains lignin nanobottles of uniform size. There are also reports in the prior art that γ-valerolactone is used as a good solvent for lignin to prepare lignin nanoparticles, but what is obtained are lignin nanospheres, so the preparation method and condition regulation are also crucial.

[0040] The amount of water added to the γ-valerolactone aqueous solution will affect the size of the formed nanobottles. Within the above volume ratio range, the more water the larger the volume, the smaller the size of the formed nanobottles. When more or less water is added, the intermolecular forces between the formed poor solvent and the good solvent will affect the formation of lignin nanobottles of uniform size or cause waste of experimental reagents.

[0041] In the present invention, the lignin raw material is selected from bioethanol refining lignin, kraft lignin or deep eutectic solvent lignin. The present invention is particularly suitable for high-value utilization of industrial lignin, with a wide source of raw materials and low cost, and no need for classification, avoiding cumbersome pretreatment steps, greatly reducing preparation costs, and high economic benefits.

[0042] In the γ-valerolactone solution of lignin of the present invention, the concentration of the lignin raw material in γ-valerolactone is 2-50 mg / mL, more preferably 10-30 mg / mL. Within the above concentration range, as the concentration of lignin increases, the size of the formed nanobottle becomes smaller.

[0043] In the present invention, the power of the ultrasound is 10-40 kHz, and the ultrasound time is 5-30 min. Ultrasound can promote the dissolution of lignin in γ-valerolactone, and those skilled in the art can appropriately adjust the ultrasound time according to the actual dissolution of the selected lignin raw material.

[0044] In the present invention, the volume ratio of the γ-valerolactone solution of lignin to the γ-valerolactone aqueous solution is 1:(9-15), and more preferably 1:(9-14).

[0045] The present invention does not impose any special restrictions on the filtering operation after ultrasonic dissolution, and the filtering operation of polymer solutions commonly used in the art can be used. The present invention preferably uses a microfiltration membrane for filtration, and the pore size of the microfiltration membrane is 0.45 μm. The filtering operation is to remove the insoluble components in the lignin raw material to avoid adverse effects on the subsequent formation of nanobottles.

[0046] The heating and stirring conditions of the present invention are: a temperature of 40-60°C, more preferably 45-55°C, and most preferably 50°C; a stirring speed of 300-800 rpm, more preferably 400-800 rpm; and suitable temperature and stirring speed are conducive to the formation of lignin nanobottles of uniform size.

[0047] In the present invention, the self-assembly time is 0.4 to 1 h, more preferably 0.4 to 0.6 h. The preparation method of the present invention can achieve rapid preparation of highly uniform lignin nanobottles.

[0048] In the present invention, the speed of the uniform dripping is 0.5 to 10 mL / min, more preferably 0.5 to 2 mL / min. The present invention does not impose any special restrictions on the specific method of uniform dripping, and the uniform dripping method commonly used in the art can be used, which can be manual uniform dripping or automatic uniform dripping. The present invention is preferably automatic uniform dripping, such as using a constant flow pump for uniform dripping.

[0049] In the present invention, after the self-assembly step is completed, the step of dialyzing the self-assembled solution in water to obtain a lignin nanobottle water suspension is also included. Further, the lignin nanobottle water suspension is freeze-dried to obtain a lignin nanobottle powder. The dialysis is to remove γ-valerolactone and finally form a nanobottle water suspension. The molecular weight of the dialysis bag used in the dialysis step of the present invention is 500~3000 Da, more preferably 1000~3000 Da; the dialysis time is 24~96 h. The water outside the dialysis bag needs to be replaced intermittently during the dialysis process.

[0050] The present invention also provides a high-uniformity lignin nanobottle prepared by the above preparation method. The size of the nanobottle prepared by the above preparation method is between 50 and 500 nm, the size of the bottle mouth is adjustable between 10 and 200 nm, and the size uniformity is very high, and the polydispersity index (PDI) is less than 0.1.

[0051] The present invention also provides an application of the high-uniformity lignin nanobottle, which is to use the high-uniformity lignin nanobottle as a nanocarrier to achieve material loading and controlled release. The loaded material can be a drug, a phase change material or a catalyst, etc., and can be used in high-end application fields such as bioengineering, drug carriers, intelligent phase change materials, and selective catalytic reactions.

[0052] At present, in the field of high-end medical drug delivery, the average particle size distribution of the carrier is directly related to effectiveness and safety. For example, large-particle carriers in injections will enter the human lungs during the injection process, causing pulmonary granulomas. Or in actual applications, larger carriers (>0.5 μm) will not only cause embolism in the lungs, but also damage the liver. Therefore, uniform size will avoid the impact of some possible large-particle carriers on human safety. Since the high-uniformity lignin nanobottles provided by the present invention have uniform size distribution, they are more effective and safer in actual processes.

[0053] Size uniformity also has a great influence on the encapsulation capacity of the nanobottle carrier. For nanobottles with poor size uniformity, smaller nanobottles have low encapsulation capacity due to their small volume, while larger nanobottles have larger mouth sizes, which will lead to more load loss, thereby reducing the encapsulation capacity and further reducing the utilization rate of the load. Therefore, the preparation of nanobottles with high size uniformity has a high practical application value.

[0054] The technical solution of the present invention is further described below in conjunction with specific embodiments. In the following embodiments, PDI represents polydispersity index, R6G represents rhodamine 6G, LNBs represents lignin nanobottle, PCM represents phase change material, and UV-Vis represents ultraviolet-visible spectrophotometer.

[0055] Example 1

[0056] This embodiment provides a method for preparing a high-uniformity lignin nanobottle.

[0057] (1) Add 5 mL of water to 4 mL of γ-valerolactone to obtain 9 mL of γ-valerolactone aqueous solution.

[0058] (2) Add kraft lignin to the good solvent γ-valerolactone to prepare a 10 mg / mL lignin γ-valerolactone solution. Ultrasonicate the lignin γ-valerolactone solution at 40 kHz for 10 min. Then filter out the insoluble components using a 0.45 μm microfiltration membrane.

[0059] (3) Take 1 mL of the γ-valerolactone solution of dissolved filtered lignin and uniformly add it to 9 mL of γ-valerolactone aqueous solution at a rate of 1 mL / min. Stir at 50 °C and 400 rpm for 0.5 h to obtain a lignin nanobottle solution.

[0060] (4) The lignin nanobottle solution was transferred to a dialysis bag (2000 Da) and dialyzed in deionized water for 48 h to displace γ-valerolactone and obtain a lignin nanobottle water suspension. The lignin nanobottle water suspension was freeze-dried to obtain lignin nanobottle powder.

[0061] Example 2

[0062] This embodiment provides a method for preparing a high-uniformity lignin nanobottle.

[0063] (1) Add 5 mL of water to 4 mL of γ-valerolactone to obtain 9 mL of γ-valerolactone aqueous solution.

[0064] (2) Add kraft lignin to the good solvent γ-valerolactone to prepare a 10 mg / mL lignin γ-valerolactone solution. Ultrasonicate the lignin γ-valerolactone solution at 40 kHz for 10 min. Then filter out the insoluble components using a 0.45 μm microfiltration membrane.

[0065] (3) Take 1 mL of the γ-valerolactone solution of dissolved filtered lignin and uniformly add it to 9 mL of γ-valerolactone aqueous solution at a rate of 1 mL / min. Stir at 50 °C and 800 rpm for 0.5 h to obtain a lignin nanobottle solution.

[0066] (4) The lignin nanobottle solution was transferred to a dialysis bag (2000 Da) and dialyzed in deionized water for 48 h to displace γ-valerolactone and obtain a lignin nanobottle water suspension. The lignin nanobottle water suspension was freeze-dried to obtain lignin nanobottle powder.

[0067] Figure 1 This is a scanning electron microscope picture of the lignin nanobottle obtained in this example. It can be seen that the prepared lignin nanobottles are uniform in size, with a particle size of 375.4 nm and a bottle mouth size of 205.2 nm.

[0068] Example 3

[0069] This embodiment provides a method for preparing a high-uniformity lignin nanobottle.

[0070] (1) Add 5 mL of water to 4 mL of γ-valerolactone to obtain 9 mL of γ-valerolactone aqueous solution.

[0071] (2) Add kraft lignin to the good solvent γ-valerolactone to prepare a 30 mg / mL lignin γ-valerolactone solution. Ultrasonicate the lignin γ-valerolactone solution at 40 kHz for 10 min. Then filter out the insoluble components using a 0.45 μm microfiltration membrane.

[0072] (3) Take 1 mL of the γ-valerolactone solution of dissolved filtered lignin and uniformly add it to 9 mL of γ-valerolactone aqueous solution at a rate of 1 mL / min. Stir at 50 °C and 800 rpm for 0.5 h to obtain a lignin nanobottle solution.

[0073] (4) The lignin nanobottle solution was transferred to a dialysis bag (2000 Da) and dialyzed in deionized water for 48 h to displace γ-valerolactone and obtain a lignin nanobottle water suspension. The lignin nanobottle water suspension was freeze-dried to obtain lignin nanobottle powder.

[0074] Example 4

[0075] This embodiment provides a method for preparing a high-uniformity lignin nanobottle.

[0076] (1) Add 7 mL of water to 4 mL of γ-valerolactone to obtain 11 mL of γ-valerolactone aqueous solution.

[0077] (2) Add kraft lignin to the good solvent γ-valerolactone to prepare a 10 mg / mL lignin γ-valerolactone solution. Ultrasonicate the lignin γ-valerolactone solution at 40 kHz for 10 min. Then filter out the insoluble components using a 0.45 μm microfiltration membrane.

[0078] (3) Take 1 mL of the γ-valerolactone solution of dissolved filtered lignin and uniformly add it to 11 mL of γ-valerolactone aqueous solution at a rate of 1 mL / min. Stir at 50 °C and 800 rpm for 0.5 h to obtain a lignin nanobottle solution.

[0079] (4) The lignin nanobottle solution was transferred to a dialysis bag (2000 Da) and dialyzed in deionized water for 48 h to displace γ-valerolactone and obtain a lignin nanobottle water suspension. The lignin nanobottle water suspension was freeze-dried to obtain lignin nanobottle powder.

[0080] Example 5

[0081] This embodiment provides a method for preparing a high-uniformity lignin nanobottle.

[0082] (1) Add 10 mL of water to 4 mL of γ-valerolactone to obtain 14 mL of γ-valerolactone aqueous solution.

[0083] (2) Add low co-solvent lignin to the good solvent γ-valerolactone to prepare a 10 mg / mL lignin γ-valerolactone solution. Ultrasonicate the lignin γ-valerolactone solution at 40 kHz for 10 min. Then filter out the insoluble components using a 0.45 μm microfiltration membrane.

[0084] (3) Take 1 mL of the filtered lignin good solvent solution and add it dropwise at a uniform rate into 14 mL of γ-valerolactone aqueous solution. The dropping speed is controlled at 1 mL / min and stirred at 50 °C and 800 rpm for 0.5 h to obtain the lignin nanobottle solution.

[0085] (4) The lignin nanobottle solution was transferred to a dialysis bag (2000 Da) and dialyzed in deionized water for 48 h to displace γ-valerolactone and obtain a lignin nanobottle water suspension. The lignin nanobottle water suspension was freeze-dried to obtain lignin nanobottle powder.

[0086] Example 6

[0087] This embodiment provides a method for preparing a high-uniformity lignin nanobottle.

[0088] (1) Add 9 mL of water to 4 mL of γ-valerolactone to obtain 13 mL of γ-valerolactone aqueous solution.

[0089] (2) Add bioethanol refined lignin to the good solvent γ-valerolactone to prepare a 10 mg / mL lignin γ-valerolactone solution. Ultrasonicate the lignin γ-valerolactone solution at 40 kHz for 10 min. Then filter out the insoluble components using a 0.45 μm microfiltration membrane.

[0090] (3) Take 1 mL of the filtered lignin good solvent solution and add it dropwise at a uniform rate into 13 mL of γ-valerolactone aqueous solution. The dropping speed is controlled at 1 mL / min and stirred at 50 °C and 800 rpm for 0.5 h to obtain the lignin nanobottle solution.

[0091] (4) The lignin nanobottle solution was transferred to a dialysis bag (2000 Da) and dialyzed in deionized water for 48 h to displace γ-valerolactone and obtain a lignin nanobottle water suspension. The lignin nanobottle water suspension was freeze-dried to obtain lignin nanobottle powder.

[0092] Figure 2 This is a scanning electron microscope picture of the lignin nanobottle obtained in this example. It can be seen that the lignin nanobottles prepared in Example 6 are uniform in size, with an average particle size of 78.5 nm and an average bottle mouth diameter of 15.2 nm.

[0093] Example 7

[0094] This embodiment provides a method for preparing a high-uniformity lignin nanobottle.

[0095] (1) Add 6 mL of water to 4 mL of γ-valerolactone to obtain 10 mL of γ-valerolactone aqueous solution.

[0096] (2) Add kraft lignin to the good solvent γ-valerolactone to prepare a 50 mg / mL lignin γ-valerolactone solution. Ultrasonicate the lignin γ-valerolactone solution at 10 kHz for 30 min. Then filter out the insoluble components using a 0.45 μm microfiltration membrane.

[0097] (3) Take 1 mL of the γ-valerolactone solution of dissolved filtered lignin and uniformly add it to 10 mL of γ-valerolactone aqueous solution at a rate of 5 mL / min. Stir at 60 °C and 800 rpm for 0.5 h to obtain a lignin nanobottle solution.

[0098] (4) The lignin nanobottle solution was transferred to a dialysis bag (1000 Da) and dialyzed in deionized water for 48 h to displace γ-valerolactone and obtain a lignin nanobottle water suspension. The lignin nanobottle water suspension was freeze-dried to obtain lignin nanobottle powder.

[0099] Comparative Example 1

[0100] Compared with Example 4, the difference is that in this comparative example, the γ-valerolactone in steps (1) to (4) is replaced by γ-butyrolactone.

[0101] Figure 3 The scanning electron microscope image of the lignin nanospheres obtained in this comparative example shows that the particle sizes of the lignin nanospheres vary greatly, and no significant lignin nanobottle structure is observed.

[0102] Comparative Example 2

[0103] Compared with Example 4, the difference is that in this comparative example, the γ-valerolactone in steps (1) to (4) is replaced by ethanol.

[0104] Figure 4 This is a scanning electron microscope image of the lignin nanobottle obtained in this comparative example. It can be seen that only lignin nanoparticles of uneven sizes were obtained, and the average particle size was 89.5 nm.

[0105] Comparative Example 3

[0106] Compared with Example 4, the difference is that in this comparative example, the γ-valerolactone in steps (1) to (4) is replaced by ethylene glycol.

[0107] Figure 5 This is a scanning electron microscope image of the lignin nanobottle obtained in this comparative example. It can be seen that only lignin nanoparticles of uneven sizes were obtained, and the average particle size was about 101 nm.

[0108] Comparative Example 4

[0109] Compared with Example 4, the difference is that in this comparative example, the 50°C in step (3) is replaced by 20°C.

[0110] Comparative Example 5

[0111] Compared with the existing lignin nanobottle preparation method.

[0112] (1) First, mix 4 mL of γ-butyrolactone with 6 mL of water to obtain a γ-butyrolactone solution.

[0113] (2) Dissolve 10 mg of alkali lignin in 1 mL of γ-butyrolactone to obtain a 10 mg / mL lignin γ-butyrolactone solution.

[0114] (3) Then, 1 mL of the lignin γ-butyrolactone solution was added to 8 mL of the γ-butyrolactone solution at a constant speed of 1 mL / min and the stirring speed was 800 r / min to obtain a lignin nanobottle solution.

[0115] (4) The lignin nanobottle solution was transferred to a dialysis bag (1000Da) and dialyzed in deionized water for 96 hours to displace γ-butyrolactone to obtain a lignin nanobottle water suspension. The lignin nanobottle water suspension was freeze-dried to obtain a lignin nanobottle powder.

[0116] Figure 6 This is a scanning electron microscope picture of the lignin nanobottle obtained in this comparative example. It can be seen that the prepared lignin nanobottles are uneven in size and have large size differences. The average particle size is 367 nm and the bottle mouth diameter is 202 nm.

[0117] Comparative Example 6

[0118] Compared with the existing lignin nanobottle preparation method.

[0119] (1) First, mix 4 mL of γ-butyrolactone with 6 mL of water to obtain a γ-butyrolactone solution.

[0120] (2) Dissolve 50 mg of alkali lignin in 1 mL of γ-butyrolactone to obtain a 50 mg / mL lignin γ-butyrolactone solution. Ultrasonicate the lignin γ-butyrolactone solution at 40 kHz for 10 min. Then filter out the insoluble components using a 0.45 μm microfiltration membrane.

[0121] (3) Then, 1 mL of the lignin γ-butyrolactone solution was added to 8 mL of the γ-butyrolactone solution at a constant speed of 1 mL / min and the stirring speed was 800 rpm to obtain a lignin nanobottle solution.

[0122] (4) The lignin nanobottle solution was transferred to a dialysis bag (1000Da) and dialyzed in deionized water for 96 h to displace γ-butyrolactone to obtain a lignin nanobottle water suspension. The lignin nanobottle water suspension was freeze-dried to obtain a lignin nanobottle powder.

[0123] The particle size of the aqueous suspensions obtained after dialysis of Examples 1 to 7 and Comparative Examples 1 to 6 was measured. The measurement results are shown in Table 1.

[0124] As can be seen from Table 1, the present invention realizes the adjustable size of lignin nanobottles under different reactions. The minimum particle size of the lignin nanobottle in the embodiment can reach 78.5nm, and the uniformity of the prepared lignin nanobottles is good, the PDI is lower than 0.1, and the lowest can be as low as 0.043. Comparative Examples 1 and 4 not only failed to successfully prepare lignin nanobottles, but also the prepared lignin nanospheres still have the problem of poor uniformity, indicating that the solvent and self-assembly temperature will affect the final nanoparticle morphology. Comparative Examples 2 and 3 not only failed to successfully prepare lignin nanobottles, but also did not even obtain spherical lignin nanomaterials, and only obtained lignin nanoparticles of irregular shape and size. Although Comparative Examples 5 and 6 successfully prepared lignin nanobottles, the prepared lignin nanobottles were uneven in size and had large size differences. From the comparison between Comparative Examples 1 and Comparative Examples 5 and 6, it can be seen that preparation conditions such as the type of poor solvent, temperature, and the volume ratio of good solvent to poor solvent will have a significant effect on the morphology of the nanobottle.

[0125] Table 1 Particle size determination of aqueous suspensions after dialysis of Examples 1 to 7 and Comparative Examples 1 to 6

[0126]

[0127] Note: “-” in the table means no or 0; polydispersity index (PDI) refers to the uniformity of particle size distribution of lignin nanobottles. The smaller the PDI, the narrower the particle size distribution and the more uniform the size distribution. Conversely, the particle size distribution is not uniform.

[0128] Application Examples

[0129] This application example is to encapsulate the phase change material lauric acid and the fluorescent dye rhodamine 6G (R6G) in the lignin nanobottle prepared in Example 2 or Comparative Example 5. R6G is a water-soluble cationic fluorescent dye, which is widely used for fluorescent labeling or quantitative analysis. The encapsulation performance of the wood nanobottle can be quantified by the unique fluorescent properties of R6G.

[0130] (1) Packaging process:

[0131] 0.5 mL of ethanol solution containing 10 mg of freeze-dried lignin nanobottle powder was dissolved in 0.5 mL of methanol solution containing 0.5 g of lauric acid and 10 mg of R6G. It was kept in a constant temperature incubator (speed 200 rpm, 44 ° C) for 2 hours to allow lauric acid and R6G molecules to diffuse into the cavity of the lignin nanobottle. Then centrifuged at 6000 rpm for 5 minutes, and the centrifuged precipitate was further washed twice with 75% (v / v) methanol aqueous solution to remove excess lauric acid and R6G. Then, 1 mL of ice water was added to the centrifuged precipitate to solidify lauric acid and retain it in the nanobottle with the dye mixture in the nanobottle. The lignin nanobottle obtained by encapsulating lauric acid and dye R6G using the lignin nanobottle obtained in Example 2 was recorded as LNBs-PCM-R6G, and the lignin nanobottle obtained by encapsulating the phase change material lauric acid and dye R6G using the lignin nanobottle obtained in Comparative Example 5 was recorded as LNBs2-PCM-R6G.

[0132] (2) Determination of load capacity:

[0133] To determine the loading capacity, lignin nanobottles (LNBs) and LNBs-PCM-R6G particles were dispersed in water, respectively, and the UV-Vis spectra of the aqueous suspensions were measured using an UV-Vis spectrophotometer (UV-Vis).

[0134] The results are as follows Figure 7 As shown in the figure, LNBs-PCM-R6G showed the characteristic peak of R6G at 530 nm, while no corresponding characteristic peak appeared in the lignin nanobottle. This strongly proves that R6G is encapsulated into the cavity of the lignin nanobottle. At the same time, it shows that the lignin nanobottle has good encapsulation ability.

[0135] In addition, the UV-visible spectra of R6G at 530 nm were used to plot a standard curve of R6G concentration. The encapsulated amount of R6G in Example 2 and Comparative Example 5 was obtained by measuring the UV-visible spectrum of the encapsulated lignin nanobottle at 530 nm and substituting it into the standard curve of R6G concentration. Figure 8 As shown, the encapsulation amount (21.01 mg / g) of Example 2 with uniform morphology is much greater than the encapsulation amount (10.08 mg / g) of the lignin nanobottle with non-uniform morphology in Comparative Example 5. This is because the large difference in particle size affects the loading capacity of the lignin nanobottle cavity. The smaller nanobottle has a low encapsulation rate due to its small volume, while the larger nanobottle has a larger bottle mouth, which will lead to more lauric acid loss. This proves that the uniform lignin nanobottle has better encapsulation performance than the non-uniform lignin nanobottle.

[0136] (3) Controlled release of LNBs-PCM-R6G:

[0137] An appropriate amount of LNBs-PCM-R6G nanobottles were dispersed in 1 mL of water and incubated at 44 °C, and the released dye (R6G was released into water and precipitated as LNBs-PCM-R6G) was collected by centrifugation (6000 rpm, 3 min) at different intervals (5, 10, 20, 40, 60, 80, 100, and 120 min), and R6G in the supernatant was quantified using an ultraviolet-visible spectrophotometer (UV-Vis).

[0138] The results are as follows Fig. 9 As shown, over time, R6G in LNBs-PCM-R6G is gradually released. The peak value of the absorption characteristic peak of R6G at 530 nm was detected by UV-visible spectrophotometer, and the release rate of R6G was quantitatively calculated. Within 120 minutes, LNBs-PCM-R6G can release 67% of R6G in the cavity. It proves that the uniformly sized lignin nanobottles obtained in Example 2 have good controllable release ability.

[0139] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a high-uniformity lignin nanobottle, characterized in that: The steps include: Mixing γ-valerolactone and water in a volume ratio of 4:(4-10) to form a γ-valerolactone aqueous solution; Dissolving the lignin raw material in γ-valerolactone by ultrasonication, and filtering to obtain a γ-valerolactone solution of lignin; in the γ-valerolactone solution of lignin, the concentration of the lignin raw material in γ-valerolactone is 2-50 mg / mL; Under heating and stirring conditions, the γ-valerolactone solution of lignin is uniformly added dropwise to the γ-valerolactone aqueous solution for self-assembly, thereby obtaining; The ultrasonic power is 10-40 kHz, the ultrasonic time is 5-30 min, the volume ratio of the γ-valerolactone solution of lignin to the γ-valerolactone aqueous solution is 1:(9-15), the heating and stirring conditions are: the temperature is 40-60°C, the stirring speed is 300-800 rpm, the self-assembly time is 0.4-1h, and the uniform dripping speed is 0.5-10 mL / min.

2. The preparation method according to claim 1, characterized in that The lignin raw material is selected from bioethanol refining lignin, kraft lignin or deep eutectic solvent lignin.

3. The preparation method according to claim 1, characterized in that: The volume ratio of the γ-valerolactone solution of lignin to the γ-valerolactone aqueous solution is 1:(9~14); the heating and stirring conditions are: the temperature is 45~55°C, the stirring speed is 400~800 rpm; the self-assembly time is 0.4~0.6h; and the uniform dripping speed is 0.5~2 mL / min.

4. The preparation method according to claim 1, characterized in that: After the self-assembly step is completed, the method further comprises the step of dialyzing the self-assembled solution in water to obtain a lignin nanobottle water suspension.

5. The preparation method according to claim 4, characterized in that: The lignin nanobottle water suspension is freeze-dried to obtain lignin nanobottle powder.

6. The preparation method according to claim 4, characterized in that: The molecular weight of the dialysis bag used in the dialysis step is 500-3000 Da.

7. The preparation method according to claim 4, characterized in that: The dialysis time is 24 to 96 hours.

8. The high-uniformity lignin nanobottle prepared by the preparation method according to any one of claims 1 to 7.

9. The use of the high uniformity lignin nanobottle as claimed in claim 8, characterized in that: The high-uniformity lignin nanobottle is used to prepare nanocarriers.