A method for preparing a low overpotential composite morphology zinc negative electrode and a zinc ion battery
By etching and discharge-charging cycle activation treatment on the surface of the zinc sheet, the (002) crystal surface and (002)/(100) coexisting crystal surface and porous fluffy microcrystal surface are formed, and the growth and over-producing zinc dendrites of zinc negative electrode are solved. The problem of high potential improves the cycle stability and overpotential reduction of zinc ion batteries, making them suitable for commercial production.
Patent Information
- Application Number
- CN202410969234.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-19
AI Technical Summary
In the aqueous zinc ion secondary battery, the zinc negative electrode has problems such as zinc dendrites growth, large electrode polarization and unsatisfactory cycle stability, which hinders its commercial development.
By performing acid etching and discharge-charge cycle activation treatment on the surface of the zinc sheet, the zinc sheet is promoted to form (002) crystal plane and (002)/(100) coexisting crystal plane and porous fluffy microcrystal surface to inhibit the growth of zinc dendrites and Reduce the overpotential.
It significantly enhances the performance stability of the zinc negative electrode during repeated charge and discharge cycles, and reduces the overpotential of the zinc negative electrode. It has a simple process and low cost, which is suitable for large-scale production.
Smart Images

Figure CN118538858B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of batteries, and in particular to a method for preparing a low overpotential composite morphology zinc negative electrode and a zinc ion battery. Background Art
[0002] Aqueous zinc-ion secondary batteries have attracted increasing attention due to their inherent safety, low cost, and high reliability. Although zinc metal has a high theoretical capacity (820Ah Kg -1 ,5854Ah L -1 ), low cost, etc., but it still has defects such as zinc dendrite growth, large electrode polarization and poor long-term cycle stability. These defects that have long plagued the performance of zinc electrodes have hindered the commercial development of aqueous zinc ion secondary batteries. Studies have shown that in Zn 2+ During the repeated stripping / deposition of Zn / Zn, preventing the dendrite growth of the Zn negative electrode has a lot to do with the atomic structure of the electrode surface and the orientation of the crystal plane. The (100) crystal plane has an uneven distribution of interfacial charge density and is most likely to form dendrite growth; while the (002) crystal plane is conducive to Zn / Zn 2+ The surface of the electrode is uniformly precipitated parallel to the electrode, the surface is relatively smooth, and dendrites are not easily formed. Therefore, adjusting and constructing the surface microstructure and crystal orientation of the zinc negative electrode will help inhibit the growth of zinc dendrites, prolong the cycle stability and reduce the polarization of the electrode.
[0003] At present, the most common method for constructing the zinc (002) crystal plane is to use heat treatment and rolling process. For example, in the Chinese invention patent CN116565111A, the zinc sheet is placed in a high-temperature furnace and annealed under the protection of an inert atmosphere; the annealed zinc sheet is placed between two rollers of a roller press for rolling; during the rolling process, the working distance between the two rollers is gradually reduced until the deformation rate of the zinc sheet reaches 300%, and the final zinc sheet (002) crystal plane texture strength is high. However, the disadvantage of this solution is that it requires heating equipment, has high cost and energy consumption, and the zinc sheet rolled by rolling is thin and has the risk of tearing.
[0004] In addition to the above schemes, other methods for inducing the preferential growth of the (002) crystal plane of the zinc negative electrode include: 1) adding sodium gluconate additives or cationic additives such as 1-butyl-3-methylimidazolium cations to the electrolyte; 2) constructing nitrogen-doped graphene films on the surface of the zinc negative electrode to induce zinc ions to grow on the electrode surface according to the (002) plane. However, the overpotential of the zinc negative electrode obtained by the above two methods is relatively high, and there is still room for improvement (reduction), and the chemical reagents / additives used or the auxiliary materials used to construct the interface on the zinc surface are very expensive, and the cost is too high, which is not conducive to the commercialization of aqueous zinc ion secondary batteries. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a method for preparing a low overpotential composite morphology zinc negative electrode and a zinc ion battery. The present invention sequentially performs acid etching and discharge-charge cycle activation treatment on the surface of the zinc sheet, which can promote the zinc sheet surface to preferentially form a (002) crystal plane and simultaneously construct a (002) / (100) coexisting crystal plane and a porous fluffy microcrystalline surface, which can not only effectively inhibit the growth of zinc dendrites, but also greatly reduce the overpotential of the zinc negative electrode; and when assembled into a zinc ion battery, the performance stability of the zinc negative electrode during repeated charge and discharge cycles can be significantly enhanced. In addition, the method of the present invention is simple in process, low in cost, and suitable for large-scale production.
[0006] The specific technical scheme of the present invention is:
[0007] In a first aspect, the present invention provides a method for preparing a low overpotential composite morphology zinc negative electrode, comprising the following steps:
[0008] 1) Remove the oxide on the surface of the zinc sheet, wash it, dry it, and immerse the zinc sheet in a phosphoric acid aqueous solution for pretreatment.
[0009] 2) The zinc sheet obtained in step 1) is washed and dried, and then immersed in a mixed aqueous solution containing halogen anions and acetic acid for discharge-charge cycle activation.
[0010] 3) The zinc sheet obtained in step 2) is washed and dried to obtain a low overpotential composite zinc negative electrode having a (002) crystal plane, a (002) / (100) coexisting crystal plane and a porous fluffy microcrystalline surface.
[0011] In step 1), after removing the oxide on the chip surface, the surface of the zinc sheet is acid-etched with a phosphoric acid aqueous solution, which can make the surface of the zinc sheet rougher, which is conducive to regulating the surface morphology of the zinc sheet in the subsequent electrochemical activation process. In step 2), the zinc sheet is immersed in a mixed aqueous solution containing halogen anions and acetic acid for discharge-charge cycle activation treatment (in this process, the zinc on the surface of the zinc sheet is used as a zinc source, and it is repeatedly converted between the two states of zinc ions and zinc, and finally zinc is deposited on the surface of the zinc sheet in the form of different crystal planes); by controlling the concentration of halogen anions / acetic acid and electrochemical process parameters, a special target morphology can be constructed on the surface of the zinc sheet - having a (002) crystal plane, a (002) / (100) coexisting crystal plane (the (100) crystal plane coexists at the grain boundary of the (002) crystal plane) and a porous fluffy microcrystalline surface. The above three surface morphologies are intermixed, among which the (002) crystal plane occupies the main area.
[0012] In the present invention, zinc flakes are used as substrates to provide zinc ions in the discharge-charge cycle activation. The role of halogen anions and acetic acid is: zinc ions in aqueous solution usually contain six water molecules, and the carboxyl group and halogen anions (taking chloride ions as an example) in acetic acid not only have a strong coordination effect on zinc ions (4Cl- + Zn(H2O)6 2+ = Zn(Cl - )4(H2O)2 2- +4H2O), and has a strong affinity for hydrogen in water molecules, and forms hydrogen bonds, which enables zinc ions to achieve partial dehydration solvation and exclude some water molecules. The addition of chloride anions can reduce the internal Helmholtz plane potential of the electrode solid-liquid interface, reduce polarization, promote the effective deposition of zinc, inhibit the side reaction of water and improve the negative electrode Coulomb efficiency.
[0013] The present invention finds that, compared with the pure (002) crystal plane, the negative electrode with the above-mentioned special composite morphology can not only effectively inhibit the growth of zinc dendrites, but also significantly reduce the overpotential of the zinc negative electrode, and when assembled into a zinc ion battery, it can significantly enhance the stability of the performance of the zinc negative electrode during repeated charge and discharge cycles.
[0014] The electrochemical process parameters have a significant impact on the morphology construction, the zinc negative electrode overpotential, and the effect of inhibiting zinc dendrite growth. Finally, the present invention found that at a current density of 0.6-3 mA / cm 2 (More preferably 0.6-1.5 mA / cm 2 ), a single discharge or charge time of 3-20h (more preferably 4-10h), and a cycle number of 1-10 cycles (more preferably 2-4 cycles), a zinc negative electrode with a target morphology can be successfully constructed, and the obtained zinc negative electrode has a good effect of inhibiting zinc dendrite growth and a low overpotential. Among the above electrochemical process parameters, the current density has the greatest impact: at high current density (≥3mA / cm 2 ), due to the rapid deposition or stripping speed of zinc ions on the surface of the zinc sheet, the zinc crystal planes observed on the surface of the zinc sheet contain a large number of (101) and (100) crystal planes in addition to the (002) orientation. The deposition orientation of zinc is not mainly based on the (002) crystal plane. In addition, under high current density, it is easy to cause uneven distribution of convex surfaces formed during deposition or concave surfaces formed during stripping. The convex surfaces formed are prone to "tip effect", which leads to the growth of dendrites during repeated discharge-charge cycles; the formation of uneven concave surfaces can easily lead to local thinning of the zinc sheet after repeated cycles, and even fractures and gaps, which seriously affect the electrode performance. On the contrary, at low current density (≤0.5mA / cm 2 ), although the overpotential of the obtained negative electrode is low, due to the slow zinc nucleation rate, a porous morphology similar to strip-like bending is observed on the surface of the zinc sheet, and no obvious (002) crystal plane is formed, so the growth of zinc dendrites cannot be effectively inhibited.
[0015] Similarly, the concentrations of halogen anions and acetic acid also have a significant effect on morphology construction, zinc negative electrode overpotential, and the effect of inhibiting zinc dendrite growth. Finally, the present invention found that the effect is better when the concentration of halogen anions is 0.2-6 mol / L (preferably 2-4 mol / L) and the concentration of acetic acid is 0.2-1.9 mol / / L (preferably 0.6-1.5 mol / L).
[0016] Preferably, in step 2), a multi-stage differentiated discharge-charge cycle process is adopted: the first stage: the current density is 0.6-0.8 mA / cm 2 , single discharge or charge time is 5-10h, cycle number is 1 circle; second stage: current density is 1.3-1.7mA / cm 2 , single discharge or charge time is 3-5h, cycle number is 1-2 circles; third stage: current density is 0.8-1.2mA / cm 2 , the single discharge or charge time is 4-5h, and the number of cycles is 1-2 circles.
[0017] The present invention finds that the surface morphology of the zinc sheet can be controlled by using the above-mentioned multi-stage differentiated electroactivation process, which can further reduce the overpotential of the zinc negative electrode and inhibit the growth of zinc dendrites.
[0018] Preferably, in step 2), the halogen anion is a chloride anion or a bromide anion.
[0019] Due to the special adsorption of chloride anions or bromide anions, their addition can reduce the internal Helmholtz plane potential of the electrode solid-liquid interface, and chloride anions also participate in the weak complexation reaction of Zn ions to form more Zn-Cl or Zn-Br superhalides. The presence of Cl anions or bromide anions reduces polarization and increases ion migration. Improving the negative electrode Coulomb efficiency and reducing polarization promotes the deposition of zinc.
[0020] Preferably, in step 2), the pH of the mixed aqueous solution is 4.8-5.2.
[0021] Preferably, in step 1), sandpaper is used to remove oxides on the surface of the zinc sheet.
[0022] Preferably, in step 1), the concentration of the phosphoric acid aqueous solution is ≥ 85 wt %.
[0023] Preferably, in step 1), the pretreatment time is 2-30 min (more preferably 5-15 min) and the temperature is room temperature.
[0024] In a second aspect, the present invention provides a zinc ion battery comprising the above-mentioned low overpotential composite morphology zinc negative electrode, positive electrode, separator and electrolyte.
[0025] Compared with the prior art, the beneficial effects of the present invention are:
[0026] (1) The present invention sequentially performs acid etching and discharge-charge cycle activation treatment on the surface of the zinc sheet, which can promote the zinc sheet surface to preferentially form a (002) crystal plane and simultaneously construct a (002) / (100) coexisting crystal plane and a porous fluffy microcrystalline surface, which can not only effectively inhibit the growth of zinc dendrites, but also greatly reduce the overpotential of the zinc negative electrode. Moreover, when assembled into a zinc ion battery, the performance stability of the zinc negative electrode during repeated charge and discharge cycles can be significantly enhanced.
[0027] (2) The method of the present invention has simple process, low cost (the price of acetic acid / potassium acetate is extremely low), and is suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 : This is the XRD diagram of the zinc sheet before and after being treated by Example 7 of the present invention.
[0029] Figure 2 and Figure 3 This is a SEM image of the zinc sheet before treatment in Example 7 of the present invention.
[0030] Figure 4 and Figure 5 This is a SEM image of the zinc sheet after being treated with phosphoric acid aqueous solution in step (1) of Example 7 of the present invention.
[0031] Figure 6 and Figure 7 This is a SEM image of the zinc sheet after treatment in Example 7 of the present invention.
[0032] Figure 8 and Fig. 9 This is a SEM image of the zinc sheet surface with the (002) crystal plane as the main area after being treated in Example 7 of the present invention.
[0033] Fig.10 and Fig.11 This is a SEM image of the (002) / (100) coexisting crystal plane region on the surface of the zinc sheet after treatment in Example 7 of the present invention.
[0034] Fig.12 and Fig.13 This is a SEM image of the porous, fluffy, microcrystalline area on the surface of the zinc sheet after being treated in Example 7 of the present invention.
[0035] Fig.14 This is the XRD diagram of the zinc sheet after being treated in Comparative Example 7 of the present invention. DETAILED DESCRIPTION
[0036] The present invention will be further described below in conjunction with the embodiments.
[0037] First, the present invention provides a method for preparing a low overpotential composite morphology zinc negative electrode, which specifically comprises the following steps:
[0038] 1) Remove the surface oxide of the zinc sheet, then wash it, dry it, and immerse the zinc sheet in a phosphoric acid aqueous solution for pretreatment.
[0039] In some specific implementation cases, the surface oxide of the zinc sheet is removed with No. 2000 metallographic sandpaper. In some specific implementation cases, the concentration of the phosphoric acid aqueous solution is ≥ 85wt%. In some specific implementation cases, the pretreatment time is 2-30min (in some more preferred implementation cases, further preferably 5-15min), and the temperature is room temperature.
[0040] 2) The zinc sheet obtained in step 1) is washed and dried, and then immersed in a mixed aqueous solution containing halogen anions and acetic acid for discharge-charge cycle activation; the concentration of the halogen anions is 0.2-6 mol / L, the concentration of the acetic acid is 0.2-1.9 mol / / L; the current density is 0.6-3 mA / cm 2 The working time of a single discharge or charge is 3-20h, and the number of cycles is 1-10.
[0041] In some more preferred embodiments, the current density is 0.6-1.5 mA / cm 2 The single charge or discharge time is 4-10h, and the number of cycles is 2-4.
[0042] In some specific implementation cases, the halogen anion is a chloride anion or a bromide anion. In some specific implementation cases, the concentration of the halogen anion is 2-4 mol / L; the concentration of the acetic acid is 0.6-1.5 mol / L. In some specific implementation cases, the pH of the mixed aqueous solution is 4.8-5.2 (adjusted by adding potassium acetate).
[0043] In some specific implementation cases, in step 2), a multi-stage differentiated discharge-charge cycle process is adopted: the first stage: the current density is 0.6-0.8 mA / cm 2 , single discharge or charge time is 5-10h, cycle number is 1 circle; second stage: current density is 1.3-1.7mA / cm 2 , single discharge or charge time is 3-5h, cycle number is 1-2 circles; third stage: current density is 0.8-1.2mA / cm 2 , the single discharge or charge time is 4-5h, and the number of cycles is 1-2 circles.
[0044] 3) The zinc sheet obtained in step 2) is washed and dried to obtain a low overpotential composite zinc negative electrode having a (002) crystal plane, a (002) / (100) coexisting crystal plane ((100) coexists at the grain boundary of (002)) and a porous fluffy microcrystalline surface.
[0045] Secondly, the present invention provides a zinc ion battery, which comprises a negative electrode, a positive electrode, a separator and an electrolyte, wherein the negative electrode is the above-mentioned low overpotential composite morphology zinc negative electrode.
[0046] Specific Examples and Comparative Examples
[0047] 1. Effect of different electrochemical processes on the performance of zinc anode
[0048] (a) Effect of different acetic acid concentrations on zinc negative electrode performance (Comparative Example 1, Example 1, Example 2 and Comparative Example 2):
[0049] (1) Use No. 2000 metallographic sandpaper to wipe off the surface oxide of the zinc sheet. After rinsing with water, cleaning and drying, place the zinc sheet in an 85wt% phosphoric acid aqueous solution for surface chemical treatment and soak it at room temperature for 10 minutes.
[0050] (2) The zinc sheet after chemical treatment in step (1) is rinsed with water and blown dry with cold air, and the zinc sheet is placed in a mixed aqueous solution containing potassium chloride (concentration of 1 mol / L) and acetic acid (concentration of 0.1-2 mol / L, see Table 1 for details) (the pH of the mixed aqueous solution is adjusted to 5 by adding an appropriate amount of potassium acetate).
[0051] (3) The zinc sheet from step (2) was subjected to electrochemical discharge-charge cycle activation treatment. The zinc sheet to be surface structure optimized was placed in the center as the research electrode, and zinc sheets of the same size were placed on both sides as the counter electrode. The current density was 1 mA / cm 2 (Relative research zinc electrode), the cycle number is 3, the first 2 single discharge and charge working time is 10 hours, the third single discharge and charge working time is 4 hours and 40 minutes.
[0052] (4) The zinc sheet after the electrochemical discharge-charge cycle activation treatment in step (3) is rinsed with water, blown dry with cold air and set aside to obtain a zinc negative electrode.
[0053] (b) Effect of different chloride ion concentrations on zinc negative electrode performance (Comparative Example 3, Example 3, Example 4, Example 5 and Comparative Example 4):
[0054] (1) Use No. 2000 metallographic sandpaper to wipe off the oxide on the surface of the zinc sheet. After rinsing with water, cleaning and drying, place the zinc sheet in an 85wt% phosphoric acid aqueous solution for surface chemical treatment and soak it at room temperature for 10 minutes.
[0055] (2) The zinc sheet after chemical treatment in step (1) is rinsed with water and blown dry with cold air, and the zinc sheet is placed in a mixed aqueous solution containing potassium chloride (concentration of 0.1-7 mol / L, see Table 1 for details) and acetic acid (concentration of 1 mol / L) (the pH of the mixed aqueous solution is adjusted to 5 by adding an appropriate amount of potassium acetate).
[0056] (3) The zinc sheet from step (2) was subjected to electrochemical discharge-charge cycle activation treatment. The zinc sheet to be surface structure optimized was placed in the center as the research electrode, and zinc sheets of the same size were placed on both sides as the counter electrode. The current density was 1.5 mA / cm 2 (Relative research zinc electrode), the cycle number is 3, the first 2 single discharge and charge working time is 10 hours, the third single discharge and charge working time is 4 hours and 40 minutes.
[0057] (4) The zinc sheet after the electrochemical discharge-charge cycle activation treatment in step (3) is rinsed with water, blown dry with cold air and set aside to obtain a zinc negative electrode.
[0058] (c) Effect of different current densities on zinc negative electrode performance (Comparative Example 5, Example 6, Example 7, Example 8 and Comparative Example 6):
[0059] (1) Use No. 2000 metallographic sandpaper to wipe off the oxide on the surface of the zinc sheet. After rinsing with water, cleaning and drying, place the zinc sheet in an 85wt% phosphoric acid aqueous solution for surface chemical treatment and soak it at room temperature for 10 minutes.
[0060] (2) Rinse the zinc sheet after chemical treatment in step (1) with water and blow dry with cold air, and place the zinc sheet in a mixed aqueous solution containing potassium chloride (concentration of 3 mol / L) and acetic acid (concentration of 1 mol / L) (the pH of the mixed aqueous solution is adjusted to 5 by adding an appropriate amount of potassium acetate).
[0061] (3) The zinc sheet of step (2) is subjected to electrochemical discharge-charge cycle activation treatment. The zinc sheet to be surface structure optimized is placed in the center as the research electrode, and zinc sheets of the same size are placed on both sides as the counter electrode. The current density is 0.1-4 mA / cm 2 (Relative to the zinc electrode studied, see Table 1 for details), the number of cycles is 3, the first 2 single discharge and charge working times are 10 hours, and the third single discharge and charge working time is 4 hours and 40 minutes.
[0062] (4) The zinc sheet after the electrochemical discharge-charge cycle activation treatment in step (3) is rinsed with water, blown dry with cold air and set aside to obtain a zinc negative electrode.
[0063] Performance Testing
[0064] (1) The electrochemical performance of the zinc negative electrodes obtained in Comparative Examples 1-6 and Examples 1-8 was tested. The results are shown in Table 1.
[0065] Table 1: Effects of different acetic acid concentrations, different chloride ion concentrations and different current densities on the overpotential of the zinc negative electrode
[0066]
[0067] From the data comparison in Table 1, we can see that:
[0068] (a) The difference between Comparative Example 1, Example 1, Example 2 and Comparative Example 2 is that the acetic acid concentration gradually increases (Comparative Example 1 = 0.1 mol / L, Example 1 = 0.6 mol / L, Example 2 = 1.5 mol / L, Comparative Example 2 = 2 mol / L). Data comparison shows that within the above-mentioned specific acetic acid concentration range, the overpotential (absolute value) of the zinc negative electrode obtained in Example 1 and Example 2 is lower. Therefore, it is better to control the acetic acid concentration within 0.2-1.5 ml / L, and more preferably 0.6-1.5 ml / L.
[0069] (b) The difference between Comparative Example 3, Example 3, Example 4, Example 5 and Comparative Example 4 is that the chloride ion concentration gradually increases (Comparative Example 3 = 0.1 mol / L, Example 3 = 0.2 mol / L, Example 4 = 2 mol / L, Example 5 = 4 mol / L, Comparative Example 4 = 7 mol / L). Data comparison shows that within the chloride ion concentration range of 0.2-7 mol / L, the overpotential of the obtained zinc negative electrode is low, but when the chloride ion concentration is too high (Comparative Example 4 = 7 mol / L), it is easy to cause more serious corrosion to the zinc negative electrode during repeated electrochemical discharge-charge cycle activation. Therefore, the preferred chloride ion concentration is 0.2-4 mol / L, and more preferably 2-4 mol / L.
[0070] (c) The difference between Comparative Example 5, Example 6, Example 7, Example 8 and Comparative Example 6 is that the current density gradually increases during the discharge-charge cycle activation treatment (Comparative Example 5 = 0.1 mA / cm 2 , Example 6 =0.6mA / cm 2 , Example 7 = 1.2 mA / cm 2 , Example 8 = 3 mA / cm 2 , Comparative Example 6 = 4 mA / cm 2 ), data comparison shows that in the range of 0.1-3mA / cm 2 In the current density range, the overpotential of the obtained zinc negative electrode is low, but the present invention finds through detection that at too low current density (Comparative Example 5 = 0.1 mA / cm 2) treatment, the zinc nucleation rate is slow, and a porous sparse morphology similar to strip bending is observed on the surface of the zinc negative electrode, and no obvious (002) crystal plane is formed. Therefore, although the zinc sheet of comparative example 5 has a lower overpotential, the effect of inhibiting the formation of zinc dendrites is poor because the (002) crystal plane is not obviously formed. On the contrary, the present invention finds that at high current density (comparative example 6 = 4mA / cm 2 ), not only the overpotential of the obtained zinc negative electrode is high, but also the convex surface formed during deposition or the concave surface formed during stripping is easily unevenly distributed. The convex surface formed is prone to "tip effect", which leads to the growth of dendrites during repeated discharge-charge cycles; the formation of uneven concave surface is easy to cause local thinning of the zinc sheet after repeated cycles, and even fracture and gap phenomenon, which seriously affects the electrode performance. Therefore, the current density is preferably 0.6-3mA / cm 2 , further preferably 0.6-1.5 mA / cm 2
[0071] (2) Analysis of zinc negative electrode surface morphology
[0072] In Example 7, the surface structures of the zinc sheets before and after treatment were analyzed by XRD and SEM, respectively.
[0073] (2.1) XRD analysis: Figure 1 is the XRD diagram of the zinc sheet before and after being treated by Example 7 of the present invention, Figure 1 The information shows that compared with the original phase structure of the zinc sheet (the curve at the bottom), in the phase structure of the zinc negative electrode after treatment in Example 7 (the curve at the top), the intensity of the (002) diffraction peak increases significantly, and there is a weaker and wider diffraction peak pattern at the bottom of the (002) and (101) peaks (the part indicated by the arrow), indicating that in addition to the formation of abundant (002) crystal planes, there is also a porous and fluffy microcrystalline structure on the surface of the zinc negative electrode. It should be emphasized that although the (100) diffraction peak and (101) diffraction peak also appear in the XRD curve of the zinc sheet after treatment in Example 7, combined with the subsequent SEM photos ( Figure 2 and Figure 3 ), no large number of (100) and (101) crystal planes were found on the surface of the zinc sheet, indicating that (100) and (101) mainly exist in the bottom layer of the zinc negative electrode rather than on the surface. For a more detailed microscopic morphology analysis, see the SEM observation results.
[0074] (2.2) Scanning electron microscope (SEM) observation: Figure 2 and Figure 3 All of them are SEM pictures of the zinc sheet before treatment in Example 7 of the present invention. Figure 4 and Figure 5 All are SEM images of the zinc negative electrode after being treated with phosphoric acid aqueous solution in step (1) of Example 7 of the present invention. Figure 6-Figure 13This is a SEM image of the zinc negative electrode after final treatment in Example 7 of the present invention.
[0075] Among them, Figure 2 and Figure 3 Observation shows that the surface of the untreated zinc sheet is relatively smooth and has a lower surface roughness.
[0076] By observation Figure 4 and Figure 5 It can be seen that after being treated with phosphoric acid aqueous solution, a large number of particles are formed on the surface of the zinc sheet, and the surface becomes obviously uneven and rougher.
[0077] Depend on Figure 6 and Figure 7 It can be seen from the observation that the zinc sheet treated by Example 7 of the present invention has a variety of different microscopic morphologies on its surface, among which the (002) crystal plane occupies the main area, and there are also (002) / (100) coexisting crystal planes and porous fluffy microcrystalline surfaces.
[0078] Figure 8 and Fig. 9 This is the SEM image of the area dominated by the (002) crystal plane; Fig.10 and Fig.11 The SEM image of the (002) / (100) coexisting crystal plane area shows that (100) coexists at the grain boundary of (002) in the (002) / (100) coexisting crystal plane. Fig.12 and Fig.13 This is the SEM image of the porous fluffy microcrystalline area.
[0079] 2. Effect of surface treatment with phosphoric acid aqueous solution on the performance of zinc negative electrode
[0080] Comparative Example 7
[0081] (1) Use 2000 metallographic sandpaper to wipe off the oxide on the surface of the zinc sheet, rinse with water, clean and blow dry.
[0082] (2) The zinc sheet treated in step (1) is placed in a mixed aqueous solution containing potassium chloride (concentration of 3 mol / L) and acetic acid (concentration of 1 mol / L) (the pH of the mixed aqueous solution is adjusted to 5 by adding an appropriate amount of potassium acetate).
[0083] (3) The zinc sheet from step (2) was subjected to electrochemical discharge-charge cycle activation treatment. The zinc sheet to be surface structure optimized was placed in the center as the research electrode, and zinc sheets of the same size were placed on both sides as the counter electrode. The current density was 1.2 mA / cm 2 (Relative research zinc electrode), the working time of a single discharge or charge is 10 hours, the number of cycles is 3, the working time of the first 2 single discharge and charge is 10 hours, and the working time of the third single discharge and charge is 4 hours and 40 minutes.
[0084] (4) The zinc sheet after the electrochemical discharge-charge cycle activation treatment in step (3) is rinsed with water, blown dry with cold air and set aside to obtain a zinc negative electrode.
[0085] Performance Testing
[0086] (1) The electrochemical performance of the zinc negative electrodes obtained in Comparative Example 7 and Example 7 was tested. The results are shown in Table 2.
[0087] Table 2: Effect of phosphoric acid aqueous solution surface treatment on the overpotential of zinc negative electrode
[0088]
[0089] From the comparison of the results in Table 2, it can be seen that the only difference between Comparative Example 7 and Example 7 is that the zinc sheet in Comparative Example 7 is not pretreated with the phosphoric acid aqueous solution. The results show that the overpotential of the zinc negative electrode finally obtained in Comparative Example 7 is approximately between +58mV and -69mV, which is significantly higher than that in Example 7. Therefore, it is proved that pretreatment of the zinc sheet with phosphoric acid aqueous solution plays an important role in reducing the overpotential of the zinc negative electrode.
[0090] (2) XRD analysis: Fig.14 The XRD diagram of the zinc sheet after treatment in Comparative Example 7 is shown in FIG. Fig.14 From the information, it can be seen that although the diffraction peak of (002) can be found on the surface of the zinc sheet, the diffraction peak of the porous fluffy microcrystals is not found, so the zinc negative electrode with the special composite morphology of the present invention cannot be obtained.
[0091] 3. Impact of multi-stage differentiated discharge-charge cycle electrochemical process
[0092] Example 9
[0093] (1) Use No. 2000 metallographic sandpaper to wipe off the oxide on the surface of the zinc sheet. After rinsing with water, cleaning and drying, place the zinc sheet in an 85wt% phosphoric acid aqueous solution for surface chemical treatment and soak it at room temperature for 10 minutes.
[0094] (2) Rinse the zinc sheet after chemical treatment in step (1) with water and blow dry with cold air, and place the zinc sheet in a mixed aqueous solution containing potassium chloride (concentration of 3 mol / L) and acetic acid (concentration of 1 mol / L) (the pH of the mixed aqueous solution is adjusted to 5 by adding an appropriate amount of potassium acetate).
[0095] (3) The zinc sheet in step (2) is subjected to a multi-stage differentiated electrochemical discharge-charge cycle activation treatment. The zinc sheet to be surface structure optimized is placed in the center as the research electrode, and zinc sheets of the same size are placed on both sides as the counter electrode. The multi-stage differentiated discharge-charge cycle process is as follows: Stage 1: Current density is 0.7 mA / cm2 , single discharge or charge time is 6h, cycle number is 1 circle; second stage: current density is 1.5mA / cm 2 , single discharge or charge time is 4h, cycle number is 2 circles; third stage: current density is 1.0mA / cm 2 , the single discharge or charge time is 5h, and the number of cycles is 2 circles.
[0096] (4) The zinc sheet after the multi-stage differentiated electrochemical discharge-charge cycle activation treatment in step (3) is rinsed with water, blown dry with cold air and set aside to obtain a zinc negative electrode.
[0097] Performance Testing
[0098] (1) The electrochemical performance of the zinc negative electrodes obtained in Example 7 and Example 9 was tested. The results are shown in Table 3.
[0099] Table 3: Effect of different discharge-charge cycle electrochemical processes on the overpotential of zinc anode
[0100]
[0101] From the comparison of the results in Table 3, it can be seen that the only difference between Example 9 and Example 7 is that Example 9 adopts a multi-stage differentiated discharge-charge cycle electrochemical treatment process. It is found that the overpotential of the zinc negative electrode after the treatment in Example 9 is about +12mV to -15mV, which is further improved on the basis of Example 7. The above overpotential data comparison shows that the use of a multi-stage differentiated discharge-charge cycle electrochemical treatment process (Example 9) can further reduce the overpotential of the zinc negative electrode.
[0102] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.
[0103] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing a low overpotential composite morphology zinc negative electrode, characterized in that: The following steps are involved: 1) Remove the oxide on the surface of the zinc sheet and immerse it in a phosphoric acid aqueous solution for pretreatment; 2) Immersing the obtained zinc sheet in a mixed aqueous solution containing halogen anions and acetic acid for discharge-charge cycle activation; wherein 1) the obtained zinc sheet is used as a research electrode, and zinc sheets are placed on both sides of the zinc sheet as counter electrodes; the concentration of halogen anions is 0.2-6 mol / L, the concentration of acetic acid is 0.2-1.9 mol / L; the current density is 0.6-3 mA / cm 2 , a single discharge or charge time is 3-20h, and the number of cycles is 1-10; the halogen anion is a chloride anion or a bromide anion; 3) The obtained zinc sheet is washed and dried to obtain a low overpotential composite zinc negative electrode having a (002) crystal plane, a (002) / (100) coexisting crystal plane and a porous fluffy microcrystalline surface, wherein (100) in the (002) / (100) coexisting crystal plane coexists at the grain boundary of (002).
2. The preparation method according to claim 1, characterized in that: In step 2), the current density is 0.6-1.5 mA / cm 2 , single discharge or charge time is 4-10h, and the number of cycles is 2-4 circles.
3. The preparation method according to claim 1, characterized in that: In step 2), a multi-stage differentiated discharge-charge cycle process is adopted: The first stage: the current density is 0.6-0.8mA / cm 2 , single discharge or charge time is 5-10h, and the number of cycles is 1 circle; The second stage: the current density is 1.3-1.7 mA / cm 2 , single discharge or charge time is 3-5h, and the number of cycles is 1-2 circles; The third stage: the current density is 0.8-1.2mA / cm 2 , the single discharge or charge time is 4-5h, and the number of cycles is 1-2 circles.
4. The preparation method according to claim 1, characterized in that: In step 2), the concentration of the halogen anion is 2-4 mol / L; the concentration of the acetic acid is 0.6-1.5 mol / L.
5. The preparation method according to claim 1, characterized in that: In step 2), the pH of the mixed aqueous solution is 4.8-5.
2.
6. The preparation method according to claim 1, characterized in that: In step 1), use sandpaper to remove the oxide on the surface of the zinc sheet.
7. The preparation method according to claim 1, characterized in that: In step 1), the concentration of the phosphoric acid aqueous solution is ≥85wt%.
8. The preparation method according to claim 1 or 7, characterized in that: In step 1), the pretreatment time is 2-30 minutes and the temperature is room temperature.
9. A zinc ion battery comprising a zinc negative electrode, a positive electrode, a separator and an electrolyte, characterized in that: The zinc negative electrode is a low overpotential composite morphology zinc negative electrode obtained by the preparation method according to any one of claims 1 to 8.