Method for modifying diaphragm of lithium-sulfur battery modified by ionic covalent organic framework, modified diaphragm and battery containing the modified diaphragm

By using the ionic covalent organic framework material TB-COF to encapsulate HSO3-ions in lithium sulfur batteries, the HSO3-@TB-COF modified separator is prepared, which solves the problems of poor conductivity and shuttle effect of lithium sulfur batteries, and improves the battery's Electrochemical performance and stability achieve efficient battery performance improvement.

CN118539085BInactive Publication Date: 2024-11-22JILIN NORMAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410634350.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-22
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Lithium sulfur batteries have poor electrochemical performance due to poor conductivity, polysulfide shuttle effect and lithium dendrites, and the existing diaphragm modification technology has problems such as increased cost, ion transmission resistance and safety.

Method used

The ionic covalent organic framework material TB-COF is used to encapsulate HSO3-ions through ion exchange process, and HSO3-@TB-COF is prepared as a modified separator. The shuttle effect of polysulfides is suppressed through electrostatic repulsion, and the mobility of lithium ions is improved. and battery stability.

Benefits of technology

It significantly improves the rate performance and cycle stability of lithium-sulfur batteries, enhances the charge and discharge efficiency and stability of the battery, reduces the capacity attenuation rate, and provides high specific surface area and good structural stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118539085B_ABST
    Figure CN118539085B_ABST
Patent Text Reader

Abstract

The invention discloses a method for modifying a lithium-sulfur battery diaphragm modified by an ionic covalent organic framework, a modified diaphragm and a battery containing the modified diaphragm, belonging to the technical field of batteries. The invention uses an ionic COF covalent organic framework material as a modified material for a multifunctional diaphragm of a lithium-sulfur battery, uses a prepared two-dimensional cationic TB-COF as a main material for modifying a lithium-sulfur battery diaphragm, and then uses an ion exchange process to convert HSO 3 ‑encapsulated into the cationic framework to obtain HSO 3 TB-COF, prepared by using 2,4,6-tris(4-formylphenyl)-1,3,5-triazine and ethidium bromide (EB) as monomers to prepare cationic TB-COF, and using HSO 3 ion to replace Br to prepare HSO 3 ‑@TB‑COF, the obtained material was coated on PP film to obtain HSO 3 ‑@TB‑COF modified diaphragm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of batteries, and in particular relates to a method for modifying a lithium-sulfur battery diaphragm modified by an ionic covalent organic skeleton, the modified diaphragm and a battery containing the modified diaphragm. Background Art

[0002] With the growing demand for high energy density and long life batteries, the research community is actively developing advanced energy storage systems. The commercialization of rechargeable lithium-ion batteries is one of the great successes of modern energy storage technology. Due to their good reliability and mature battery assembly technology, lithium-ion batteries currently dominate the portable energy storage market. Although the energy density of current lithium-ion batteries can reach about 200 Wh / kg by utilizing intercalation materials as electrodes, applications involving electric vehicles and smart grids may require rechargeable batteries with new battery chemistries to achieve higher energy density, thereby achieving longer driving range and higher energy storage capacity. In addition, the lithiated transition metal oxide ion battery cathodes used in commercial lithium-ion batteries are often expensive, scarce or toxic to the environment. Therefore, in order to successfully enter the future battery market, it is necessary to explore new electrode materials that are naturally abundant and environmentally friendly. Lithium-sulfur batteries (LSBs) have attracted widespread attention from academia and industry due to their high theoretical energy density of 2600 Wh / kg and ultra-high theoretical discharge capacity of 1675 mAh / g.

[0003] Despite the outstanding advantages of lithium-sulfur batteries (LSBs), their commercialization process still faces many obstacles. First, the poor conductivity of elemental sulfur and polysulfides (LiPS) hinders the utilization of their inherent high specific capacity, thereby compromising the high-rate performance of the battery. In addition, during the charge and discharge process, the intermediate products of lithium-sulfur batteries (LSBs) are easily dissolved in ether electrolytes. This formation phenomenon not only causes the active materials to detach from the battery electrodes, reducing the effective utilization of these materials, but also causes LiPS to shuttle back and forth between the electrodes, resulting in a "shuttle effect", which leads to the deterioration of the overall electrochemical performance of lithium-sulfur batteries (LSBs). Third, the significant volume change of elemental sulfur during the cycle can cause the active materials to detach from the electrodes, thereby affecting the stability of the positive electrode materials. In addition, the uneven deposition of lithium on the lithium electrode during the cycle can also lead to the formation of severe lithium dendrites, which are likely to dissolve, break and separate from the electrode, resulting in the formation of "dead lithium". Therefore, this process significantly reduces the battery capacity and cycle life.

[0004] In order to overcome the above shortcomings of lithium-sulfur batteries (LSBs), some researchers have adopted various strategies to optimize the electrochemical performance of lithium-sulfur batteries (LSBs) from the aspects of cathode electrode structure and composition, electrolyte optimization, separator modification and anode electrode interface design.

[0005] Covalent organic frameworks (COFs) are promising candidates for separator modification due to their well-defined structures, large surface areas, uniform pore distributions, and abundant functional groups. The structural features of COFs bring considerable advantages to separator modification, including polysulfide adsorption and lithium ion migration. The permanent porosity of COFs can confine polysulfides to the cathode region and promote lithium ion conduction. In addition, the abundant heteroatoms in COFs, such as imines and triazines, can interact with sulfur through lithiophilic and sulfurophilic interactions. The good compatibility of covalent organic framework materials (COFs), carbon materials, and inorganic materials further enriches the interactions with sulfur species. These interactions can synergistically capture polysulfides in the cathode region of soluble species. Recent research progress has shown that COFs have advantages in separator modification and can improve the electrochemical performance of lithium-sulfur batteries.

[0006] Defects and shortcomings of the existing technology:

[0007] So far, the modification of lithium-sulfur batteries can be mainly divided into the following aspects: (1) Diaphragm modification: using covalent organic frameworks (COF), polymers, nanocomposites and other materials to modify the diaphragm to improve the cycle life and safety of the battery. (2) Positive and negative electrode modification: by designing new positive and negative electrode materials, such as sulfur-carbon composites, sulfide-coated carbon nanotubes, etc., to improve the energy density and cycle stability of the battery. (3) Electrolyte modification: adding lithium salts, additives or using ionic liquids to improve the conductivity and stability of the electrolyte, thereby improving the performance of the battery.

[0008] However, the current membrane modification technology still has some shortcomings: (1) Increased cost: Some membrane modification technologies require expensive additives, which increases the cost of battery production. (2) Ion transport resistance: Some modified membranes may affect the transmission rate of lithium ions or sulfur, limiting battery performance. (3) Safety issues: Some modifiers may cause battery safety and stability issues, such as thermal runaway and short circuit risks. Summary of the invention

[0009] In view of the problems existing in the prior art, the present application proposes a method for modifying a lithium-sulfur battery diaphragm modified by an ionic covalent organic framework, a modified diaphragm, and a battery containing the modified diaphragm. The present application uses a covalent organic framework material of an ionic COF as a modified material for a multifunctional diaphragm of a lithium-sulfur battery. First, the prepared two-dimensional cationic COFs (TB-COF) are used as the main material for modifying the lithium-sulfur battery diaphragm. Then, HSO3- is encapsulated into the cationic framework through an ion exchange process, and is named HSO3-@TB-COF. The present application discloses a method for improving the electrochemical performance of a Li-S battery. The preparation process is as follows: 2,4,6-tris(4-formylphenyl)-1,3,5-triazine and ethidium bromide (EB) are used as monomers to prepare a cationic COF (TB-COF), and then HSO3- is used through an ion exchange method. - Ion replacement Br - HSO3-@TB-COF was prepared and the obtained material was coated on PP film to obtain HSO3 - @TB-COF modified diaphragm.

[0010] The above-mentioned object of the present invention is achieved by the following technical solutions:

[0011] A method for preparing a modified diaphragm for a lithium-sulfur battery using an ionic covalent organic framework, specifically comprising the following steps:

[0012] S1. Synthesis of TB-COF

[0013] 2,4,6-tris(4-formylphenyl)-1,3,5-triazine, ethidium bromide (EB), the mixed solution and the acetic acid solution were sequentially added into a pyrex tube, and then rapidly frozen in liquid nitrogen after ultrasonication, and degassed by three cycles of freezing-evacuation-freezing, and then vacuum sealed and heated, and the deep red precipitate was collected by centrifugation, washed three times with acetone, and finally vacuum dried to obtain TB-COF;

[0014] S2、HSO3 - Preparation of @TB-COF

[0015] TB-COF was dispersed in 0.1 M sodium bisulfite solution, stirred at room temperature for 24 h, then filtered, washed with deionized water 2-3 times, and vacuum dried to obtain HSO3 - @TB-COF;

[0016] S3. Preparation of modified diaphragm

[0017] (1) Dry grinding: HSO3 - @TB-COF, polyvinylidene fluoride (PVDF) and Super-P were mixed and ball-milled for 30 min to obtain a mixed material;

[0018] (2) Wet grinding: Add N-methylpyrrolidone (NMP) solution to the mixed material and ball mill for 1-2 h to obtain a slurry;

[0019] (3) coating the slurry on the surface of polypropylene and then vacuum drying to obtain a modified diaphragm;

[0020] The molar ratio of 2,4,6-tris(4-formylphenyl)-1,3,5-triazine to ethidium bromide (EB) in step S1 is 2:3;

[0021] The mixed solution in step S1 is a mixed solution of n-butanol and o-dichlorobenzene, and the volume ratio of n-butanol to o-dichlorobenzene is (1-4):1;

[0022] The concentration of the acetic acid solution in step S1 is 3-9 M, and the volume ratio of the acetic acid solution to the mixed solution is 1:(8-20);

[0023] The ultrasonic time in step S1 is 5 to 10 minutes;

[0024] The heating in step S1 is specifically heating at 120°C for 72 to 120 hours;

[0025] The vacuum drying temperature in step S1 is 80 to 100°C, and the vacuum drying time is 10 to 12 hours;

[0026] The dosage ratio of TB-COF and sodium bisulfite solution in step S2 is 100 mg: (80 ~ 100) mL;

[0027] The vacuum drying temperature in step S2 is 80-100°C;

[0028] HSO3 in step S3 - @The weight ratio of TB-COF, polyvinylidene fluoride (PVDF) and Super-P is 7:1:2;

[0029] The vacuum drying temperature in step S3 is 50 to 60°C, and the vacuum drying time is 12 to 24 hours;

[0030] A lithium-sulfur battery modified diaphragm prepared by using the covalent organic framework material obtained by the above method;

[0031] A lithium-sulfur battery comprises a diaphragm which is a lithium-sulfur battery modified diaphragm prepared by using the above-mentioned covalent organic framework material.

[0032] Compared with the prior art, the present invention has the following advantages:

[0033] 1. A cationic covalent organic framework TB-COF was synthesized by a solvothermal method. HSO3 with anionic groups was prepared through an ion exchange process. - @TB-COF. TB-COF and HSO3 - @TB-COF exhibits good stability and high specific surface area. As a separator modification material for Li-S batteries, it can enhance the stability of the battery.

[0034] 2. TB-COF and HSO3 - @TB-COF has an ordered structure that can increase the conductivity of lithium ions in the separator, thereby improving the charge and discharge efficiency of the battery. In addition, TB-COF has cationic sites that can promote lithium ion transport, thereby promoting battery reaction kinetics. Compared with TB-COF, the introduction of HSO3 - As anionic groups, anionic groups can form electrostatic repulsion with soluble polysulfides, allowing positively charged lithium ions to jump while inhibiting the migration of negatively charged polysulfides to the anode. This mechanism helps to inhibit the shuttle effect of polysulfides and improve the rate performance and cycle stability of the battery. The application of this modified separator in Li-S batteries will significantly improve battery performance and provide new ideas for the electrochemical performance of Li-S batteries;

[0035] 3. HSO3 - @TB-COF has anionic groups that can effectively inhibit the shuttle effect by repelling polysulfide anions through electrostatic repulsion, and HSO3 - @The anionic groups in TB-COF can provide coordination sites for lithium ions, thereby improving the mobility of lithium ions. Experimental results show that after 500 cycles at a current density of 1 C, the first cycle can provide a high initial capacity of 968 mAh / g, and the capacity decay rate is only 0.04%. Under the same conditions, the initial capacity of the TB-COF modified battery is 931 mAh / g, and the decay rate is 0.1%. Therefore, using HSO3 - The Li-S batteries with @TB-COF separators show excellent rate capability and stable long-cycle performance, providing a new approach to explore effective functional separators for developing high-performance Li-S batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 Schematic diagram of the synthesis process of the polymer HSO3-@TB-COF of the present invention;

[0037] Figure 2 is the XRD pattern of the polymer obtained in Example 1 of the present invention;

[0038] Figure 3is a scanning electron microscope image of the polymer obtained in Example 1 of the present invention, wherein: Figure 3 (a) is the scanning electron microscopy image of polymer TB-COF; Figure 3 (b) is the scanning electron microscopy image of the polymer HSO3-@TB-COF;

[0039] Figure 4 The nitrogen adsorption-desorption analysis and pore size distribution diagram of the polymer obtained in Example 1 of the present invention are shown in FIG. Figure 4 (a) TB-COF and HSO3 - @TB-COF N2 adsorption and desorption isotherm diagram, Figure 4 (b) TB-COF and HSO3 - @TB-COF pore size distribution diagram;

[0040] Figure 5 This is the XPS graph of the polymer obtained in Example 1 of the present invention;

[0041] Figure 6 This is a CV diagram of the Li-S battery prepared in Example 1 of the present invention, wherein: Figure 6 (a) is the CV diagram of TB-COF battery. Figure 6 (b) HSO3 - @CV diagram of TB-COF battery; Figure 6 (c) CV graphs of two modified batteries. Figure 6 (d) EIS graph of TB-COF and HSO3-@TB-COF batteries;

[0042] Figure 7 This is a performance diagram of the Li-S battery prepared in Example 1 of the present invention, wherein: Figure 7 (a) Rate performance of TB-COF and HSO3-@TB-COF modified batteries; Figure 7 (b) and Figure 7 (c) Discharge-charge curves of the modified batteries of TB-COF and HSO3-@TB-COF at different current densities of 0.1C, 0.2C, 0.5C, 1C and 2C, respectively. Figure 7 (d) TB-COF and HSO3 - @TB-COF charge and discharge comparison at 0.1 C, Figure 7 (e) TB-COF and HSO3 - @TB-COF modified battery 500 long cycle performance diagram at 1 C;

[0043] Figure 8 is the XRD pattern of the polymer obtained in Example 2 of the present invention;

[0044] Fig. 9is the XRD pattern of the polymer obtained in Example 3 of the present invention;

[0045] Fig.10 XRD pattern of the polymer obtained in Example 4 of the present invention. DETAILED DESCRIPTION

[0046] The following will clearly and completely describe the concept of the present invention and the technical effects produced in combination with the embodiments and drawings, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.

[0047] The present invention is further described below in conjunction with the embodiments. The instruments and equipment used in the embodiments of the present invention and their models are: Shanghai Chenhua electrochemical workstation (Chenhua CHI660E) and Blue Electric Battery Test System (CT2001A).

[0048] The cyclic voltammetry curves of Li-S batteries at 0.1 mV s in the voltage range of 1.7-2.8 V were measured on a Shanghai Chenhua electrochemical workstation (Chenhua CHI660E). The electrochemical impedance spectroscopy was used to measure the cycling stability at 1 C and the rate performance of Li-S batteries at different current densities on a Blue Battery Test System (CT2001A).

[0049] The assembly process of the Li-S battery of the present invention comprises the following steps:

[0050] 1. Preparation of positive electrode

[0051] Carbon / sulfur (C / S) composites: Super-P powder and sulfur powder were first mixed in a mass ratio of 2.5:7.5, ground thoroughly in a mortar, and then placed in a polytetrafluoroethylene-lined reactor and heated at 155 °C for 12-20 h in an argon atmosphere.

[0052] Preparation of positive electrode: C / S, Super-P and polyvinylidene fluoride (PVDF) were fully mixed at a ratio of m(C / S): m(Super-P): m(PVDF) = 8:1:1; the mixture was ball-milled in an agate ball mill for 30 to 60 min; 10 to 30 mL of N-methylpyrrolidone (NMP) was then added and the mixture was ball-milled again for 1 to 2 h to prepare a uniform slurry; the slurry was coated on a carbon aluminum foil and evenly coated using a four-sided sampler, and dried in a vacuum drying oven at 50 to 60 °C for 12 h. After drying, the mixture was cut into 12 mm discs with a sulfur content of 1 to 1.5 mg cm -2 , and obtain the positive electrode sheet;

[0053] 2. Configuration of conventional electrolyte

[0054] In the electrolyte solvent of ethylene glycol dimethyl ether (DME) and 1,3-dioxolane (DOL) in a volume ratio of 1:1, 30 ~ 40 μL of 1 mol L -1 LiTFSI and 1 wt% LiNO3 were used as solutes; DOL / DME electrolyte in Li-S battery was prepared by magnetic stirring for 12 to 24 h.

[0055] 3. Assembly of Li-S battery:

[0056] In a glove box filled with argon with an oxygen content of < 0.01 ppm and a water content of < 0.01 ppm, the assembly was performed in the following order: a. Place the positive electrode shell; b. Place the positive electrode sheet; c. Drop the electrolyte, which is a conventional electrolyte containing 1 M LiTFSI and 1 wt% LiNO3 as solutes, and v (DOL): v (DME) = 1:1 as a solvent; d. Place the diaphragm; e. Place the lithium sheet; f. Place the gasket; g. Place the shrapnel; h. Place the negative electrode shell; Use a battery packaging machine to package the battery and apply a pressure of 5 MPa;

[0057] The diaphragm described in the above step 3 is a modified diaphragm for preparing a lithium-sulfur battery using the covalent organic framework material of the present invention.

[0058] Example 1

[0059] S1. 0.2 mmol of 2,4,6-tris(4-formylphenyl)-1,3,5-triazine, 0.3 mmol of ethidium bromide (EB), 2 mL of a mixture of n-butanol and o-dichlorobenzene in a volume ratio of 1:1, and 0.2 mL of a 9M acetic acid solution were added to a pyrex tube in sequence, ultrasonicated for 10 min, quickly frozen at 77 K with liquid nitrogen, degassed by three freeze-pump-freeze cycles, vacuum sealed, heated at 120 ºC for 72 h, and the dark red precipitate was collected by centrifugation, washed three times with acetone, and then vacuum dried at 100 ºC for 12 h to obtain the corresponding TB-COF with a yield of 76%;

[0060] S2, disperse 100 mg of TB-COF in 100 mL, 0.1M sodium bisulfite solution and stir at room temperature for 24 h, then filter the mixed solution and wash with deionized water; repeat the above steps, and finally vacuum dry to obtain HSO3-@TB-COF, the process is as follows: Figure 1 As shown in Figure 2, the SEM images of TB-COF polymer and HSO3-@TB-COF polymer show that the polymer has an irregular stripe structure, such as Figure 3As shown;

[0061] S3. Preparation of modified diaphragm

[0062] (1) Dry grinding: TB-COF was mixed with PVDF and Super-P in a weight ratio of 7:1:2, and ball milled for 30 min;

[0063] (2) Wet grinding: Add NMP solution to the above-mentioned uniformly ground material and ball mill for 1 h to obtain a slurry;

[0064] (3) The mixed slurry was evenly coated on the surface of polypropylene with a 40 mm scraper, and then placed in a vacuum oven at 60 °C for 12 h;

[0065] (4) The diaphragm obtained in the previous step was cut into discs with a diameter of 16 mm to obtain a modified diaphragm.

[0066] Example 2

[0067] 0.2 mmol of 2,4,6-tris(4-formylphenyl)-1,3,5-triazine, 0.3 mmol of ethidium bromide (EB), 1 mL of a mixture of mesitylene and 1,4-dioxane in a volume ratio of 4:1, and 0.1 mL of a 6 M acetic acid solution were added to a pyrex tube in sequence, ultrasonicated for 10 min, quickly frozen at 77 K with liquid nitrogen, degassed by three freeze-pump-freeze cycles, vacuum sealed, heated at 120 ºC for 72 h, and the dark red precipitate was collected by centrifugation, washed three times with acetone, and then vacuum dried at 100 ºC for 12 h to obtain the corresponding TB-COF with a yield of 57%; Figure 8 This is the XRD pattern of the polymer obtained in Example 2 of the present invention.

[0068] Example 3

[0069] 0.2 mmol of 2,4,6-tris(4-formylphenyl)-1,3,5-triazine, 0.3 mmol of ethidium bromide (EB), 2 mL of a mixture of n-butanol and mesitylene in a volume ratio of 3:2, and 0.1 mL of a 9 M acetic acid solution were added to a pyrex tube in sequence, ultrasonicated for 10 min, quickly frozen at 77 K with liquid nitrogen, degassed by three freeze-pump-freeze cycles, vacuum sealed, heated at 120 ºC for 72 h, and the dark red precipitate was collected by centrifugation, washed three times with acetone, and then vacuum dried at 100 ºC for 12 h to obtain the corresponding TB-COF with a yield of 48%; Fig. 9 is the XRD pattern of the obtained polymer.

[0070] Example 4

[0071] 0.2 mmol of 2,4,6-tris(4-formylphenyl)-1,3,5-triazine, 0.3 mmol of ethidium bromide (EB), 1 mL of N,N-dimethylformamide solution, and 0.3 mL of 3 M acetic acid solution were added to a pyrex tube in sequence, ultrasonicated for 10 min, quickly frozen at 77 K with liquid nitrogen, degassed by three freeze-pump-freeze cycles, vacuum sealed, heated at 120 ºC for 72 h, and the dark red precipitate was collected by centrifugation, washed three times with acetone, and then vacuum dried at 100 ºC for 12 h to obtain the corresponding TB-COF with a yield of 68%; Fig.10 is the XRD pattern of the obtained polymer.

[0072] The TB-COF obtained in Example 1 exhibits high crystallinity, such as Figure 2 The XRD pattern of TB-COF shown in the figure shows that the synthesized TB-COF shows strong diffraction peaks, indicating that TB-COF has high crystallinity; TB-COF shows strong diffraction peaks at 2θ = 2.3° and 4.72°, and a broad peak at 26°, which are attributed to the 100, 200 and 001 crystal planes, respectively. TB-COF was lattice modeled and Pawley refined using Materials Studio. The experimental data are in good agreement with the calculated PXRD pattern of the Trigonal crystal system. The unit cell parameters provided by Pawley refinement are a = b = 44.49 Å, c = 2.99 Å, α = β = 90° and γ = 120°, Rwp = 3.08% and Rp = 2.47%. At the same time, the crystal structure of TB-COF was theoretically simulated, and the results showed that TB-COF is consistent with the AA stacking model. Compared with TB-COF, HSO3 - The crystallinity of @TB-COF remains almost unchanged, indicating that the COF framework still retains high crystallinity after the ion exchange experiment.

[0073] Figure 4 TB-COF and HSO3 in Example 1 at 77 K - @TB-COF polymers were subjected to nitrogen adsorption / desorption experiments, and their specific surface area and porous properties were experimentally analyzed; both materials showed the characteristics of type IV adsorption isotherms, TB-COF and HSO3 - The BET surface areas of @TB-COF are 386.97 m 2 / g and 182 m 2 / g, and the pore volume is 0.35 cm 3 / g and 0.3 cm 3 / g; the pore size distribution (PSD) of TB-COF and HSO3-@TB-COF was calculated by non-local density functional theory (NLDFT) method. The results showed that the pore size distribution range of these two polymers is concentrated between 1-2 nm; specifically, the maximum pore size of TB-COF is 1.92 nm, while that of HSO3 - The maximum pore size of @TB-COF is 1.08 nm. Compared with TB-COF, HSO3 - @TB-COF's pore size has become smaller because of HSO3 - Anions occupied the pores of TB-COF;

[0074] Figure 5 TB-COF and HSO3 obtained in Example 1 - The X-ray photoelectron spectrum of @TB-COF; XPS results show that there are C, N, and Br elements in TB-COF. The C 1s spectrum can be fitted into two peaks, with the peak at 283.5 eV corresponding to the C=C bond and the peak at 285.2 eV corresponding to the diffraction peak of C=N. The N 1s spectrum can be fitted into three peaks, namely N in the triazine ring (398.7 eV), -N + = (400.0 eV) and C=N (401.2 eV). Compared with the XPS spectrum of TB-COF, HSO3 - The diffraction peak of Br in the spectrum of @TB-COF disappears, and a new diffraction peak from HSO3 appears. - The diffraction peaks of S in the anion are at 166.8 eV and 168 eV, showing HSO3 - The strong absorption peak at 162.7 eV is derived from HSO3 − Weak decomposition.

[0075] The assembly process of lithium-sulfur batteries is as follows:

[0076] 1. Preparation of positive electrode

[0077] Carbon / sulfur (C / S) composites: Super-P powder and sulfur powder were first mixed in a mass ratio of 2.5:7.5, ground thoroughly in a mortar, and then placed in a polytetrafluoroethylene-lined reactor and heated at 155 °C for 12 h in an argon atmosphere;

[0078] Preparation of positive electrode: Carbon / sulfur (C / S) composite material, Super-P and polyvinylidene fluoride (PVDF) were mixed at a ratio of m(C / S): m(Super-P): m(PVDF) = 8:1:1. The mixture was placed in an agate ball mill and ball milled for 30 min. Then 10 ml of N-methylpyrrolidone (NMP) was added and ball milled again for 1 h to make a uniform slurry. The slurry was coated on carbon aluminum foil and evenly coated using a four-sided sampler. The mixture was dried in a vacuum drying oven at 50 °C for 12 h and cut into 12 mm discs after drying. The sulfur content was 1-1.5 mg·cm -2 , and obtain the positive electrode sheet;

[0079] 2. Prepare electrolyte

[0080] In the electrolyte solvent of ethylene glycol dimethyl ether (DME) and 1,3-dioxolane (DOL) at a volume ratio of 1:1, 30 μL of 1 mol L-1 LiTFSI and 1 wt% LiNO3 were added as solutes; the DOL / DME electrolyte commonly used in Li-S batteries was prepared by magnetic stirring for 24 h.

[0081] 3. Assembly of Li-S battery:

[0082] In a glove box filled with argon with an oxygen content of < 0.01 ppm and a water content of < 0.01 ppm, assembly was performed in the following order: a. Place the positive electrode shell; b. Place the positive electrode plate; c. Drop the electrolyte; d. Place the diaphragm prepared in Example 1; e. Place the lithium plate; f. Place the gasket; g. Place the shrapnel; h. Place the negative electrode shell; Use a battery packaging machine to package the battery and apply a pressure of 5 MPa.

[0083] Electrochemical performance test: Measure the cyclic voltammetry curve of the above-mentioned Li-S battery at 0.1 mV / s in the voltage range of 1.7~2.8 V. Electrochemical impedance, cycle stability at 1 C and rate performance of the Li-S battery at different current densities.

[0084] Figure 6 middle Figure 6 (a) shows the use of HSO3 - Rate performance of Li-S batteries with @TB-COF and TB-COF separators at a scan rate of 0.1 mV / s; using HSO3 - The separator of @TB-COF exhibited an excellent initial capacity of 1247 mAh / g at 0.1 C, while the initial capacity of TB-COF was 1117 mAh / g; HSO3 -The discharge capacities of the Li-S battery of @TB-COF at 0.2 C, 0.5 C, 1.0 C, 1.5 C, and 2.0 C are 1065 mAh / g, 930 mAh / g, 834 mAh / g, and 746 mAh / g, respectively, which are significantly larger than the discharge capacities of TB-COF (949 mAh / g, 807 mAh / g, 713 mAh / g, and 619 mAh / g). When the current density is switched back to 0.1 C, the HSO3 - @TB-COF battery showed a discharge capacity of 1008 mAh / g; the above results show that HSO3 - @TB-COF membrane batteries show strong resistance to current shocks, which is because HSO3 - @The presence of HSO3- in the TB-COF interlayer limits the shuttling of polysulfides, thereby improving the rate performance; HSO3 - @TB-COF and TB-COF battery constant current charge and discharge curves at different rates are as follows Figure 6 (b) and 6 (c); the results show that even at 2 C, HSO3 - @The discharge curve of the TB-COF battery still shows two typical discharge platforms. It is worth noting that Figure 6 (d) shows that HSO3 is used at 0.1 C - The battery of @TB-COF presents a stable platform with a polarization voltage of 0.13 V, while the polarization voltage of the TB-COF battery is 0.16 V, which indicates that compared with TB-COF, the battery with HSO3 - The HSO3-@TB-COF is more conducive to inhibiting polysulfides, thus providing a larger specific capacity and lower polarization;

[0085] Figure 7 middle Figure 7 (a) shows the use of HSO3 - @TB-COF and TB-COF separator Li-S battery rate performance, using HSO3 - The separator of @TB-COF exhibits an excellent initial capacity of 1247 mAh / g at 0.1 C, while the initial capacity of TB-COF is 1117 mAh / g. The discharge capacities of the Li-S battery of HSO3-@TB-COF at 0.2C, 0.5C, 1.0C, 1.5C, and 2.0C are 1065 mAh / g, 930 mAh / g, 834 mAh / g, and 746 mAh / g, respectively, which are significantly larger than the discharge capacities of TB-COF (949 mAh / g, 807 mAh / g, 713 mAh / g, and 619 mAh / g). When the current density is switched back to 0.1 C, the initial capacity of HSO3-@TB-COF is 1117 mAh / g.- @TB-COF battery showed a discharge capacity of 1008 mAh / g; the above results show that HSO3 - @TB-COF membrane batteries show strong resistance to current shocks, which is because HSO3 - @TB-COF interlayer HSO3 - The presence of HSO3 limits the shuttling of polysulfides, thereby improving the rate performance; - @TB-COF and TB-COF battery constant current charge and discharge curves at different rates are as follows Figure 7 (b) and 7 (c); the results show that even at 2 C, HSO3 - @The discharge curve of the TB-COF battery still shows two typical discharge platforms. It is worth noting that Figure 7 (d) shows that HSO3 is used at 0.1 C - The battery of @TB-COF presents a stable platform with a polarization voltage of 0.13 V, while the polarization voltage of the TB-COF battery is 0.16 V, which indicates that compared with TB-COF, the battery with HSO3 - The HSO3-@TB-COF is more conducive to inhibiting polysulfides, thus providing a larger specific capacity and lower polarization; in addition, the use of HSO3 - @TB-COF and TB-COF membrane lithium-sulfur batteries were subjected to long cycle tests, such as Figure 7 (e) As shown, HSO3 - The battery with @TB-COF has a capacity of 961 mAh / g after the first cycle at 1 C, and even after 500 cycles, it still maintains a capacity of 785 mAh / g, corresponding to a capacity decay rate of 0.04%. However, the battery with TB-COF has a lower initial capacity of 813 mAh / g, and retains a capacity of 432 mAh / g after cycling, with a capacity decay rate of 0.12%. The experimental results once again show that HSO3 - @TB-HSO3 in COF - It can repel polysulfides and inhibit the shuttle effect, thereby ensuring the stable cyclability of the battery.

[0086] The above embodiments are only partial implementation schemes of the present invention, but the protection scope of the present invention is not limited thereto. The various aspects and implementation schemes of the present invention disclosed herein are only examples of specific ways to make and use the present invention. The present invention is not limited to any limitation due to the sequence and specific operations of the embodiments. Any replacement and changes that can be easily thought of by any researcher familiar with the technical field within the technical scope disclosed by the present invention should be included in the protection scope of the present invention.

Claims

1. A method for modifying a lithium-sulfur battery diaphragm modified with an ionic covalent organic framework, characterized in that: The following steps are involved: S1. Synthesis of TB-COF 2,4,6-tris(4-formylphenyl)-1,3,5-triazine, ethidium bromide (EB), the mixed solution and the acetic acid solution were sequentially added into a pyrex tube, and then rapidly frozen in liquid nitrogen after ultrasonication, and degassed by three cycles of freezing-evacuation-freezing, and then vacuum sealed and heated, and the deep red precipitate was collected by centrifugation, washed three times with acetone, and finally vacuum dried to obtain TB-COF; S2、HSO3 - Preparation of @TB-COF TB-COF was dispersed in 0.1 M sodium bisulfite solution, stirred at room temperature for 24 h, then filtered, washed with deionized water 2-3 times, and vacuum dried to obtain HSO3 - @TB-COF; S3. Preparation of modified diaphragm Add HSO3 in a weight ratio of 7:1:2 - @TB-COF, polyvinylidene fluoride (PVDF) and Super-P were mixed and ball-milled for 30 min, and then N-methylpyrrolidone (NMP) solution was added and ball-milled for 1-2 h to obtain a slurry; the slurry was coated on the surface of polypropylene and then vacuum dried to obtain a modified diaphragm; The molar ratio of 2,4,6-tris(4-formylphenyl)-1,3,5-triazine to ethidium bromide (EB) is 2:3; The mixed liquid is a mixed liquid of n-butanol and o-dichlorobenzene; The dosage ratio of the TB-COF and the sodium bisulfite solution is 100 mg: (80-100) mL.

2. The method for modifying the diaphragm of a lithium-sulfur battery modified with an ionic covalent organic framework according to claim 1, characterized in that: The volume ratio of n-butanol to o-dichlorobenzene is (1-4):

1.

3. The method for modifying the diaphragm of a lithium-sulfur battery modified with an ionic covalent organic framework according to claim 1, characterized in that: The concentration of the acetic acid solution in step S1 is 3-9 M, and the volume ratio of the acetic acid solution to the mixed solution is 1:(8-20).

4. The method for modifying the diaphragm of a lithium-sulfur battery modified with an ionic covalent organic framework according to claim 1, characterized in that: The ultrasonic time in step S1 is 5 to 10 minutes.

5. The method for modifying the diaphragm of a lithium-sulfur battery modified with an ionic covalent organic framework according to claim 1, characterized in that: The heating in step S1 is heating at 120°C for 72 to 120 hours.

6. The method for modifying the diaphragm of a lithium-sulfur battery modified with an ionic covalent organic framework according to claim 1, characterized in that: The vacuum drying temperature in step S1 is 80 to 100°C, and the vacuum drying time is 10 to 12 hours.

7. The method for modifying the diaphragm of a lithium-sulfur battery modified with an ionic covalent organic framework according to claim 1, characterized in that: The vacuum drying temperature in step S2 is 80-100°C.

8. The method for modifying the diaphragm of a lithium-sulfur battery modified with an ionic covalent organic framework according to claim 1, characterized in that: The vacuum drying temperature in step S3 is 50 to 60° C., and the vacuum drying time is 12 to 24 h.

9. A lithium-sulfur battery modified diaphragm modified with an ionic covalent organic framework prepared by the method according to any one of claims 1 to 8.

10. A lithium-sulfur battery, wherein the separator contained therein is the lithium-sulfur battery modified separator modified with the ionic covalent organic framework according to claim 9.