Method for producing long glass fiber and long glass fiber
By adjusting the composition of glass raw materials, ensuring that the S+A-B-C range is within a specific range, the recycling rate and temperature problems in the manufacturing of long glass fibers are solved, and efficient glass fiber reuse and low-temperature spinning are achieved.
Patent Information
- Application Number
- CN202280082060.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-12-27
- Filing Date
- 2022-10-04
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-10-04
AI Technical Summary
In the method of producing long glass fibers using recycled glass fibers, it is difficult to increase the recirculation rate, while suppressing the rise in the liquid phase temperature of the molten glass and narrowing the operating temperature range, and reducing the spinning temperature.
By adjusting the composition of glass raw materials, ensure that the S+A-B-C range is 5.2≤S+A-B-C≤46.9, and the specific content range is 11-75% of the recycled glass fiber and glass fiber mineral materials, satisfying the specific SiO2, Al2O3, B2O3, etc. , CaO and other components to increase the recycling rate and reduce the spinning temperature.
It is achieved to increase the recirculation rate, suppress the increase in the liquid phase temperature and operating temperature range of the molten glass, reduce the spinning temperature, and produce long glass fibers with lower molten glass spinning temperature.
Smart Images

Figure BDA0004887779760000261 
Figure BDA0004887779760000271 
Figure BDA0004887779760000281
Abstract
Description
[Technical field]
[0001] The invention relates to a method for manufacturing long glass fibers and the long glass fibers. [Background Technology]
[0002] Conventionally, glass fiber reinforced resin molded products have been widely used as metal substitute materials for automobile parts and the like because they contribute to reducing environmental loads by improving fuel efficiency as a result of weight reduction.
[0003] In recent years, with the increasing concern about environmental issues, in order to reduce the amount of waste, it is expected to recover and reuse glass fibers from used glass fiber reinforced resin molded products. Patent document 1 describes a method for producing a glass fiber reinforced plastic sheet by recycling glass fibers (hereinafter sometimes referred to as "recovered glass fibers") recovered by dissolving resin from a glass fiber reinforced resin molded product.
[0004] The present inventors have provided a method for producing long glass fibers, which comprises mixing glass fibers recovered from glass fiber reinforced resin molded products with various ores or materials refined from ores, i.e., glass fiber mineral materials, as raw materials, melting and spinning the mixture into long fibers (Patent Document 2).
[0005] From the perspective of reducing the amount of waste, it is expected to increase the amount of recycled glass fiber used relative to the total amount of glass raw materials (hereinafter sometimes referred to as "recycling rate"). However, in the method for manufacturing long glass fibers using recycled glass fibers, the content of components other than glass fibers increases by a manufacturing method with a high recycling rate, so compared with the method for manufacturing long glass fibers using only glass fiber mineral materials, the liquidus temperature of the molten glass obtained by melting the glass raw materials increases, the operating temperature range of the molten glass becomes narrower, and the spinnability of the molten glass decreases. In addition, depending on the glass composition of the manufactured glass fiber, the spinning temperature (1000 poise temperature) increases, and a large amount of energy is required to keep the furnace at a high temperature. Even if the recycling rate is increased, there is a disadvantage of causing environmental load.
[0006] [Prior art literature]
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Publication No. 2003-55475
[0009] Patent Document 2: Japanese Patent Application No. 2021-107957 [Summary of the invention]
[0010] Problems to be solved by the invention
[0011] In a method for producing long glass fibers using recycled glass fibers, it is desired to increase the recycling rate, suppress the increase in the liquidus temperature of the molten glass and the narrowing of the operating temperature range of the molten glass, and produce long glass fibers with a low spinning temperature, but such a method for producing long glass fibers has not yet been provided. The problem to be solved by the present invention is to provide a method for producing long glass fibers using recycled glass fibers, the method being able to increase the recycling rate, suppress the increase in the liquidus temperature of the molten glass and the narrowing of the operating temperature range of the molten glass, and produce long glass fibers with a low spinning temperature.
[0012] Means for solving problems
[0013] The inventors have repeatedly conducted research in view of the above-mentioned problems and have found that when the glass compositions of the recycled glass fiber and the glass fiber mineral material are different and satisfy a predetermined relationship, the recycling rate is increased, the increase in the liquidus temperature of the molten glass and the narrowing of the operating temperature range of the molten glass are suppressed, and the spinning temperature is lowered. The present invention has been completed based on these findings.
[0014] The present invention is a method for producing long glass fibers, comprising: a glass melting step of melting glass raw materials including glass fibers recovered from glass fiber reinforced resin molded products and glass fiber mineral materials to produce molten glass; and
[0015] a spinning step of spinning the molten glass to form long glass fibers,
[0016] The glass raw material contains glass fibers recovered from the glass fiber reinforced resin molded product in a range of 11 to 75% by mass and satisfies the following formula (1):
[0017] 5.2≤S+ABC≤46.9 (1)
[0018] Among them, S, A, B and C are as follows:
[0019] S = the content of SiO2 relative to the total amount of the glass fiber mineral material (mass %) - the content of SiO2 relative to the total amount of glass fibers recovered from the glass fiber reinforced resin molded product (mass %)
[0020] A = the content of Al2O3 relative to the total amount of the glass fiber mineral material (mass %) - the content of Al2O3 relative to the total amount of glass fibers recovered from the glass fiber reinforced resin molded product (mass %)
[0021] B = the content of B2O3 relative to the total amount of the glass fiber mineral material (mass %) - the content of B2O3 relative to the total amount of glass fibers recovered from the glass fiber reinforced resin molded product (mass %)
[0022] C=CaO content (mass %) relative to the total amount of the glass fiber mineral material−CaO content (mass %) relative to the total amount of glass fibers recovered from the glass fiber reinforced resin molded product.
[0023] The method for producing long glass fibers of the present invention can improve the recycling rate, suppress the increase in liquidus temperature and the narrowing of the operating temperature range of the molten glass, and reduce the spinning temperature of the molten glass to produce long glass fibers.
[0024] In the method for producing a long glass fiber of the present invention, it is preferred that the following formula (2) is satisfied:
[0025] 10.8≤S+ABC≤34.3 (2)
[0026] Wherein, S, A, B and C are as described above.
[0027] When S, A, B, and C satisfy the above formula (2), the spinning temperature of the molten glass can be further lowered to produce long glass fibers in which a decrease in the elastic modulus of the glass fibers is suppressed.
[0028] The content of the glass fiber recovered from the glass fiber reinforced resin molded product in the glass raw material is preferably in the range of 15 to 75 mass %, more preferably in the range of 15 to 60 mass %. When the content is in this range, the liquidus temperature of the molten glass can be lowered to produce long glass fibers.
[0029] In the method for producing a long glass fiber of the present invention, it is more preferable to satisfy the following formula (3):
[0030] 14.9≤S+ABC≤32.4 (3)
[0031] Wherein, S, A, B and C are as described above.
[0032] When S, A, B, and C satisfy the above formula (3), the increase in the liquidus temperature of the molten glass and the narrowing of the operating temperature range can be further suppressed to produce long glass fibers.
[0033] In the method for producing a long glass fiber of the present invention, it is further preferred that the following formula (4) is satisfied:
[0034] 21.9≤S+ABC≤30.4 (4)
[0035] Wherein, S, A, B and C are as described above.
[0036] When S, A, B and C satisfy the above formula (4), the spinning temperature of the molten glass can be particularly lowered to produce long glass fibers.
[0037] The present invention also provides a long glass fiber obtained by melting and spinning a glass raw material containing glass fibers recovered from a glass fiber reinforced resin molded product and a glass fiber mineral material, wherein the glass raw material contains glass fibers recovered from the glass fiber reinforced resin molded product in an amount in the range of 11 to 75% by mass and satisfies the above formula (1), and the long glass fiber is spun to contain SiO2 in an amount in the range of 48.00 to 62.00% by mass, Al2O3 in an amount in the range of 12.00 to 21.40% by mass, B2O3 in an amount in the range of 0.10 to 15.00% by mass, CaO in an amount in the range of 10.00 to 22.50% by mass, MgO in an amount in the range of 1.30 to 10.00% by mass, and P2O5, TiO2, and ZnO in an amount in the range of 0.01 to 10.00% by mass in total, relative to the total amount of the long glass fiber. The long glass fiber of the present invention is a long glass fiber in which the recycling rate of raw materials is large, the spinning temperature of the molten glass is reduced, and the increase in the liquidus temperature of the molten glass and the narrowing of the operating temperature range of the molten glass are suppressed. [Specific implementation method]
[0038] Embodiments of the present invention will be described in more detail.
[0039] The method for producing long glass fibers of the present embodiment includes a glass melting step of melting glass raw materials including recycled glass fibers and glass fiber mineral materials to produce molten glass, and a spinning step of spinning the molten glass to produce long glass fibers.
[0040] The long glass fibers of the present embodiment are obtained by melting and spinning the glass raw material including the recycled glass fibers and the glass fiber mineral material.
[0041] [Glass fiber reinforced resin molded products]
[0042] The glass fiber reinforced resin molded product can be obtained, for example, by the following method: the glass filaments of the glass fiber are bundled, and the short strands with a specified length and a thermoplastic resin are mixed with a twin-shaft kneading machine to obtain resin pellets, and the obtained resin pellets are used for injection molding. In addition, the glass fiber reinforced resin molded product can be obtained by injection compression molding, two-color molding, hollow molding, foam molding (including supercritical fluid foam molding), insert molding, in-mold coating molding, extrusion molding, sheet molding, thermoforming, rotational molding, lamination molding, compression molding, blow molding, stamping molding, infusion, hand lay-up, spraying, resin transfer molding, sheet molding compound molding, bulk molding compound molding, pultrusion molding, filament winding and other known molding methods.
[0043] <Glass Fiber>
[0044] The glass composition of the glass of the above-mentioned glass fibre that forms the above-mentioned glass-fiber reinforced resin molded product is not particularly limited. As the glass composition that can be adopted for above-mentioned glass fibre, for example, the most commonly used E glass composition, acid-resistant glass composition, high-strength high elastic modulus glass composition, high elastic modulus easy manufacturability glass composition and low dielectric constant low dielectric loss tangent glass composition etc. can be enumerated. From the viewpoint of versatility, the glass composition of the glass of the above-mentioned glass fibre that forms the above-mentioned glass-fiber reinforced resin molded product is preferably E glass composition or acid-resistant glass composition. In addition, because the circulation is many and the effect of reducing environmental load is good, the glass composition of the glass of the above-mentioned glass fibre that forms the above-mentioned glass-fiber reinforced resin molded product is more preferably E glass composition.
[0045] The E glass composition is as follows: relative to the total amount of glass fiber, it contains SiO2 in the range of 52.0 to 56.0 mass%, Al2O3 in the range of 12.0 to 16.0 mass%, MgO and CaO in the range of 20.0 to 25.0 mass% in total, and B2O3 in the range of 0.0 to 10.0 mass%.
[0046] The acid-resistant glass composition is a composition containing SiO2 in a range of 52.0 to 62.0 mass %, Al2O3 in a range of 12.0 to 16.0 mass %, and MgO and CaO in a range of 16.0 to 30.0 mass % in total, relative to the total amount of the glass fiber.
[0047] The above-mentioned high-strength and high-elastic modulus glass composition is the following composition: relative to the total amount of glass fiber, it contains SiO2 in the range of 60.0 to 70.0 mass%, Al2O3 in the range of 20.0 to 30.0 mass%, MgO in the range of 5.0 to 15.0 mass%, Fe2O3 in the range of 0 to 1.5 mass%, and Na2O, K2O and Li2O in the range of 0 to 0.2 mass% in total.
[0048] The above-mentioned high elastic modulus and easy-to-manufacture glass composition is the following composition: relative to the total amount of glass fiber, it contains SiO2 in the range of 57.0 to 60.0 mass%, Al2O3 in the range of 17.5 to 20.0 mass%, MgO in the range of 8.5 to 12.0 mass%, CaO in the range of 10.0 to 13.0 mass%, and B2O3 in the range of 0.5 to 1.5 mass%, and the total amount of SiO2, Al2O3, MgO and CaO is greater than 98.0 mass%.
[0049] The above-mentioned low dielectric constant and low dielectric loss tangent glass composition is the following composition: relative to the total amount of glass fiber, it contains SiO2 in the range of 48.0 to 62.0 mass%, B2O3 in the range of 17.0 to 26.0 mass%, Al2O3 in the range of 9.0 to 18.0 mass%, CaO in the range of 0.1 to 9.0 mass%, MgO in the range of 0 to 6.0 mass%, Na2O, K2O and Li2O in the range of 0.05 to 0.5 mass%, TiO2 in the range of 0 to 5.0 mass%, SrO in the range of 0 to 6.0 mass%, F2 and Cl2 in the range of 0 to 3.0 mass%, and P2O5 in the range of 0 to 6.0 mass%.
[0050] <Resin>
[0051] As the resin forming the above-mentioned glass fiber reinforced resin molded product, thermoplastic resins or thermosetting resins can be listed, but from the viewpoint of the recyclability of the resin itself, thermoplastic resins are preferred. As the thermoplastic resin forming the above-mentioned glass fiber reinforced resin molded product, polyethylene, polypropylene, polystyrene, styrene / maleic anhydride resin, styrene / maleimide resin, polyacrylonitrile, acrylonitrile / styrene (AS) resin, acrylonitrile / butadiene / styrene (ABS) resin, chlorinated polyethylene / acrylonitrile / styrene (ACS) resin, acrylonitrile / ethylene / styrene (AES) resin, acrylonitrile / styrene / methyl acrylate (ASA) resin, styrene / acrylonitrile (SAN) resin, methacrylic resin, polyvinyl chloride (PVC), polyvinylidene chloride (PVDC), polyamide, polyacetal, polyethylene terephthalate (PET), polybutylene terephthalate (PBT), Polytrimethylene terephthalate (PTT), polycarbonate, polyarylene sulfide, polyethersulfone (PES), polyphenylene sulfone (PPSU), polyphenylene ether (PPE), modified polyphenylene ether (m-PPE), polyaryletherketone, liquid crystal polymer (LCP), fluororesin, polyetherimide (PEI), polyarylate (PAR), polysulfone (PSF), polyamideimide (PAI), polyaminobismaleimide (PABM), thermoplastic polyimide (TPI), polyethylene naphthalate (PEN), ethylene / vinyl acetate (EVA) resin, ionomer (IO) resin, polybutadiene, styrene / butadiene resin, polybutene, polymethylpentene, olefin / vinyl alcohol resin, cyclic olefin resin, cellulose resin, polylactic acid, etc.
[0052] Examples of the polyethylene include high-density polyethylene (HDPE), medium-density polyethylene, low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), and ultra-high molecular weight polyethylene.
[0053] Examples of the polypropylene include isotactic polypropylene, atactic polypropylene, and syndiotactic polypropylene.
[0054] Examples of the polystyrene include general-purpose polystyrene (GPPS) which is atactic polystyrene having an atactic structure, high impact polystyrene (HIPS) obtained by adding a rubber component to GPPS, and syndiotactic polystyrene having a syndiotactic structure.
[0055] Examples of the methacrylic resin include polymers obtained by polymerizing one of acrylic acid, methacrylic acid, styrene, methyl acrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate, butyl methacrylate, and fatty acid vinyl esters alone or by copolymerizing two or more thereof.
[0056] Examples of the polyvinyl chloride include homopolymers of vinyl chloride polymerized by conventionally known methods such as emulsion polymerization, suspension polymerization, microsuspension polymerization, and bulk polymerization, copolymers of vinyl chloride monomers and copolymerizable monomers, and graft copolymers obtained by grafting vinyl chloride monomers onto polymers.
[0057] Examples of the polyamide include polycaprolactam (nylon 6), polyhexamethylene adipamide (nylon 66), polybutylene adipamide (nylon 46), polybutylene sebacate (nylon 410), polypentamethylene adipamide (nylon 56), polypentamethylene sebacate (nylon 510), polyhexamethylene sebacate (nylon 610), polyhexamethylene dodecanoylamine (nylon 612), polydecanediamide (nylon 106), and polydecanediamide. (Nylon 1010), polydodecane diamide (nylon 1012), polyundecanamide (nylon 11), polyundecanamide adipamide (nylon 116), polydodecaneamide (nylon 12), polyxylene adipamide (nylon XD6), polyxylene sebacamide (nylon XD10), polym-phenylene adipamide (nylon MXD6), polyp-phenylene adipamide (nylon PXD6), polybutylene terephthalamide (nylon 4T), polypentamethylene terephthalamide (nylon 5T), polyhexamethylene terephthalamide (nylon 6T), polyhexamethylene isophthalamide (nylon 6I), polynonamethylene terephthalamide (nylon 9T), polydecamethylene terephthalamide (nylon 10T), polyundecanediamine (nylon 11T), polydodecane terephthalamide (nylon 12T), polybutylene isophthalamide (nylon 4I), polybis(3-methyl-4-amino) The invention also includes one of the components such as poly(3-methyl-4-aminohexyl)methane terephthalamide (nylon PACMT), poly(3-methyl-4-aminohexyl)methane isophthalamide (nylon PACMI), poly(3-methyl-4-aminohexyl)methane dodecanamide (nylon PACM12), poly(3-methyl-4-aminohexyl)methane tetradecanoamide (nylon PACM14), and copolymers formed by combining two or more of these components.
[0058] Examples of the polyacetal include homopolymers having oxymethylene units as main repeating units and copolymers mainly composed of oxymethylene units and containing oxyalkylene units having 2 to 8 adjacent carbon atoms in the main chain.
[0059] Examples of the polyethylene terephthalate include polymers obtained by polycondensing terephthalic acid or a derivative thereof with ethylene glycol.
[0060] Examples of the polybutylene terephthalate include polymers obtained by polycondensing terephthalic acid or a derivative thereof with 1,4-butanediol.
[0061] Examples of the polytrimethylene terephthalate include polymers obtained by polycondensing terephthalic acid or a derivative thereof with 1,3-propylene glycol.
[0062] Examples of the polycarbonate include polymers obtained by an ester exchange method in which a dihydroxydiaryl compound is reacted with a carbonate such as diphenyl carbonate in a molten state, and polymers obtained by a phosgene method in which a dihydroxydiaryl compound is reacted with phosgene.
[0063] Examples of the polyarylene sulfide include linear polyphenylene sulfide, cross-linked polyphenylene sulfide having a high molecular weight by a curing reaction after polymerization, polyphenylene sulfide sulfone, polyphenylene sulfide, and polyphenylene sulfide ketone.
[0064] Examples of the modified polyphenylene ether include polymer alloys of poly(2,6-dimethyl-1,4-phenylene) ether and polystyrene, polymer alloys of poly(2,6-dimethyl-1,4-phenylene) ether and styrene / butadiene copolymers, polymer alloys of poly(2,6-dimethyl-1,4-phenylene) ether and styrene / maleic anhydride copolymers, polymer alloys of poly(2,6-dimethyl-1,4-phenylene) ether and polyamides, and polymer alloys of poly(2,6-dimethyl-1,4-phenylene) ether and styrene / butadiene / acrylonitrile copolymers.
[0065] Examples of the polyaryletherketone include polyetherketone (PEK), polyetheretherketone (PEEK), polyetherketoneketone (PEKK), and polyetheretherketoneketone (PEEKK).
[0066] As the above-mentioned liquid crystal polymer (LCP), there can be listed (co)polymers composed of at least one structural unit selected from aromatic hydroxycarbonyl units, aromatic dihydroxy units, aromatic dicarbonyl units, aliphatic dihydroxy units and aliphatic dicarbonyl units as thermotropic liquid crystal polyesters.
[0067] Examples of the fluororesins include polytetrafluoroethylene (PTFE), perfluoroalkoxy resin (PFA), fluorinated ethylene propylene resin (FEP), fluorinated ethylene tetrafluoroethylene resin (ETFE), polyvinyl fluoride (PVF), polyvinylidene fluoride (PVDF), polychlorotrifluoroethylene (PCTFE), and ethylene / chlorotrifluoroethylene resin (ECTFE).
[0068] Examples of the ionomer (IO) resin include copolymers of olefins or styrene and unsaturated carboxylic acids, and polymers in which a part of the carboxyl groups is neutralized with metal ions.
[0069] Examples of the olefin / vinyl alcohol resin include ethylene / vinyl alcohol copolymers, propylene / vinyl alcohol copolymers, ethylene / vinyl acetate copolymer saponified products, and propylene / vinyl acetate copolymer saponified products.
[0070] Examples of the cyclic olefin resin include monocyclic compounds such as cyclohexene, polycyclic compounds such as tetracyclopentadiene, and polymers of cyclic olefin monomers.
[0071] Examples of the polylactic acid include poly-L-lactic acid which is a homopolymer of L-lactic acid, poly-D-lactic acid which is a homopolymer of D-lactic acid, and stereocomplex polylactic acid which is a mixture thereof.
[0072] Examples of the cellulose resin include methyl cellulose, ethyl cellulose, hydroxy cellulose, hydroxymethyl cellulose, hydroxyethyl cellulose, hydroxyethyl methyl cellulose, hydroxypropyl methyl cellulose, cellulose acetate, cellulose propionate, and cellulose butyrate.
[0073] At least one of these thermoplastic resins can be used.
[0074] Examples of the thermosetting resins include unsaturated polyester resins, vinyl ester resins, epoxy (EP) resins, melamine (MF) resins, phenolic resins (PF), polyurethane resins (PU), polyisocyanates, polyisocyanurates, polyimides (PI), urea-formaldehyde (UF) resins, silicone (SI) resins, furan (FR) resins, benzoguanamine (BR) resins, alkyd resins, xylene resins, bismaleimide triazine (BT) resins, and diallyl phthalate resins (PDAP).
[0075] <Additives>
[0076] In addition to glass fiber and resin, various additives may be included in the glass fiber reinforced resin molded product, such as flame retardant, colorant, mold release agent, antioxidant, ultraviolet absorber, antistatic agent, nucleating agent, plasticizer filler, modifier, etc.
[0077] As the above-mentioned flame retardants, there can be listed non-halogen phosphates, halogen-containing phosphates, non-halogen condensed phosphates, halogen-containing condensed phosphates, polyphosphates, red phosphorus as phosphorus-based flame retardants, TBA (tetrabromobisphenol A), DBDPO (decabromodiphenyl ether), OCTA (octabromodiphenyl ether), TBP (tribromophenol) as bromine-based flame retardants, aluminum hydroxide, antimony trioxide, tin oxide, tin hydroxide, molybdenum oxide, antimony pentoxide and magnesium hydroxide as inorganic flame retardants.
[0078] Examples of the colorant include titanium oxide, zinc oxide, zinc sulfide, and carbon black.
[0079] Examples of the release agent include talc stearate, metal soaps, polyethylene wax, ethylenebisstearamide, EDA (ethylenediamine), EBA (ethylenebisstearamide), higher fatty acid sodium salts, and higher fatty acid potassium salts.
[0080] Examples of the antioxidant include phenolic antioxidants, amine antioxidants, sulfur antioxidants, and phosphorus antioxidants.
[0081] Examples of the ultraviolet absorber include salicylate ultraviolet absorbers, benzophenone ultraviolet absorbers, benzotriazole ultraviolet absorbers, cyanoacrylate ultraviolet absorbers, nickel chelate ultraviolet absorbers, and hindered amine ultraviolet absorbers.
[0082] Examples of the antistatic agent include anionic surfactants, cationic surfactants, nonionic surfactants, and amphoteric surfactants.
[0083] Examples of the nucleating agent include talc, dibenzylidene sorbitol, and β-crystal nucleating agents.
[0084] Examples of the plasticizer include phthalic acid plasticizers such as DOP (dioctyl phthalate), DBP (dibutyl phthalate), DHP (diheptyl phthalate), DIDP (diisodecyl phthalate), and DINP (diisononyl phthalate), fatty acid plasticizers, phosphate plasticizers such as TCP (tricresyl phosphate), TMP (trimethyl phosphate), and TEP (triethyl phosphate), adipic acid plasticizers such as DOA (dioctyl adipate), DINA (diisononyl adipate), and DIDA (diisodecyl adipate), polyester plasticizers, and epoxy plasticizers.
[0085] Examples of the filler include talc, mica, glass flakes, glass beads, and calcium carbonate.
[0086] Examples of the above-mentioned modifiers include polybutadiene, styrene-butadiene copolymers, styrene-butadiene-styrene block copolymers, acrylonitrile-butadiene-styrene copolymers, methyl methacrylate-butadiene-styrene copolymers, methyl methacrylate-acrylonitrile-butadiene-styrene copolymers, methyl methacrylate-butadiene copolymers, acrylonitrile-styrene-acrylic rubber copolymers, acrylonitrile-ethylene-propylene rubber-styrene copolymers, methyl methacrylate-acrylic rubber copolymers, methyl methacrylate-acrylic rubber-styrene copolymers, methyl methacrylate-acrylic-butadiene rubber copolymers, methyl methacrylate-acrylic-butadiene rubber-styrene copolymers, methyl methacrylate-(acrylic-silicone IPN rubber) copolymers, and natural rubber.
[0087] <Recycled Glass Fiber>
[0088] The glass fibers are recovered from the glass fiber reinforced resin molded product by, for example, burning the thermoplastic resin contained in the glass fiber reinforced resin molded product, dissolving the resin contained in the glass fiber reinforced thermoplastic resin molded product in a solvent such as benzyl alcohol, etc., wherein the burning is carried out by heating the glass fiber reinforced resin molded product at 450 to 800° C. for 0.5 to 8 hours.
[0089] The recycled glass fiber recovered as described above has a trace amount of organic matter from the glass fiber reinforced resin molded product and organic matter used when recovering the glass fiber from the glass fiber reinforced resin molded product remaining on the surface. The ignition loss of the recycled glass fiber is, for example, in the range of 0.001 to 0.500 mass%, preferably in the range of 0.002 to 0.400 mass%, more preferably in the range of 0.003 to 0.300 mass%, further preferably in the range of 0.004 to 0.200 mass%, further preferably in the range of 0.005 to 0.115 mass%, particularly preferably in the range of 0.010 to 0.100 mass%, even more preferably in the range of 0.015 to 0.075 mass%, and most preferably in the range of 0.020 to 0.060 mass%.
[0090] Here, the ignition loss is an index indicating the amount of trace amounts of organic matter remaining on the surface of the recycled glass fiber, and is measured in accordance with JIS R 3420:2013.
[0091] The number average fiber length of the above-mentioned recycled glass fiber is, for example, in the range of 5 to 5000 μm. From the viewpoint of the solubility of the molten glass after being put into the melting furnace, the number average fiber length of the above-mentioned recycled glass fiber is preferably in the range of 10 to 500 μm, more preferably in the range of 15 to 500 μm, further preferably in the range of 20 to 450 μm, further preferably in the range of 25 to 400 μm, particularly preferably in the range of 30 to 350 μm, particularly preferably in the range of 35 to 330 μm, and most preferably in the range of 40 to 300 μm. In addition, the above-mentioned recycled glass fiber can be recovered from the above-mentioned glass fiber reinforced resin molded product and then crushed into a specified length in a pulverizer such as a ball mill. At this time, the number average fiber length of the above-mentioned recycled glass fiber refers to the number average fiber length of the recycled glass fiber after crushing.
[0092] Here, the number average fiber length of the above-mentioned recycled glass fiber can be calculated by the following method. First, the above-mentioned recycled glass fiber is moved to a glass culture dish, and acetone is used to disperse the above-mentioned recycled glass fiber on the surface of the culture dish. Then, for more than 1000 above-mentioned recycled glass fibers dispersed on the surface of the culture dish, the fiber length is measured using a stereo microscope, and the average value is calculated, and the average value is used as the number average fiber length of the recycled glass fiber.
[0093] The recycled glass fiber may also contain trace amounts of components other than glass fiber from additives contained in the glass fiber reinforced resin molded product. Components other than glass fiber include, for example, metal oxides such as zinc oxide and titanium oxide, non-metal oxides such as phosphorus pentoxide, and organic matter. The metal oxides and non-metal oxides affect the spinnability of the molten glass.
[0094] In the method for producing long glass fibers of the present embodiment, the glass raw material contains the recycled glass fibers in a range of 11 to 75% by mass. When the content of the recycled glass fibers in the glass raw material is less than 11% by mass, the recycling rate in the method for producing long glass fibers is too small. On the other hand, when the content of the recycled glass fibers in the glass raw material is greater than 75% by mass, the liquidus temperature of the molten glass becomes high, and the spinnability of the molten glass decreases.
[0095] The glass raw material preferably contains 15 to 75% by mass, more preferably 15 to 60% by mass of the recycled glass fiber. When the content of the recycled glass fiber is within this range, the liquidus temperature of the glass fiber of the present embodiment can be set to 1250° C. or less. The glass raw material more preferably contains 17 to 50% by mass of the recycled glass fiber, further preferably contains 20 to 45% by mass of the recycled glass fiber, particularly preferably contains 26 to 42% by mass of the recycled glass fiber, and most preferably contains 30 to 40% by mass of the recycled glass fiber.
[0096] <Glass fiber mineral materials>
[0097] The glass fiber mineral material is composed of at least one of a plurality of ores and materials refined from these ores (hereinafter sometimes referred to as "refined materials from ores"). Based on the components contained in the ores and the refined materials from these ores, the types of the ores and the refined materials from these ores, and the content ratios of the ores and the refined materials from these ores can be determined so that the overall glass composition becomes a desired glass composition (hereinafter sometimes referred to as "designed glass composition").
[0098] Examples of the above-mentioned ore include silica sand, feldspar, clay, and limestone. In addition, examples of the above-mentioned refined materials derived from minerals include silica powder, dolomite, talc, clay, alumina, and soda ash.
[0099] <Glass composition of recycled glass fiber and glass fiber mineral materials>
[0100] When the glass composition of the recycled glass fiber is compared with the glass composition of the glass fiber mineral material, the difference in the content of SiO2, Al2O3, B2O3 and CaO satisfies the relationship shown in the following formula (1). That is,
[0101] Assuming that S=the content rate (mass %) of SiO2 relative to the total amount of the above-mentioned glass fiber mineral material-the content rate (mass %) of SiO2 relative to the total amount of the glass fiber recovered from the above-mentioned glass fiber reinforced resin molded product,
[0102] A = the content of Al2O3 relative to the total amount of the above-mentioned glass fiber mineral material (mass %) - the content of Al2O3 relative to the total amount of glass fibers recovered from the above-mentioned glass fiber reinforced resin molded product (mass %),
[0103] B = the content of B2O3 relative to the total amount of the above-mentioned glass fiber mineral material (mass %) - the content of B2O3 relative to the total amount of glass fibers recovered from the above-mentioned glass fiber reinforced resin molded product (mass %),
[0104] When C=the content (mass %) of CaO relative to the total amount of the glass fiber mineral material-the content (mass %) of CaO relative to the total amount of glass fibers recovered from the glass fiber reinforced resin molded article,
[0105] 5.2≤S+ABC≤46.9 (1).
[0106] Among them, regarding the content of the above-mentioned components of the recycled glass fiber and the glass fiber mineral material, Li as a light element can be measured using an ICP emission spectrometer, and other elements can be measured using a wavelength dispersive fluorescent X-ray analyzer.
[0107] As a measuring method, first, a glass batch (formed by mixing glass raw materials) or a glass fiber (in the case where organic matter is attached to the surface of the glass fiber, or in the case where the glass fiber is mainly contained in an organic matter (resin) as a reinforcing material, the organic matter is removed by heating in a muffle furnace at 300 to 650°C for 0.5 to 24 hours, etc.) is placed in a platinum crucible, and in an electric furnace, the glass batch is kept at 1550°C for 4 hours and at 1650°C for 2 hours, and is stirred while melting, and the glass fiber is kept at 1550°C for 6 hours, and is stirred while melting, thereby obtaining a homogeneous molten glass. Then, the obtained molten glass is flowed onto a carbon plate to form glass scraps, which are then crushed and powdered to form glass powder. For Li, which is a light element, the obtained glass powder is decomposed by heating with acid, and then quantitatively analyzed using an ICP emission spectrometer. For other elements, the glass powder is pressed into a disk shape and then quantitatively analyzed using a wavelength dispersive X-ray fluorescence analyzer. The quantitative analysis results can be converted into oxides to calculate the content and total amount of each component, and the content rate of each component can be calculated based on these values.
[0108] SiO2 and Al2O3 of the glass fiber mineral material respectively make the network of the glass firm, thus contributing to the increase of the spinning temperature of the molten glass and the improvement of the elastic modulus of the long glass fiber. On the other hand, B2O3 and CaO of the glass fiber mineral material respectively have a tendency to reduce the viscosity of the molten glass. In addition, when the difference between the glass composition of the glass fiber mineral material and the recycled glass fiber is small, the influence of the trace residual organic and inorganic substances in the recycled glass fiber becomes relatively large, and the liquidus temperature and spinning temperature of the molten glass rise. As a result, when S+ABC satisfies the above formula (1), it is possible to increase the recycling rate, suppress the increase of the liquidus temperature and the narrowing of the working temperature range of the molten glass, and reduce the spinning temperature of the molten glass to manufacture the long glass fiber. When S+ABC is less than 5.2, the liquidus temperature degradation degree of the molten glass becomes too high. On the other hand, when S+ABC is greater than 46.9, the spinning temperature of the molten glass becomes too high.
[0109] Specifically, when S+ABC satisfies the above formula (1), in the method for producing long glass fibers of this embodiment, the spinning temperature can be set to 1400°C or less, the liquidus temperature degradation degree of the molten glass can be set to 50°C or less, and the operating temperature range degradation degree can be set to 80°C or less.
[0110] The degree of liquidus temperature degradation refers to the liquidus temperature increased by mixing recycled glass fibers with glass raw materials composed of glass fiber mineral materials. Specifically, it is the difference between the liquidus temperature of molten glass in the method for manufacturing long glass fibers prepared by mixing recycled glass fibers and the liquidus temperature of molten glass obtained by melting glass raw materials composed of glass fiber mineral materials without mixing recycled glass fibers.
[0111] In addition, the above-mentioned operating temperature range degradation degree indicates the operating temperature range narrowed by mixing recycled glass fibers with glass raw materials composed of glass fiber mineral materials. Specifically, it is the difference between the following operating temperature range of molten glass obtained by melting glass raw materials prepared without mixing recycled glass fibers and the following operating temperature range of molten glass in the method of manufacturing long glass fibers by glass raw materials composed of glass fiber mineral materials prepared by mixing recycled glass fibers.
[0112] The above operating temperature range is the difference between the spinning temperature and the liquidus temperature.
[0113] More preferably, S+ABC satisfies the following formula (2).
[0114] 10.8≤S+ABC≤34.3 (2)
[0115] When the above formula (2) is satisfied, the spinning temperature of the above molten glass can be further reduced to produce long glass fibers in which the reduction in the elastic modulus of the glass fiber is further suppressed. Specifically, the elastic modulus of the long glass fibers obtained by the long fiber manufacturing method of this embodiment can be made to be greater than the elastic modulus of standard E glass (88 GPa). The fiber-reinforced resin molded product containing long glass fibers having an elastic modulus of greater than 88 GPa is a fiber-reinforced resin molded product that fully obtains the reinforcement effect of the long glass fibers. Furthermore, in the long fiber manufacturing method of this embodiment, the spinning temperature can be made below 1350°C.
[0116] Among them, the elastic modulus of the long glass fiber refers to the Young's modulus measured by the following method. First, the long glass fiber is kept at a temperature of 1550°C for 6 hours, and is melted while stirring to obtain a homogeneous molten glass. Next, the obtained molten glass is flowed onto a carbon plate and cooled to make glass scraps. Then, a cutting machine, such as a diamond cutter and a grinder, is used to process the obtained glass scraps into a test piece of 25mm×25mm×5mm, and the Young's modulus is measured as an index of the elastic modulus using an ultrasonic pulse method according to JISR1602:1995. In addition, the value of the above-mentioned Young's modulus can be regarded as the same value as the value of the Young's modulus obtained by measuring the glass scraps obtained by the following method from the following glass raw material instead of the glass scraps obtained by melting the above-mentioned long glass fibers, and the glass raw material is used for manufacturing the above-mentioned long glass fibers, as a mixture of recycled glass fibers and glass fiber mineral materials, or a glass raw material prepared in a manner having the same composition as the above-mentioned long glass fibers. The method for obtaining glass scraps from glass raw materials is as follows: first, the glass raw materials are placed in a platinum crucible, and the platinum crucible is kept in an electric furnace at a temperature ranging from 1400 to 1650° C. for 4 hours, and the glass raw materials are melted while being stirred to obtain a homogeneous molten glass. Then, the molten glass is poured onto a carbon plate and cooled to obtain glass scraps.
[0117] More preferably, S+ABC satisfies the following formula (3).
[0118] 14.9≤S+ABC≤32.4 (3)
[0119] When S, A, B and C satisfy the above formula (3), the increase in the liquidus temperature of the molten glass and the narrowing of the operating temperature range can be further suppressed to produce long glass fibers. Specifically, in the method for producing long fibers of this embodiment, the liquidus temperature degradation degree can be set to 10°C or less, and the operating temperature range degradation degree can be set to 30°C or less.
[0120] Particularly preferably, S+ABC satisfies the following formula (4).
[0121] 21.9≤S+ABC≤30.4 (4)
[0122] When S, A, B, and C satisfy the above formula (4), the spinning temperature of the molten glass can be particularly low to produce long glass fibers. Specifically, in the long fiber production method of the present embodiment, the spinning temperature can be 1320° C. or lower.
[0123] The S is preferably 0.5 or more from the viewpoint of contributing to an increase in the elastic modulus of the long glass fiber, and is preferably 12.4 or less from the viewpoint of contributing to a decrease in the spinning temperature. The S is more preferably in the range of 1.9 to 9.4, further preferably in the range of 2.4 to 8.0, particularly preferably in the range of 2.7 to 7.7, and most preferably in the range of 5.1 to 7.5.
[0124] The above-mentioned A is preferably not less than -3.4 from the viewpoint of contributing to an increase in the elastic modulus of the long glass fiber, and is preferably not more than 13.9 from the viewpoint of contributing to a decrease in the spinning temperature. The above-mentioned A is more preferably in the range of -1.4 to 9.6, further preferably in the range of 0.3 to 8.3, particularly preferably in the range of 0.9 to 7.5, and most preferably in the range of 3.0 to 7.0.
[0125] The above B is preferably -9.9 or more from the viewpoint of contributing to lowering the spinning temperature, and is preferably 17.4 or less from the viewpoint of contributing to increasing the elastic modulus of the long glass fiber. The above B is more preferably in the range of -8.9 to 14.9, further preferably in the range of -7.9 to 9.9, particularly preferably in the range of -6.9 to 8.4, and most preferably in the range of -5.5 to 0.0.
[0126] The C is preferably -20.0 or more from the viewpoint of contributing to lowering the spinning temperature, and is preferably 6.9 or less from the viewpoint of contributing to increasing the elastic modulus of the long glass fiber. The C is more preferably in the range of -14.9 to 4.9, further preferably in the range of -13.4 to 5.4, particularly preferably in the range of -12.5 to 2.5, and most preferably in the range of -9.8 to -4.3.
[0127] The long glass fiber of the present embodiment is spun to contain SiO2 in the range of 48.00 to 62.00 mass %, Al2O3 in the range of 12.00 to 21.40 mass %, B2O3 in the range of 0.10 to 15.00 mass %, CaO in the range of 10.00 to 22.50 mass %, MgO in the range of 1.30 to 10.00 mass %, and P2O5, TiO2, and ZnO in the range of 0.01 to 10.00 mass %, relative to the total amount of the long glass fiber. In addition, the long glass fiber of the present embodiment contains less than 5.00 mass % of other components, or even contains no other components.
[0128] When the glass composition of the above-mentioned long glass fibers is within the above-mentioned range, when general recycled glass fibers, i.e., recycled glass fibers having E glass fibers and acid-resistant glass fibers, are used, the composition difference between the glass fiber mineral material and the recycled glass fibers will not become too small, and when the recycling rate of the raw materials increases, the spinning temperature of the above-mentioned molten glass is lower, and the increase in the liquidus temperature of the above-mentioned molten glass and the narrowing of the operating temperature range of the above-mentioned molten glass are suppressed.
[0129] The long glass fibers of the present embodiment are spun to preferably contain SiO2 in the range of 50.00 to 60.00 mass %, Al2O3 in the range of 13.00 to 19.00 mass %, B2O3 in the range of 0.30 to 5.00 mass %, CaO in the range of 12.00 to 20.00 mass %, MgO in the range of 2.50 to 9.00 mass %, and P2O5, TiO2 and ZnO in the range of 0.01 to 9.50 mass %, relative to the total amount of the long glass fibers, and other components are in the range of 0 to 4.00 mass %.
[0130] The long glass fibers of the present embodiment are spun to preferably contain SiO2 in the range of 51.00 to 59.00 mass %, Al2O3 in the range of 14.00 to 18.50 mass %, B2O3 in the range of 1.00 to 4.50 mass %, CaO in the range of 12.50 to 19.00 mass %, MgO in the range of 3.00 to 8.50 mass %, and P2O5, TiO2 and ZnO in the range of 0.01 to 9.00 mass %, relative to the total amount of the long glass fibers, and other components are in the range of 0 to 3.00 mass %.
[0131] The long glass fibers of the present embodiment are spun to preferably contain SiO2 in the range of 52.00 to 58.00 mass %, Al2O3 in the range of 14.50 to 18.00 mass %, B2O3 in the range of 1.50 to 4.00 mass %, CaO in the range of 13.00 to 18.00 mass %, MgO in the range of 3.50 to 8.00 mass %, and P2O5, TiO2 and ZnO in the range of 0.01 to 8.50 mass % in total, relative to the total amount of the long glass fibers, and other components are in the range of 0 to 2.00 mass %.
[0132] In addition, P2O5, TiO2 and ZnO are components contained in the additives contained in the above-mentioned glass fiber reinforced resin molded product.
[0133] In the long glass fiber of the present embodiment, the total of the absolute values of S, A, B and C is preferably 10.6 or more from the viewpoint of contributing to improving the spinnability of the molten glass even if the recycling rate is increased, and is preferably 46.9 or less from the viewpoint of preventing phase separation of the molten glass. The total of the absolute values of S, A, B and C is more preferably in the range of 12.8 to 31.1, further preferably in the range of 17.1 to 29.9, particularly preferably in the range of 18.1 to 29.4, and most preferably in the range of 22.9 to 28.9.
[0134] In one embodiment of the method for producing long glass fibers of the present embodiment, the glass raw material is supplied to a melting furnace and melted at a temperature in the range of 1400 to 1650° C., for example. Then, the molten molten glass is pulled out from a nozzle head in the range of 1 to 30,000 of a platinum sleeve controlled to a predetermined temperature and quenched to form glass filaments. Next, a sizing agent or adhesive is applied to the formed glass filaments using an applicator as a coating device, and while a sizing device is used to sizing the glass filaments in the range of 1 to 30,000, the sizing device is used to sizing the glass filaments, and the sizing device is used to sizing the glass filaments, and the sizing device is used to sizing the glass filaments, and the sizing device is used to sizing the glass filaments at a high speed to a bobbin, thereby obtaining glass fibers.
[0135] Here, a nozzle head having a non-circular shape and having at least one of a protrusion and a notch for rapidly cooling molten glass may be used as the nozzle head, and the temperature conditions may be controlled to obtain long glass fibers composed of glass filaments having a flat cross-sectional shape.
[0136] The long glass fiber obtained by the production method of this embodiment has a length of at least 1000 m.
[0137] The converted fiber diameter of the glass filament constituting the long glass fiber of the present embodiment is, for example, in the range of 3.0 to 100.0 μm, preferably in the range of 4.0 to 70.0 μm, more preferably in the range of 5.0 to 50.0 μm, further preferably in the range of 6.5 μm to 40.0 μm, and particularly preferably in the range of 7.0 to 30.0 μm. Among them, the converted fiber diameter of the glass filament refers to the diameter of a perfect circle having the same area as the area of the cross-sectional shape of the glass filament. In addition, the cross section of the glass filament refers to the cross section perpendicular to the fiber length direction of the glass fiber.
[0138] The cross-sectional shape of the glass filaments constituting the long glass fiber of the present embodiment is usually circular. When the glass filaments have a flat cross-sectional shape, as its shape, for example, an oblong, an ellipse and a rectangle can be listed. Wherein, an oblong refers to a shape in which the short side portions of the rectangle are replaced with a semicircle with the short side as the diameter.
[0139] When the glass filaments constituting the long glass fibers of the present embodiment have a flat cross-sectional shape, the ratio of the major axis to the minor axis in the cross section (major axis / minor axis) is, for example, in the range of 2.0 to 10.0, and preferably in the range of 3.0 to 8.0.
[0140] The long glass fibers of the present embodiment can be processed into various forms. As forms into which the long glass fibers of the present embodiment can be processed, chopped strands can be listed. The number of glass filaments constituting the chopped strands (the number of bundled strands) is preferably 1 to 20,000, more preferably 50 to 10,000, and further preferably 200 to 8,000. The length of the long glass fibers constituting the chopped strands is preferably 1.0 to 100.0 mm, more preferably 1.2 to 51.0 mm, further preferably 1.5 to 30.0 mm, particularly preferably 2.0 to 15.0 mm, and most preferably 2.3 to 7.8 mm. In addition, as forms into which the long glass fibers of the present embodiment can be processed, in addition to chopped strands, for example, there can be listed coarse yarns of long glass fibers consisting of 10 to 30,000 glass filaments without cutting, and cut fibers obtained by crushing long glass fibers consisting of 1 to 20,000 glass filaments into a length of 0.001 to 0.900 mm by a known device such as a ball mill or a Henschel mixer.
[0141] The long glass fiber of the present embodiment is processed into short strands, for example, and the short strands are mixed with a thermoplastic resin by a twin-shaft mixer, and the obtained resin particles are used for injection molding, so that a glass fiber reinforced resin molded product can be obtained. In addition, the above-mentioned glass fiber reinforced resin molded product can also be obtained by known molding methods such as injection compression molding, two-color molding, hollow molding, foam molding (including supercritical fluid foam molding), insert molding, in-mold coating molding, extrusion molding, sheet molding, thermoforming, rotational molding, lamination molding, compression molding, blow molding, stamping molding, infusion, hand paste, spraying, resin transfer molding, sheet molding compound molding, bulk molding compound molding, pultrusion, and fiber winding.
[0142] The glass fiber reinforced resin molded products are used, for example, for parts such as housings and frames of portable electronic devices such as smartphones, automotive electrical parts such as battery tray covers, sensors, and coil bobbins, electronic equipment parts other than portable electronic devices, and electrical connection terminal parts.
[0143] In the long glass fiber of this embodiment, the surface may be coated with an organic substance for the purpose of improving the adhesion between the glass fiber and the resin, improving the uniform dispersion of the glass fiber in the mixture of the glass fiber and the resin, etc. Examples of such organic substances include polyurethane resins, epoxy resins, vinyl acetate resins, acrylic resins, modified polypropylene, especially carboxylic acid-modified polypropylene, (poly)carboxylic acids, especially maleic acid and unsaturated monomer copolymers, and silane coupling agents.
[0144] In addition to the above-mentioned resin or silane coupling agent, the long glass fiber of this embodiment may be coated with a composition including a lubricant, a surfactant, etc. The composition coats the long glass fiber of this embodiment at a ratio of 0.1 to 2.0 mass % based on the mass of the long glass fiber not coated with the composition.
[0145] The coating of the long glass fiber with the organic substance is carried out as follows: for example, in the manufacturing process of the long glass fiber, the above-mentioned sizing agent or adhesive is applied to the long glass fiber using a known method such as a roller coater. The above-mentioned sizing agent or adhesive contains the above-mentioned resin, the above-mentioned silane coupling agent or the above-mentioned solution of the combination. The coating of the above-mentioned long glass fiber is completed by drying the long glass fiber coated with the above-mentioned resin, the above-mentioned silane coupling agent or the above-mentioned solution of the combination.
[0146] Examples of the silane coupling agent include aminosilane, chlorosilane, epoxysilane, mercaptosilane, vinylsilane, acrylic silane, and cationic silane. The silane coupling agent may be one of these compounds or a combination of two or more thereof.
[0147] Examples of the aminosilane include γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, N-β-(aminoethyl)-N′-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, and γ-anilinopropyltrimethoxysilane.
[0148] Examples of the chlorosilane include γ-chloropropyltrimethoxysilane and the like.
[0149] Examples of the epoxysilane include γ-glycidoxypropyltrimethoxysilane and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane.
[0150] Examples of the mercaptosilane include γ-mercaptotrimethoxysilane and the like.
[0151] Examples of the vinylsilane include vinyltrimethoxysilane and N-β-(N-vinylbenzylaminoethyl)-γ-aminopropyltrimethoxysilane.
[0152] As said acrylic silane, γ-methacryloxypropyltrimethoxysilane etc. are mentioned, for example.
[0153] Examples of the cationic silane include N-(vinylbenzyl)-2-aminoethyl-3-aminopropyltrimethoxysilane hydrochloride and N-phenyl-3-aminopropyltrimethoxysilane hydrochloride.
[0154] Examples of the lubricant include modified silicone oil, animal oil, hydrogenated animal oil, vegetable oil, hydrogenated vegetable oil, animal wax, vegetable wax, mineral wax, condensates of higher saturated fatty acids and higher saturated alcohols, polyethyleneimine, polyalkyl polyamine alkylamide derivatives, fatty acid amides, and quaternary ammonium salts. The lubricant may be used alone or in combination of two or more.
[0155] Examples of the animal oil include beef tallow and the like.
[0156] Examples of the vegetable oil include soybean oil, coconut oil, rapeseed oil, palm oil, and castor oil.
[0157] Examples of the animal wax include beeswax and lanolin.
[0158] Examples of the vegetable wax include candelilla wax and carnauba wax.
[0159] Examples of the mineral wax include paraffin wax and montan wax.
[0160] Examples of the condensate of the higher saturated fatty acid and the higher saturated alcohol include stearic acid esters such as lauryl stearate.
[0161] Examples of the fatty acid amide include dehydration condensates of polyethylene polyamines such as diethylenetriamine, triethylenetetramine, and tetraethylenepentamine, and fatty acids such as lauric acid, myristic acid, palmitic acid, and stearic acid.
[0162] Examples of the quaternary ammonium salt include alkyltrimethylammonium salts such as lauryltrimethylammonium chloride.
[0163] Examples of the surfactant include nonionic surfactants, cationic surfactants, anionic surfactants, and amphoteric surfactants. The surfactant may be used alone or in combination of two or more.
[0164] Examples of the nonionic surfactant include ethylene oxide propylene oxide alkyl ethers, polyoxyethylene alkyl ethers, polyoxyethylene-polyoxypropylene-block copolymers, alkyl polyoxyethylene-polyoxypropylene-block copolymer ethers, polyoxyethylene fatty acid esters, polyoxyethylene fatty acid monoesters, polyoxyethylene fatty acid diesters, polyoxyethylene sorbitan fatty acid esters, glycerol fatty acid ester ethylene oxide adducts, polyoxyethylene stearyl ethers, hydrogenated castor oil ethylene oxide adducts, alkylamine ethylene oxide adducts, fatty acid amide ethylene oxide adducts, glycerol fatty acid esters, polyglycerol fatty acid esters, pentaerythritol fatty acid esters, sorbitol fatty acid esters, sorbitan fatty acid esters, sucrose fatty acid esters, polyol alkyl ethers, fatty acid alkanolamides, acetylene glycols, acetylene alcohols, ethylene oxide adducts of acetylene glycols, and ethylene oxide adducts of acetylene alcohols.
[0165] Examples of the cationic surfactants include alkyl dimethyl benzyl ammonium chloride, alkyl trimethyl ammonium chloride, alkyl dimethyl ethyl ammonium ethyl sulfate, higher alkylamine salts (acetates, hydrochlorides, etc.), ethylene oxide adducts of higher alkylamines, condensates of higher fatty acids and polyalkylene polyamines, salts of esters of higher fatty acids and alkanolamines, salts of higher fatty acid amides, imidazoline type cationic surfactants, and alkyl pyridinium salts.
[0166] Examples of the anionic surfactant include higher alcohol sulfates, higher alkyl ether sulfates, α-olefin sulfates, alkylbenzene sulfonates, α-olefin sulfonates, reaction products of fatty acid halides and N-methyltaurine, dialkyl sulfosuccinates, higher alcohol phosphates, and phosphates of higher alcohol ethylene oxide adducts.
[0167] Examples of the amphoteric surfactant include amino acid-type amphoteric surfactants such as alkylaminopropionic acid alkali metal salts, and betaine-type and imidazoline-type amphoteric surfactants such as alkyldimethylbetaine.
[0168] Example
[0169] Hereinafter, the present invention will be described in more detail based on Examples, but the present invention is not limited thereto.
[0170] In Examples and Comparative Examples, various physical properties were measured or calculated as follows.
[0171] <Glass Composition>
[0172] A glass raw material as a mixture of recycled glass fiber and glass fiber mineral material of each embodiment or comparative example is placed in a platinum crucible, and the platinum crucible is kept in an electric furnace at a temperature in the range of 1400 to 1650°C for 4 hours, and the glass raw material is melted while being stirred to obtain a homogeneous molten glass. Next, the blocky glass scraps obtained by flowing the molten glass onto a carbon plate and cooling are crushed and powdered to make glass powder. After the glass powder is formed into a disc shape by a press, a wavelength dispersion type fluorescent X-ray analyzer is used for quantitative analysis. These quantitative analysis results are converted into oxides to calculate the content and total amount of each component, and the content of each component is obtained based on these numerical values.
[0173] <Spinning Temperature>
[0174] The glass scraps of each embodiment or comparative example obtained by the above method were melted in a platinum crucible using a high-temperature electric furnace equipped with a rotary Brookfield viscometer (manufactured by Shibaura Systems Co., Ltd.). The viscosity of the molten glass was continuously measured using the viscometer provided in the electric furnace while changing the melting temperature. The temperature corresponding to a rotational viscosity of 1000 poise was measured as the spinning temperature.
[0175] <Liquid phase temperature>
[0176] The glass scraps of each embodiment or comparative example obtained by the above method were crushed, and 40 g of glass particles with a particle size of 0.5 to 1.5 mm were placed in a 180×20×15 mm platinum boat, and heated for more than 8 hours in a tubular electric furnace with a temperature gradient of 1000 to 1500° C. Then, the glass scraps were taken out of the tubular electric furnace and observed with a polarizing microscope to determine the position where crystallization (devitrification) from the glass began to precipitate. The temperature in the tubular electric furnace was actually measured using a B thermocouple, and the temperature at which the crystallization began to precipitate was determined and used as the liquidus temperature.
[0177] <Operating temperature range>
[0178] The difference between the spinning temperature and the liquidus temperature was calculated as the operating temperature range.
[0179] <Elastic modulus>
[0180] The glass chips of each example or comparative example obtained by the above method were processed into test pieces of 25 mm×25 mm×5 mm using a cutting machine such as a diamond cutter and a grinder, and the Young's modulus was measured as an index of elastic modulus by an ultrasonic pulse method in accordance with JIS R1602:1995.
[0181] <Liquid phase temperature degradation and operating temperature range degradation>
[0182] The glass fiber mineral material used in each embodiment or comparative example is prepared into glass raw material without mixing with recycled glass fiber, and the glass raw material is placed in a platinum crucible, and the platinum crucible is kept in an electric furnace at a temperature range of 1400 to 1650°C for 4 hours, and the glass raw material is melted while being stirred to obtain a homogeneous molten glass. Then, the molten glass is poured onto a carbon plate and cooled to obtain block-shaped glass scraps, which are used as reference glass. The value obtained by subtracting the liquidus temperature of the molten glass obtained by melting the reference glass from the liquidus temperature of the molten glass in the manufacturing method of the long glass fiber of each embodiment or comparative example is calculated as the liquidus temperature degradation degree. In addition, the value obtained by subtracting the operating range temperature of the molten glass in the manufacturing method of the long glass fiber of each embodiment or comparative example from the operating range temperature of the molten glass obtained by melting the reference glass is calculated as the operating range temperature degradation degree.
[0183] [Example 1]
[0184] After heating the glass fiber reinforced thermoplastic resin molded product at 625°C for 4 hours and incinerating the thermoplastic resin, the residual glass fiber A is recovered. The glass composition of the recovered glass fiber A is shown in Table 1 below, and the number average fiber length of the recovered glass fiber A is 320 μm. 33 parts by mass of recovered glass fiber A are mixed with 67 parts by mass of glass fiber mineral material D having composition D shown in Table 2 below to obtain glass raw material. Then, the glass raw material is placed in a platinum crucible, and the platinum crucible is kept in an electric furnace at a temperature in the range of 1400 to 1650°C for 4 hours, while the glass raw material is stirred and melted to obtain a homogeneous molten glass. Then, the molten glass is flowed onto a carbon plate and cooled to obtain block-shaped glass scraps, and the glass composition, spinning temperature and liquidus temperature are measured, and the operating temperature range, liquidus temperature degradation degree and operating range temperature degradation degree are calculated. The results are shown in Table 3 below.
[0185] [Example 2]
[0186] The same operation as in Example 1 was carried out except that 20 parts by mass of recycled glass fiber A was mixed with 80 parts by mass of glass fiber mineral material D to obtain glass raw material. The results are shown in Table 3 below.
[0187] [Example 3]
[0188] The same operation as in Example 1 was carried out except that 50 parts by mass of recycled glass fiber A was mixed with 50 parts by mass of glass fiber mineral material D to obtain glass raw material. The results are shown in Table 3 below.
[0189] [Example 4]
[0190] The same operation as in Example 1 was carried out except that recycled glass fibers C having the glass composition shown in Table 1 below were recovered. The results are shown in Table 3 below.
[0191] [Example 5]
[0192] The same operation as in Example 1 was carried out except that recycled glass fibers B having the glass composition shown in the following Table 1 were recovered. The results are shown in the following Table 3.
[0193] [Example 6]
[0194] The same operation as in Example 1 was carried out except that 50 parts by mass of recycled glass fiber B was mixed with 50 parts by mass of glass fiber mineral material D to obtain glass raw material. The results are shown in Table 3 below.
[0195] [Example 7]
[0196] The same operation as in Example 1 was carried out except that the glass fiber mineral material E having the composition E shown in Table 2 below was used. The results are shown in Table 3 below.
[0197] [Example 8]
[0198] The same operation as in Example 1 was carried out except that 50 parts by mass of recycled glass fiber A was mixed with 50 parts by mass of glass fiber mineral material E to obtain glass raw material. The results are shown in Table 3 below.
[0199] [Example 9]
[0200] The same operation as in Example 1 was carried out except that 70 parts by mass of recycled glass fiber A was mixed with 30 parts by mass of glass fiber mineral material D to obtain glass raw material. The results are shown in Table 4 below.
[0201] [Example 10]
[0202] The same operation as in Example 1 was carried out except that the glass fiber mineral material F having the composition F shown in the following Table 2 was used. The results are shown in the following Table 4.
[0203] [Example 11]
[0204] The same operation as in Example 1 was carried out except that the glass fiber mineral material G having the composition G shown in the following Table 2 was used. The results are shown in the following Table 4.
[0205] [Comparative Example 1]
[0206] The same operation as in Example 1 was carried out except that the glass fiber mineral material H having the composition H shown in the following Table 2 was used. The results are shown in the following Table 4.
[0207] [Comparative Example 2]
[0208] The same operation as in Example 1 was carried out except that 20 parts by mass of recycled glass fiber A was mixed with 80 parts by mass of the glass fiber mineral material H to obtain a glass raw material. The results are shown in Table 4 below.
[0209] [Comparative Example 3]
[0210] The same operation as in Example 1 was carried out except that the glass fiber mineral material I having the composition I shown in the following Table 2 was used. The results are shown in the following Table 4.
[0211] [Reference Example 1]
[0212] The same operation as in Example 1 was carried out except that 10 parts by mass of recycled glass fiber A was mixed with 90 parts by mass of the glass fiber mineral material H to obtain a glass raw material. The results are shown in Table 4 below.
[0213] [Table 1]
[0214] Table 1
[0215]
[0216] In addition, the unit of the constituent components is mass %.
[0217] [Table 2]
[0218] Table 2
[0219]
[0220] In addition, the unit of the constituent components is mass %. Table 2 also shows the liquidus temperature, spinning temperature, and operating temperature range of molten glass obtained by melting glass fiber mineral materials D to I having compositions D to I, respectively.
[0221] [Table 3]
[0222] Table 3
[0223]
[0224] In addition, the unit of the constituent components is mass %.
[0225] [Table 4]
[0226] Table 4
[0227]
[0228] In addition, the unit of the constituent components is mass %.
[0229] The liquidus temperature degradation degree and the operating temperature range degradation degree of the molten glass in the long glass fiber manufacturing method of Comparative Examples 1 and 2, in which S+ABC is less than the prescribed range, are large. The liquidus temperature of the molten glass in the long glass fiber manufacturing method of Comparative Example 1 is higher than its spinning temperature. In addition, the liquidus temperature and the spinning temperature of the molten glass in the long glass fiber manufacturing method of Comparative Example 3, in which S+ABC is greater than the prescribed range, are high, and its operating temperature range is narrow.
[0230] On the other hand, in the long glass fiber production methods of Examples 1 to 11 in which S+ABC was within the specified range, the liquidus temperature and spinning temperature of the molten glass were low, the operating temperature range was wide, and the liquidus temperature degradation degree and the operating temperature range degradation degree were small.
Claims
1. A method for producing a long glass fiber, comprising: A glass melting step of melting glass raw materials to produce molten glass, wherein the glass raw materials include glass fibers recovered from glass fiber reinforced resin molded products and glass fiber mineral materials; as well as a spinning step of spinning the molten glass to form long glass fibers, The glass raw material contains glass fibers recovered from the glass fiber reinforced resin molded product in an amount ranging from 11 to 75% by mass. The long glass fibers are spun to contain, relative to the total amount of the long glass fibers, 48.00 to 62.00% by mass of SiO2, 12.00 to 21.40% by mass of Al2O3, 0.10 to 15.00% by mass of B2O3, 10.00 to 22.50% by mass of CaO, 1.30 to 10.00% by mass of MgO, and 0.01 to 10.00% by mass of P2O5, TiO2, and ZnO in total, And satisfy the following formula (1): 5.2≤S+ABC≤46.9 (1) Among them, S, A, B and C are as follows: S = the content rate (mass %) of SiO2 relative to the total amount of the glass fiber mineral material - the content rate (mass %) of SiO2 relative to the total amount of glass fibers recovered from the glass fiber reinforced resin molded product, A = the content rate (mass %) of Al2O3 relative to the total amount of the glass fiber mineral material - the content rate (mass %) of Al2O3 relative to the total amount of glass fibers recovered from the glass fiber reinforced resin molded product, B = the content rate (mass %) of B2O3 relative to the total amount of the glass fiber mineral material - the content rate (mass %) of B2O3 relative to the total amount of glass fibers recovered from the glass fiber reinforced resin molded product, C=CaO content (mass %) relative to the total amount of the glass fiber mineral material−CaO content (mass %) relative to the total amount of glass fibers recovered from the glass fiber reinforced resin molded product.
2. The method for producing long glass fibers according to claim 1, wherein: Satisfies the following formula (2): 10.8≤S+ABC≤34.3 (2) Wherein, S, A, B and C are as described above.
3. The method for producing long glass fibers according to claim 1, wherein: The content of the glass fiber recovered from the glass fiber reinforced resin molded product in the glass raw material is in the range of 15 to 60% by mass.
4. The method for producing a long glass fiber according to any one of claims 1 to 3, wherein: Satisfies the following formula (3): 14.9≤S+ABC≤32.4 (3) Wherein, S, A, B and C are as described above.
5. The method for producing long glass fibers according to claim 4, wherein: Satisfies the following formula (4): 21.9≤S+ABC≤30.4 (4) Wherein, S, A, B and C are as described above.