A wear-resistant material for shield cutter and preparation method thereof

By activating diamond and combining it with nickel-based solder, the problem of diamond carbonization at high temperatures is solved, the wear resistance of the wear-resistant layer is improved, and the service life of the shield knife is extended.

CN118544029BActive Publication Date: 2024-10-29ZHENGZHOU RES INST OF MECHANICAL ENG CO LTD +3
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411025696.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-10-29
Estimated Expiration
2044-07-30

Smart Images

  • Figure CN118544029B_ABST
    Figure CN118544029B_ABST
Patent Text Reader

Abstract

The invention provides a wear-resistant material for a shield cutter and a preparation method thereof. The preparation method comprises S100: preparing an activation liquid; S200: mixing the activation liquid with diamond, heating, and obtaining active diamond after screening; S300: adding a solvent, a flux, and a thixotropic agent into a reaction kettle for mixing and stirring to obtain a flux paste; S400: mixing and stirring the active diamond, a nickel-based solder, and the flux paste to obtain a wear-resistant material. The technical problem solved by the invention is that in the existing preparation process of the wear-resistant material, when the temperature exceeds 800°C, the diamond is easily carbonized, thereby causing the physical properties of the diamond to decrease, so that the wear-resistant effect of the wear-resistant layer made of the wear-resistant material is poor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wear-resistant materials for cutting tools, and in particular to a wear-resistant material for shield cutting tools and a preparation method thereof. Background Art

[0002] The main function of the shield cutter is to perform cutting and excavation operations when the shield machine is excavating a tunnel. Its service life is the key to the overall excavation efficiency of the shield machine, the project progress and cost control. During the excavation process, the force state of the cutter body is complex. In addition to the main radial pressure, it is also affected by various other factors such as impact load, eccentric load of uneven soft and hard strata, eccentric wear, and severe friction of hard mineral sand and gravel in the rock and soil, resulting in strong wear. Therefore, the material used to make the shield cutter is usually selected from materials with high hardness, high wear resistance and good impact toughness.

[0003] The shield cutter is composed of alloy steel, cemented carbide and a wear-resistant layer. The wear-resistant layer is usually made by coating the wear-resistant material on the force-bearing surface of the cutter. Diamond, as the material with the highest hardness among known materials, is the preferred hard material for wear-resistant materials.

[0004] However, there is at least one of the following problems in the related art: during the preparation process of existing wear-resistant materials, when the temperature exceeds 800°C, diamond is easily carbonized, resulting in a decrease in the physical properties of diamond, making the wear-resistant layer made of the wear-resistant material have poor wear resistance. Summary of the invention

[0005] The technical problem solved by the present invention is that during the preparation process of the existing wear-resistant material, when the temperature exceeds 800°C, the diamond is easily carbonized, which leads to a decrease in the physical properties of the diamond, resulting in poor wear resistance of the wear-resistant layer made of the wear-resistant material.

[0006] In order to solve the above problems, the present invention provides a method for preparing a wear-resistant material for a shield cutter, the preparation method comprising:

[0007] S100: preparing activation solution;

[0008] S200: mixing the activation liquid with diamond, heating, and obtaining active diamond after screening;

[0009] S300: adding a solvent, a soldering flux, and a thixotropic agent into a reaction kettle, mixing and stirring, to obtain a soldering flux paste;

[0010] S400: Active diamond, nickel-based brazing filler metal and flux paste are mixed and stirred to obtain wear-resistant material.

[0011] Compared with the prior art, the technical effect achieved by adopting this technical solution is as follows: this solution improves the wear resistance of the wear-resistant material by adding active diamond as the hard phase of the wear-resistant material into the nickel-based solder.

[0012] Specifically, diamond is composed of carbon atoms tightly arranged in a tetrahedral structure, and each carbon atom is connected to the surrounding carbon atoms through strong and stable covalent bonds. Therefore, diamond has relatively stable chemical properties. However, when the temperature of traditional diamond exceeds 800°C, diamond is easy to carbonize, which reduces the physical properties of diamond and further affects the wear resistance of diamond. This scheme activates diamond by preparing an activation liquid to protect diamond from carbonization in an environment exceeding 800°C. At the same time, diamond has its own active groups to enhance the bonding force between diamond and metal and improve the connection activity and strength of diamond.

[0013] In one embodiment of the present invention, S100 specifically includes:

[0014] S110: mixing a silane coupling agent and water to perform a reaction to obtain an intermediate product;

[0015] S120: mixing the intermediate product with carboxyl boric acid and catalyst A for secondary reaction to obtain an activation solution;

[0016] The temperature of the primary reaction is 40°C to 90°C, the pressure of the primary reaction is 7MPa to 9MPa, the time of the primary reaction is 25min to 35min, the temperature of the secondary reaction is 60°C to 70°C, and the time of the secondary reaction is 1h to 1.5h.

[0017] Compared with the prior art, the technical effect achieved by adopting this technical solution is: improving the oxidation resistance of diamond and enhancing the surface activation performance of diamond.

[0018] Specifically, the silane coupling agent and water are mixed to undergo a hydrolysis reaction to generate an intermediate product carrying a silanol group (-Si—OH). The temperature of the primary reaction is controlled to be 40°C-90°C to accelerate the speed of the chemical reaction, thereby increasing the conversion rate of the primary reaction and allowing the silane coupling agent to be fully hydrolyzed. Furthermore, the present invention preferably sets the time for the primary reaction to 30 minutes and the time for the secondary reaction to 1 hour, and accurately controls the reaction time for the hydrolysis of the silane coupling agent to avoid unnecessary side reactions, thereby further increasing the conversion rate of the silane coupling agent and improving the utilization rate of the material. The pressure during the primary reaction is controlled to increase the concentration of the reactants, further accelerating the reaction rate of the primary reaction.

[0019] Furthermore, the intermediate product reacts with carboxyl boric acid under the action of catalyst A to generate an activation solution carrying both boric acid groups and silanol groups (-Si—OH). After the activation solution is mixed with diamond, the silanol groups (-Si—OH) of the activation solution react with the active hydroxyl groups on the surface of the diamond to undergo condensation reaction for adsorption and interconnection.

[0020] In one embodiment of the present invention, the chemical formula of the silane coupling agent is R—Si—X3, wherein R is an organic functional group and X is a hydrolyzable group.

[0021] Compared with the prior art, the technical effect achieved by adopting this technical solution is: improving the high-temperature oxidation resistance of diamond, while strengthening the surface activity of diamond, promoting bonding with metal materials, improving the connection strength, and making the diamond less likely to fall off.

[0022] Specifically, the chemical formula of silane coupling agent is R-Si-X3; where R is an organic functional group, such as methyl, vinyl, octenyl, amino; X is a hydrolyzable group, Si is silicon, and Si-X forms a silanol group (-Si-OH) after hydrolysis; thus, during the mixing process of active liquid and diamond, the silanol group (-Si-OH) reacts with the active hydroxyl groups on the surface of diamond particles to form hydrogen bonds and condense into -SiO-M covalent bonds (M represents the surface of diamond particles), making them adsorbed and connected. At the same time, the condensation reaction proceeds in a multi-dimensional direction, and the silanol groups (-Si-OH) of each silane molecule associate and aggregate with each other to form a three-dimensional short-chain cross-linked network structure of gel aggregates (SiO2 cross-linked polymer film) covering the surface of diamond powder particles, making the diamond surface organic and functional. Then, a SiO2 nano-gel film containing active oxygen groups is obtained on the surface of diamond. The film can be continuously and densely coated on the surface of diamond particles by relying on its own cross-linking shrinkage stress, and can evenly disperse diamonds, so that the hard phase in the wear-resistant material can be evenly distributed, avoiding the situation that diamonds are easily agglomerated in traditional preparation methods; at the same time, it can isolate the air on the surface of diamonds to form a protective layer, thereby improving the high-temperature oxidation resistance of diamonds. In addition, the boric acid active groups carried by silane are adsorbed on the surface of diamonds along with silane. Boric acid (H3BO3) decomposes into boric acid (B2O3) when heated. The generated boric acid (B2O3) forms fusible borates with metal oxides, thereby enhancing the ability to remove interface oxides, thereby enhancing the connection strength between diamonds and nickel-based solders, making diamonds less likely to fall off, and enhancing the adhesion between wear-resistant materials and diamond surfaces.

[0023] In one embodiment of the present invention, the activation solution and diamond are mixed and heated for 3 hours to 3.5 hours; and / or the activation solution and diamond are mixed and heated at a temperature of 60° C. to 80° C.

[0024] Compared with the prior art, the technical effect achieved by adopting the technical solution is as follows: the mixing time of diamond and activation liquid is increased, so as to ensure that the activation liquid can fully penetrate into the diamond lattice gap and chemically react with the diamond surface, thereby improving the activation effect of diamond. Furthermore, the preferred mixing and heating time of the activation liquid and diamond of the present invention is 3 hours, and the mixing and heating temperature range of the activation liquid and diamond is 60°C to 80°C, so as to avoid the situation that the high-temperature modified diamond breaks due to thermal cracks and thermal stress, thereby improving the thermal stability of the diamond, and further improving the wear resistance of the wear-resistant material.

[0025] In one embodiment of the present invention, the temperature for adding the solvent, flux and thixotropic agent into the reaction kettle for mixing and stirring is 90°C to 150°C; and / or the temperature for mixing and stirring the active diamond, nickel-based solder and solder paste is 15°C to 30°C; and / or the time for mixing and stirring the active diamond, nickel-based solder and solder paste is 1.5h to 2.5h; and / or the vacuum degree for mixing and stirring the active diamond, nickel-based solder and solder paste is -80KPa to -100KPa.

[0026] Compared with the prior art, the technical effect achieved by adopting this technical solution is: the wear resistance of the wear-resistant material is further improved, thereby extending the service life of the shield cutter.

[0027] Preferably, the time for mixing and stirring the active diamond, nickel-based solder and solder paste is 2 hours, and the vacuum degree for mixing and stirring the active diamond, nickel-based solder and solder paste is -90 KPa.

[0028] In one embodiment of the present invention, the preparation method further comprises:

[0029] S500: The wear-resistant material is evenly applied to the working surface of the shield cutter and dried, and the thickness of the wear-resistant material evenly applied to the working surface is 5mm to 10mm;

[0030] S600: After the shield cutter coated with the wear-resistant material is dried, gradient heating is performed;

[0031] S700: After the wear-resistant material is combined with the shield cutter, gradient cooling is performed to reduce the temperature of the wear-resistant material and the shield cutter to room temperature to obtain a wear-resistant layer.

[0032] Compared with the prior art, the technical effect achieved by adopting this technical solution is: the wear resistance of the wear-resistant layer is improved.

[0033] Preferably, the thickness of the wear-resistant material uniformly coated on the working surface is 5 mm to 8 mm.

[0034] Specifically, in the prior art, the wear-resistant layer of the shield cutter is mainly formed by surfacing a layer of wear-resistant layer on the surface of an alloy steel substrate to prevent damage to the shield cutter due to wear during use. However, due to the rapid heating and cooling during the surfacing process, thermal stress is generated in the wear-resistant area, resulting in deformation and cracks in the wear-resistant layer, and the wear-resistant layer at the crack is easily oxidized, which in turn affects the wear-resistant effect of the wear-resistant layer.

[0035] Furthermore, the present solution forms a wear-resistant layer by coating the wear-resistant material on the shield cutter and then combining the wear-resistant material and the shield cutter using gradient heating and gradient cooling, thereby avoiding thermal stress in the wear-resistant area, which may cause deformation and cracks in the wear-resistant layer and make the wear-resistant layer easily oxidized, thereby improving the wear resistance of the wear-resistant layer.

[0036] In one embodiment of the present invention, the drying time is 10 min to 20 min, and the drying temperature is 100°C; and / or the target temperature of the gradient heating is 1010°C to 1177°C; and / or the gradient heating time is 35 min to 50 min; and / or the stay time after the gradient heating is completed is 3 min to 5 min; and / or the gradient cooling time is 1 h to 2 h.

[0037] Compared with the prior art, the technical effect achieved by adopting this technical solution is: the wear resistance of the wear-resistant layer is further improved.

[0038] Furthermore, the preferred drying time of the present invention is 15 minutes, the drying temperature is 100°C, the target temperature of the gradient heating is 1010°C to 1177°C; the gradient heating time is 40 minutes; the stay time is 3 minutes after the gradient heating is completed; and the gradient cooling time is 1.5 hours.

[0039] The present invention also provides a wear-resistant material for a shield cutter, the wear-resistant material is made by the preparation method described in any of the above technical solutions, and the wear-resistant material comprises 2 to 8 parts by mass of active diamond micropowder; 4 to 10 parts by mass of active nanodiamond; 2 to 6 parts by mass of solvent; 2 to 4 parts by mass of thixotropic agent; 1 to 5 parts by mass of soldering flux; 81 to 93 parts by mass of nickel-based solder; wherein the nickel-based solder is selected from Ni 60 、N i60 M.Ni 62 、Ni 45 , BNi-2 nickel-based alloy.

[0040] Compared with the existing technology, the technical effect achieved by adopting this technical solution is: the wear resistance of the wear-resistant material is improved, thereby extending the service life of the shield cutter.

[0041] Specifically, the wear-resistant material includes composite diamond particles composed of diamond micropowder and nanodiamonds, which increases the diamond content on the wear surface of the wear-resistant layer, and the exposure of nanodiamonds fills the gaps in the diamond micropowder, protecting the nickel-based brazing alloy matrix. Furthermore, after adding nanodiamonds, the diamonds on the coating surface tend to be saturated, increasing the proportion of diamonds per unit area, improving the wear resistance of the shield cutter, and thus extending the service life of the shield cutter.

[0042] In one embodiment of the present invention, the nickel-based brazing filler metal is a powder material, and the particle size of the powder material is 200-300 mesh; and / or the particle size of the active diamond micropowder is 30 μm-60 μm; and / or the particle size of the active nanodiamond is 100 nm-200 nm.

[0043] Compared with the existing technology, the technical effect achieved by adopting this technical solution is: the wear resistance of the wear-resistant material is further improved, thereby extending the service life of the shield cutter.

[0044] In one embodiment of the present invention, the solvent is selected from one or more of glycerol, fatty alcohol, and octanol; and / or the thixotropic agent is selected from one or more of hydrogenated castor oil and polyamide wax; and / or the flux is selected from one or more of borax, potassium fluoride, calcium fluoride, and sodium fluoride.

[0045] Compared with the prior art, the technical effect achieved by adopting the technical scheme is as follows: borax, potassium fluoride, calcium fluoride and sodium fluoride are selected as fluxes to remove oxides on the welding surface, thereby promoting the bonding between diamond and metal; the thixotropic agent is selected from one or more of hydrogenated castor oil and polyamide wax, and the solvent is selected from one or more of propylene glycol, fatty alcohol and octanol to prevent the sedimentation of diamond and metal powder, thereby avoiding the liquid-solid separation phenomenon of the wear-resistant material.

[0046] After adopting the technical solution of the present invention, the following technical effects can be achieved: the present invention activates diamond by preparing an activation solution to protect the diamond from being carbonized in an environment exceeding 800°C, and at the same time enables the diamond to have its own active groups, promotes the bonding of diamond with nickel-based solder, protects the wear resistance of diamond, and thus improves the wear resistance of the wear-resistant layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings to be used in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative work.

[0048] Figure 1Reaction formula 1 provided by the present invention;

[0049] Figure 2 Reaction formula 2 provided by the present invention;

[0050] Figure 3 Reaction formula 3 provided by the present invention;

[0051] Figure 4 A mirror image of the anti-oxidation gel film on the surface of the diamond after wear provided by the present invention;

[0052] Figure 5 A mirror image of the wear-resistant layer provided in Example 1 of the present invention;

[0053] Figure 6 This is a mirror image of the wear-resistant layer provided in Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0054] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0055] The present invention provides a method for preparing a wear-resistant material for a shield cutter, the preparation method comprising:

[0056] S100: preparing activation solution;

[0057] S200: mixing the activation liquid with diamond, heating, and obtaining active diamond after screening;

[0058] S300: adding a solvent, a soldering flux, and a thixotropic agent into a reaction kettle, mixing and stirring, to obtain a soldering flux paste;

[0059] S400: Active diamond, nickel-based brazing filler metal and flux paste are mixed and stirred to obtain wear-resistant material.

[0060] Specifically, by adding active diamond as the hard phase of the wear-resistant material to the nickel-based brazing filler metal, the wear resistance of the wear-resistant material is improved. Diamond is composed of carbon atoms tightly arranged in a tetrahedral structure, and each carbon atom is connected to the surrounding carbon atoms through a strong and stable covalent bond. Therefore, diamond has relatively stable chemical properties, but when the temperature of traditional diamond exceeds 800°C, diamond is easy to carbonize, which reduces the physical properties of diamond and affects the wear resistance of diamond. This scheme activates diamond by preparing an activation liquid to protect diamond from carbonization in an environment exceeding 800°C. At the same time, the diamond has its own active groups to enhance the bonding force between diamond and metal, thereby improving the connection activity and strength of diamond.

[0061] Furthermore, S100 specifically includes:

[0062] S110: mixing a silane coupling agent and water to perform a reaction to obtain an intermediate product;

[0063] S120: mixing the intermediate product with carboxyl boric acid and catalyst A for secondary reaction to obtain an activation solution;

[0064] The temperature of the first reaction is 40℃~90℃, the pressure of the first reaction is 7MPa~9MPa, the time of the first reaction is 25min~35min, the temperature of the second reaction is 60℃~70℃, and the time of the second reaction is 1h~1.5h. This improves the oxidation resistance of diamond and enhances the surface activation performance of diamond.

[0065] For example, the temperature of the primary reaction is 40°C to 90°C, the pressure of the primary reaction is 7MPa to 9MPa, the time of the primary reaction is 30min, the temperature of the secondary reaction is 60°C to 70°C, and the time of the secondary reaction is 1h.

[0066] It should be noted that the pressure of the secondary reaction is the normal pressure of the experimental environment, so no further explanation is given here.

[0067] For example, if Figure 1 As shown, it is reaction formula 1 of the hydrolysis process of the silane coupling agent provided by the present invention. The silane coupling agent used in the embodiment of the present invention is vinyltrimethoxysilane. Vinyltrimethoxysilane and water are mixed to undergo a hydrolysis reaction. After the hydrolysis of vinyltrimethoxysilane, an intermediate product carrying both a silanol group (-Si—OH) and ethyl alcohol is generated.

[0068] For example again, the silane coupling agent of the present invention may also be vinyl triethoxysilane, and its reaction principle is the same as that of vinyl trimethoxysilane, which will not be described in detail here.

[0069] Specifically, by controlling the temperature of the primary reaction to 40°C to 90°C to speed up the chemical reaction, the conversion rate of the primary reaction is increased, so that the silane coupling agent can be fully hydrolyzed; the time of the primary reaction is controlled to 30 minutes, and the reaction time of the hydrolysis of the silane coupling agent is accurately controlled to avoid unnecessary side reactions, thereby further improving the conversion rate of the silane coupling agent and improving the utilization rate of the material; the pressure during the primary reaction is controlled to increase the concentration of the reactants, further accelerating the reaction rate of the primary reaction.

[0070] Furthermore, the intermediate product reacts with carboxyl boric acid under the action of catalyst A to generate an activation solution carrying both boric acid groups and silanol groups (-Si—OH). After the activation solution is mixed with diamond, the silanol groups (-Si—OH) of the activation solution react with the active hydroxyl groups on the surface of the diamond to undergo condensation reaction for adsorption and interconnection.

[0071] For example, the carboxyl boronic acid provided in the embodiment of the present invention is (2,5-dicarboxyphenyl)boric acid, such as Figure 2 As shown, it is a reaction formula for the reaction of the intermediate product provided in an embodiment of the present invention with (2,5-dicarboxyphenyl)boric acid, wherein the hydroxyl group (-OH) of ethyl alcohol in the intermediate product and the carboxyl group (-COOH) of (2,5-dicarboxyphenyl)boric acid undergo an esterification reaction under the action of catalyst A to generate an activation solution carrying both a boric acid group and a silanol group (-Si—OH). After the activation solution is mixed with diamond, the silanol group (-Si—OH) of the activation solution undergoes a condensation reaction with the active hydroxyl group on the surface of the diamond to perform adsorption interconnection.

[0072] Preferably, the catalyst A of the present invention is selected from one or more of zinc oxide and stannous chloride to accelerate the esterification reaction between the hydroxyl group (-OH) of ethyl alcohol in the intermediate product and the carboxyl group (-COOH) of (2,5-dicarboxyphenyl)boric acid.

[0073] Furthermore, the chemical formula of the silane coupling agent is R-Si-X3, where R is an organic functional group and X is a hydrolyzable group. This improves the high-temperature oxidation resistance of diamond and enhances the connection strength between diamond and nickel-based solder, making it difficult for diamond to fall off.

[0074] Specifically, if Figure 3 As shown, the general chemical formula of silane coupling agent is R—Si—X3; wherein R is an organic functional group, such as methyl, vinyl, octenyl, amino; Si is silicon, X is a hydrolyzable group, and Si—X forms a silanol group (-Si—OH) after hydrolysis; thus, during the mixing process of active liquid and diamond, the silanol group (-Si—OH) reacts with the hydroxyl group on the surface of the diamond particle to form a hydrogen bond and condense into a -SiO—M covalent bond (M represents the surface of the diamond particle) for adsorption connection. At the same time, the condensation reaction proceeds in a multi-dimensional direction, and the silanol groups (-Si—OH) of each silane molecule associate and aggregate with each other to form a three-dimensional short-chain cross-linked network structure of gel aggregates (SiO2 cross-linked polymer film) covering the surface of the diamond powder particles, making the diamond surface organic and functionalized, such as Figure 4As shown, it is the anti-oxidation gel film on the surface of diamond after wear provided by the present invention. Then, a SiO2 nano-gel film containing active oxygen groups is obtained on the surface of diamond. The coating can be continuously and densely coated on the surface of diamond particles by relying on its own cross-linking shrinkage stress, and can evenly disperse diamonds, so that the hard phase in the wear-resistant material can be evenly distributed, avoiding the diamond agglomeration that is easy to occur in the traditional preparation method; at the same time, it can isolate the air on the surface of diamond to form a protective layer, thereby improving the high-temperature oxidation resistance of diamond. In addition, the boric acid active group carried in the activation solution, boric acid (H3BO3) decomposes into boric acid (B2O3) when heated, and the generated boric acid (B2O3) forms a fusible borate with the metal oxide, thereby enhancing the ability to remove the interface oxide, and then enhancing the connection strength between the diamond and the nickel-based solder, making the diamond not easy to fall off, and enhancing the adhesion between the wear-resistant material and the diamond surface.

[0075] Furthermore, the time for mixing the activation liquid with the diamond and heating is 3 hours; and / or the temperature for mixing the activation liquid with the diamond and heating is 60°C to 80°C. The time for mixing the diamond with the activation liquid is increased to ensure that the activation liquid can fully penetrate into the diamond lattice gap and react chemically with the diamond surface, thereby improving the activation effect of the diamond. Furthermore, the temperature range for mixing the activation liquid with the diamond and heating is 60°C to 80°C, which avoids the diamond breakage caused by thermal cracks and thermal stress of the high-temperature modified diamond, thereby improving the thermal stability of the diamond, and then improving the wear resistance of the wear-resistant material.

[0076] Furthermore, the temperature for mixing and stirring the solvent, solder flux and thixotropic agent in the reaction kettle is 90°C to 150°C; and / or the temperature for mixing and stirring the active diamond, nickel-based solder and solder paste is 15°C to 30°C; and / or the time for mixing and stirring the active diamond, nickel-based solder and solder paste is 1.5h to 2.5h; and / or the vacuum degree for mixing and stirring the active diamond, nickel-based solder and solder paste is -80KPa to -100KPa. The wear resistance of the wear-resistant material is further improved, thereby extending the service life of the shield cutter.

[0077] Preferably, the time for mixing and stirring the active diamond, nickel-based solder and solder paste is 2 hours, and the vacuum degree for mixing and stirring the active diamond, nickel-based solder and solder paste is -90 KPa.

[0078] Furthermore, the preparation method also includes:

[0079] S500: The wear-resistant material is evenly applied to the working surface of the shield cutter and dried, and the thickness of the wear-resistant material evenly applied to the working surface is 5mm to 10mm;

[0080] S600: After the shield cutter coated with the wear-resistant material is dried, gradient heating is performed;

[0081] S700: After the wear-resistant material is combined with the shield cutter, the temperature is gradually reduced to reduce the temperature of the wear-resistant material and the shield cutter to room temperature to obtain a wear-resistant layer. The wear-resistant effect of the wear-resistant layer is improved.

[0082] Preferably, the thickness of the wear-resistant material uniformly coated on the working surface is 5 mm to 8 mm.

[0083] Specifically, in the prior art, the wear-resistant layer of the shield cutter is mainly welded on the surface of the alloy steel substrate to prevent damage to the shield cutter due to wear during use. However, due to the rapid heating and cooling process during the welding process, thermal stress is generated in the wear-resistant area, which causes deformation and cracks in the wear-resistant layer, making the wear-resistant layer easily oxidized, thereby affecting the wear-resistant effect of the wear-resistant layer.

[0084] Furthermore, the present solution forms a wear-resistant layer by coating the wear-resistant material on the shield cutter and then combining the wear-resistant material and the shield cutter using gradient heating and gradient cooling, thereby avoiding thermal stress in the wear-resistant area, which may cause deformation and cracks in the wear-resistant layer and make the wear-resistant layer easily oxidized, thereby improving the wear resistance of the wear-resistant layer.

[0085] Furthermore, the drying time is 10 min to 20 min, and the drying temperature is 100°C; and / or the target temperature of the gradient heating is 1010°C to 1177°C; and / or the gradient heating time is 35 min to 50 min; and / or the stay time after the gradient heating is completed is 3 min to 5 min; and / or the gradient cooling time is 1 h to 2 h.

[0086] Specifically, the preferred drying time of the present invention is 15 minutes, the drying temperature is 100°C, the target temperature of the gradient heating is 1010°C to 1177°C, the gradient heating time is 40 minutes, the stay time is 3 minutes after the gradient heating is completed, and the gradient cooling time is 1.5 hours, which further improves the wear resistance of the wear-resistant layer.

[0087] The present invention also provides a wear-resistant material for a shield cutter, the wear-resistant material is made by the preparation method described in any of the above technical solutions, and the wear-resistant material comprises 2 to 8 parts by mass of active diamond micropowder; 4 to 10 parts by mass of active nanodiamond; 2 to 6 parts by mass of solvent; 2 to 4 parts by mass of thixotropic agent; 1 to 5 parts by mass of soldering flux; 81 to 93 parts by mass of nickel-based solder; wherein the nickel-based solder is selected from Ni 60 、N i60 M.Ni 62 、Ni45 At least one of BNi-2 nickel-based alloys. The wear resistance of the wear-resistant material is improved, thereby extending the service life of the shield cutter.

[0088] Specifically, the wear-resistant material includes composite diamond particles composed of diamond micropowder and nanodiamonds, which increases the diamond content on the wear surface of the wear-resistant layer, and the exposure of nanodiamonds fills the gaps in the diamond micropowder, protecting the nickel-based brazing alloy matrix. Furthermore, after adding nanodiamonds, the diamonds on the coating surface tend to be saturated, increasing the proportion of diamonds per unit area, improving the wear resistance of the shield cutter, and thus extending the service life of the shield cutter.

[0089] Furthermore, the nickel-based brazing filler metal is a powder material, and the particle size of the powder material is 200-300 mesh; and / or the particle size of the active diamond micropowder is 30 μm-60 μm; and / or the particle size of the active nano-diamond is 100 nm-200 nm. This further improves the wear resistance of the wear-resistant material, thereby extending the service life of the shield cutter.

[0090] Furthermore, the solvent is selected from one or more of glycerol, fatty alcohol, and octanol; and / or the thixotropic agent is selected from one or more of hydrogenated castor oil and polyamide wax; and / or the flux is selected from one or more of borax, potassium fluoride, calcium fluoride, and sodium fluoride.

[0091] Specifically, borax, potassium fluoride, calcium fluoride and sodium fluoride are selected as flux to remove oxides on the welding surface, thereby promoting the bonding between diamond and metal; the thixotropic agent is selected from one or more of hydrogenated castor oil and polyamide wax, and the solvent is selected from one or more of glycerol, fatty alcohol and octanol to prevent the sedimentation of diamond and metal powder, thereby avoiding the liquid-solid separation of the wear-resistant material.

[0092] In one embodiment of the present invention, the preparation process of activated diamond is as follows:

[0093] Add 85 to 95 parts by mass of vinyl trimethoxysilane and 5 to 15 parts by mass of distilled water into a reactor, heat to 40 to 90°C, and react for 30 minutes under a pressure of 7 MPa to 9 MPa to obtain an intermediate product. Then, mix the intermediate product with (2,5-dicarboxyphenyl)boric acid and catalyst A at a temperature of 60 to 70°C for esterification to obtain an activation solution. Finally, stir and mix the activation solution with diamond, heat to 60 to 80°C and stir for 3 hours, and sieve to obtain active diamond.

[0094] [Example 1]

[0095] This embodiment provides a shield cutter, and the specific operation is as follows.

[0096] Step 1: Calculate by mass, weigh 3 parts by mass of propylene glycol, 1 part by mass of polyamide wax, 1 part by mass of borax, 1 part by mass of potassium fluoride, and 1 part by mass of sodium fluoride, put them into a reactor, stir and mix them evenly at 90°C to 150°C to obtain soldering paste; cool to 15°C to 30°C, weigh 2 parts by mass of modified active diamond micropowder and 4 parts by mass of nano-active diamond, and 87 parts by mass of BNi-2 solder powder, add them into the reactor, stir at 15°C to 30°C for 2 hours, and obtain a wear-resistant material.

[0097] Step 2: Evenly apply the prepared wear-resistant material to the working surface of the shield cutter, and control the thickness of the coating layer to 5 mm, put it into the oven, adjust the oven temperature to 100°C and dry it for 15 minutes.

[0098] Step 3: Place the shield cutter coated with wear-resistant material after drying on a high-temperature resistant bracket for fixation, heat it to 1010℃~1177℃ through induction heating, perform gradient heating for 40 minutes, stay for 3 minutes after completing the gradient heating, and perform gradient cooling to reduce the temperature of the wear-resistant material and the shield cutter to room temperature.

[0099] [Example 2]

[0100] This embodiment provides a shield cutter, and its preparation method refers to that of Embodiment 1, except that, in step 1, the active diamond powder is 3 parts by mass, the nano-active diamond is 5 parts by mass, and the BNi-2 solder powder is 85 parts by mass.

[0101] [Example 3]

[0102] This embodiment provides a shield cutter, and its preparation method refers to that of Embodiment 1, except that, in step one, the active diamond micropowder is 4 parts by mass, the nano-active diamond is 6 parts by mass, the BNi-2 solder powder is 82 parts by mass, and the propylene glycol is 4 parts by mass.

[0103] [Example 4]

[0104] This embodiment provides a shield cutter, and its preparation method refers to that of Embodiment 1, except that, in step one, the active diamond micropowder is 5 parts by mass, the nano-active diamond is 7 parts by mass, the BNi-2 solder powder is 80 parts by mass, and the propylene glycol is 4 parts by mass.

[0105] [Comparative Example 1]

[0106] This comparative example provides a shield cutter, and its preparation method refers to Example 1, except that the preparation materials in step one are: 2 parts by mass of ordinary diamond powder (30μm~40μm), 4 parts by mass of nano diamond (100nm~150nm), 3 parts by mass of propylene glycol, 1 part by mass of polyamide wax, 1 part by mass of borax, 1 part by mass of potassium fluoride, 1 part by mass of sodium fluoride, and 87 parts by mass of BNi-2 solder powder (200 mesh~300 mesh).

[0107] [Comparative Example 2]

[0108] This comparative example provides a shield cutter, and its preparation method refers to Example 1, except that the preparation materials in step one are: 6 parts by mass (30 μm to 40 μm) of ordinary diamond powder, 3 parts by mass of propylene glycol, 1 part by mass of polyamide wax, 1 part by mass of borax, 1 part by mass of potassium fluoride, 1 part by mass of sodium fluoride, and 87 parts by mass of BNi-2 solder powder (200 mesh to 300 mesh).

[0109] [Comparative Example 3]

[0110] This comparative example provides a shield cutter, the difference being that the working surface of the shield cutter is not coated with wear-resistant material.

[0111] In order to compare and illustrate the difference in performance of the wear-resistant layer between the embodiment of the present invention and the comparative example, a shield cutter base body with a stress-bearing surface of 210 mm in length, 110 mm in width, and 220 mm in height, all of which were made of 42CrMo steel, was selected.

[0112] Wear tests were conducted using shield blades of Examples 1-4 and Comparative Examples 1-3 as test objects. The wear tests of the present invention were all conducted on the same wear test device. The wear test used clay layer slurry commonly used in shield blade engineering. The clay layer slurry was placed in a working tank. The shield blade was mounted on a drive shaft, which was driven by a hydraulic motor to achieve rotary motion. The speed of the drive shaft was 10 r / min. The wear test lasted for 6 hours. The wear amount of the shield blade after the wear test was tested, and the results are shown in Table 1.

[0113] Table 1 Wear parameters and analysis results of examples and comparative examples

[0114]

[0115] Refer to Table 1 and Figure 6 , Comparative Example 1 uses a wear-resistant layer prepared with ordinary diamond. From Table 1, it can be seen that after the wear test of the shield cutter in Comparative Example 1, the wear amount of the shield cutter is measured to be 35.5 / g, indicating that the diamond is burned and carbonized; combined with Figure 6 It can be seen that the diamond in the wear-resistant layer is obviously carbonized. Figure 5In Example 1, the wear-resistant layer is prepared by using diamond activated by an activation liquid. From Table 1, it can be seen that after the wear test of the shield cutter in Example 1, the wear loss of the shield cutter is measured to be 19.4 / g, indicating that the coating layer is intact and the diamond is not burned; combined with Figure 5 It can be seen that no carbide is found in the diamond in the prepared wear-resistant layer.

[0116] By comparing Example 1 and Comparative Example 1, it can be concluded that the activated diamond is not carbonized in an environment exceeding 800°C, so that the wear resistance of the diamond is increased, thereby increasing the wear resistance of the wear-resistant layer, and further improving the wear resistance of the shield cutter.

[0117] Furthermore, the comparison principle between Examples 2-4 and Comparative Examples 2-3 is the same as the comparison principle between the above-mentioned Example 1 and Comparative Example 1, and therefore, it will not be repeated here.

[0118] In this specification, the writing method of "S100", "S200" and "S300" is to facilitate the description of the embodiments of the present invention. The present invention can also be implemented in other ways different from those described herein. Therefore, the protection scope of the present invention is not limited by the order of the specific embodiments of the above writing method.

[0119] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.

Claims

1. A method for preparing a wear-resistant material for a shield cutter, characterized in that: The preparation method comprises: S100: preparing activation solution; S200: mixing the activation solution with diamond, heating, and obtaining active diamond after screening; S300: adding a solvent, a soldering flux, and a thixotropic agent into a reaction kettle, mixing and stirring, to obtain a soldering flux paste; S400: mixing and stirring the active diamond, nickel-based brazing filler metal and the soldering paste to obtain the wear-resistant material; S500: evenly coating the wear-resistant material on the working surface of the shield cutter and performing a drying process, wherein the thickness of the wear-resistant material evenly coated on the working surface is 5 mm to 10 mm; S600: performing gradient heating on the shield cutter coated with the wear-resistant material after the drying process is completed; S700: After the wear-resistant material is combined with the shield cutter, a gradient temperature reduction is performed to reduce the temperature of the wear-resistant material and the shield cutter to room temperature to obtain a wear-resistant layer; The S100 specifically includes: S110: mixing a silane coupling agent and water to perform a reaction to obtain an intermediate product; S120: mixing the intermediate product with carboxyl boric acid and catalyst A to perform a secondary reaction to obtain the activation solution; The temperature of the primary reaction is 40°C to 90°C, the pressure of the primary reaction is 7MPa to 9MPa, the time of the primary reaction is 25min to 35min, the temperature of the secondary reaction is 60°C to 70°C, and the time of the secondary reaction is 1h to 1.5h.

2. The preparation method according to claim 1, characterized in that: The chemical formula of the silane coupling agent is R—Si—X3; Wherein, R is an organic functional group, Si is silicon, and X is a hydrolyzable group.

3. The preparation method according to claim 1, characterized in that: The activation solution and the diamond are mixed and heated for 3 hours to 3.5 hours; and / or The activation solution and the diamond are mixed and heated at a temperature of 60°C to 80°C.

4. The preparation method according to claim 1, characterized in that: The temperature of adding the solvent, soldering flux and thixotropic agent into the reaction kettle for mixing and stirring is 90° C. to 150° C.; and / or The temperature for mixing and stirring the active diamond, nickel-based solder and the soldering paste is 15° C. to 30° C.; and / or The time for mixing and stirring the active diamond, nickel-based solder and the soldering paste is 1.5 hours to 2.5 hours; and / or The vacuum degree of the mixing and stirring of the active diamond, nickel-based solder and the solder paste is -80KPa to -100KPa.

5. The preparation method according to claim 1, characterized in that: The drying time is 10 to 20 minutes, and the drying temperature is 100° C.; and / or The target temperature of the gradient heating is 1010°C to 1177°C; and / or The gradient heating time is 35 min to 50 min; and / or After completing the gradient heating, the heating is stopped for 3 to 5 minutes; and / or The time of the gradient cooling is 1 h to 2 h.

6. A wear-resistant material for a shield cutter, characterized in that: The wear-resistant material is made by the preparation method according to any one of claims 1 to 5, and the wear-resistant material comprises: 2 to 8 parts by mass of active diamond powder; 4 to 10 parts by mass of active nanodiamond; 2 to 6 parts by mass of solvent; 2 to 4 parts by mass of thixotropic agent; 1 to 5 parts by mass of flux; 81 to 93 parts by mass of nickel-based solder; Wherein, the nickel-based brazing filler metal is selected from Ni 60 、N i60 M.Ni 62 、Ni 45 , BNi-2 nickel-based alloy.

7. The wear-resistant material according to claim 6, characterized in that: The nickel-based solder is a powder material, and the particle size of the powder material is 200-300 mesh; and / or The particle size of the active diamond powder is 30 μm to 60 μm; and / or The particle size of the active nano-diamond is 100 nm-200 nm.

8. The wear-resistant material according to claim 6, characterized in that: The solvent is selected from one or more of glycerol, fatty alcohol, and octanol; and / or The thixotropic agent is selected from one or more of hydrogenated castor oil and polyamide wax; and / or The soldering flux is selected from one or more of borax, potassium fluoride, calcium fluoride and sodium fluoride.

Citation Information

Patent Citations

  • Diamond flux-cored wire for additive manufacturing and preparation method of diamond flux-cored wire

    CN117300430A