A method for recovering ferrophosphorus from lithium extraction tailings

Through ball milling treatment and segmented pickling and leaching technology, the problem of low recovery rate of phosphorus and iron in lithium extraction tailings is solved, efficient and low-cost resource recovery is achieved, and resource utilization reaches battery-level standards.

CN118545689BActive Publication Date: 2024-10-29SHENZHEN GALAXY ENVIRONMENT CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411000854.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-10-29
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

In the existing technology, the recovery rate of phosphorus and iron in the lithium extraction tailings is low, and the purity of the obtained resources cannot reach battery-grade standards. There are high energy consumption, high cost, and pollution problems.

Method used

After ball milling, segmented pickling and segmented leaching are performed. By controlling the dosage of acid and surfactant, impurity elements are removed, the extraction efficiency of phosphorus and iron is improved, the acidity and alkali dosage are reduced, and battery-grade ferric phosphate dihydrate is synthesized. .

Benefits of technology

It achieves efficient extraction of phosphorus and iron from lithium extraction tailings, reduces production costs and environmental pollution, improves resource recovery rate, and reaches battery-level standards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118545689B_ABST
    Figure CN118545689B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of recycling and utilization of new energy materials, and discloses a method for recovering phosphorus iron from lithium extraction tailings. The method comprises the following steps: carrying out ball milling treatment on the lithium extraction tailings; adding an acid solution and a surfactant for pickling; adding an acid solution and a reducing agent for leaching; adding a reducing agent, then adding a impurity removing agent, and filtering to obtain an impurity removing solution; adding an oxidizing agent to completely oxidize Fe<supgt;2+< / supgt; in the impurity removing solution to obtain solution A; adding a phosphorus-containing solution to adjust the molar ratio of iron to phosphorus in solution A to obtain solution B; adding an alkali to adjust the pH value of solution B to be acidic, reacting, and performing solid-liquid separation to obtain filter cake A; adding water to filter cake A for aging, and performing solid-liquid separation to obtain filter cake B; washing filter cake B and then drying to obtain battery-grade iron phosphate dihydrate, wherein the surfactant is sodium dodecyl sulfate; and the impurity removing agent is a fluoride. Through the mutual cooperation of each process, the method has a high extraction rate of phosphorus iron, and the synthesized iron phosphate dihydrate meets the battery-grade standard.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of recycling and utilizing new energy materials, and in particular relates to a method for recycling ferrophosphorus in lithium extraction tailings. Background Art

[0002] Lithium iron phosphate is widely used due to its good cycle performance, high specific capacity and energy density. Currently, the main method for recycling lithium iron phosphate in industrial production is hydrometallurgy, and the products are mainly lithium salt solutions and battery-grade lithium carbonate. However, current industrial technology only focuses on the extraction and recovery of lithium from lithium iron phosphate, and the tailings produced after lithium extraction cannot be efficiently utilized. Due to the presence of other elements besides iron and phosphorus in the lithium extraction tailings, and the variety of these elements and low net content, the recovery rate of iron and phosphorus is not high. Faced with the current dilemma of lithium battery recycling, in order to improve the economic and social benefits of lithium battery recycling, finding a suitable method to recycle large amounts of lithium extraction tailings can not only reduce pollution but also promote the recycling of resources.

[0003] The main component of lithium extraction tailings is iron phosphate, and it also contains some impurity elements, such as aluminum, copper and other metal elements.

[0004] Existing methods for recovering phosphorus and iron from lithium extraction tailings include direct acid dissolution and roasting-acid dissolution. Direct acid dissolution suffers from high acid consumption, large equipment investment, and difficulty recycling the acid medium. The roasting-acid dissolution process also requires long roasting and acid dissolution times, and the residue after acid dissolution is difficult to handle.

[0005] Moreover, the purity of phosphorus and iron resources recovered by existing methods is relatively low and cannot reach battery grade levels.

[0006] Therefore, it is urgent to develop an extraction method with low energy consumption, low cost, and high phosphorus and iron recovery rate to achieve resource utilization, harmlessness, and reduced disposal of lithium extraction tailings. The phosphorus and iron resources obtained should be of battery-grade quality. Summary of the Invention

[0007] The present invention aims to address at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention proposes a method for recovering ferrophosphorus from lithium extraction tailings. The method can efficiently extract phosphorus and iron from the lithium extraction tailings and synthesize battery-grade ferric phosphate dihydrate. The method involves ball milling the lithium extraction tailings to effectively expose encapsulated impurity elements and improve impurity removal efficiency. The tailings are then subjected to staged acid washing. By controlling the amount of acid and surfactant, impurities (primarily aluminum) in the tailings are partially or completely dissolved, reducing subsequent impurity removal costs and minimizing ferrophosphorus and ferrophosphorus losses. Staged leaching is then performed, controlling the amount of acid to efficiently extract the ferrophosphorus and ferrophosphorus from the tailings, reduce the acidity of the leachate, and reduce the amount of alkali required in the subsequent synthesis process. The method has the advantages of low energy consumption, no pollution, simple process, easy process control, and good economic benefits.

[0008] In order to achieve the above object, the present invention adopts the following technical solutions:

[0009] A method for recovering ferrophosphorus from lithium extraction tailings comprises the following steps:

[0010] (1) ball milling the lithium extraction tailings to obtain lithium extraction tailings powder;

[0011] (2) adding an acid solution and a surfactant to the lithium extraction tailings powder for pickling to obtain pickled residue;

[0012] (3) adding acid solution and reducing agent to the pickling residue for leaching to obtain leached residue and leaching solution containing phosphorus and iron elements;

[0013] (4) adding a reducing agent to the leachate containing phosphorus and iron elements, and then adding an impurity remover, and filtering to obtain an impurity-removed liquid;

[0014] (5) Add an oxidant to the impurity removal solution to make Fe 2+ After complete oxidation, solution A is obtained;

[0015] (6) adding a phosphorus-containing solution to the solution A and adjusting the molar ratio of iron to phosphorus in the solution A to obtain a solution B;

[0016] (7) adding alkali to adjust the pH value of solution B to acidic, reacting, and then separating the solid and liquid to obtain filter cake A;

[0017] (8) adding water to the filter cake A for aging, and then performing solid-liquid separation to obtain filter cake B;

[0018] (9) Washing filter cake B and drying it to obtain battery-grade ferric phosphate dihydrate;

[0019] The surfactant is sodium lauryl sulfate;

[0020] The impurity remover is fluoride.

[0021] Preferably, the pickling is staged pickling, and the leaching is staged leaching.

[0022] Preferably, the method comprises the following steps:

[0023] (1) ball milling the lithium extraction tailings to obtain lithium extraction tailings powder;

[0024] (2) adding acid solution and surfactant to the lithium extraction tailings powder for segmented pickling to obtain pickling residue;

[0025] (3) adding acid solution and reducing agent to the pickling residue for staged leaching to obtain leached residue and leaching solution containing phosphorus and iron elements;

[0026] (4) adding a reducing agent to the leachate containing phosphorus and iron elements, and then adding an impurity remover, and filtering to obtain a de-impurity liquid;

[0027] (5) Add an oxidant to the impurity removal solution to make Fe 2+ After complete oxidation, solution A is obtained;

[0028] (6) adding a phosphorus-containing solution to the solution A to adjust the molar ratio of iron to phosphorus in the solution A to 1:(1-1.5) to obtain a solution B;

[0029] (7) Add ammonia water to adjust the pH value of solution B to acidic, react at 40-100°C for 0.1-3h, and then separate the solid and liquid to obtain filter cake A;

[0030] (8) Add filter cake A to water, age it at 40-100°C for 0.1-3h, and then separate the solid and liquid to obtain filter cake B;

[0031] (9) After washing filter cake B, it is dried to obtain battery-grade iron phosphate dihydrate.

[0032] The valuable elements in the lithium extraction tailings used in the present invention are mainly phosphorus and iron, which exist in the form of iron phosphate, and the impurity elements are mainly aluminum. First, through ball milling treatment, the encapsulated impurity elements are effectively exposed, thereby improving the efficiency of impurity removal. Then, pickling is performed, and the amount of acid and surfactant used is controlled to partially or completely dissolve the impurities (mainly aluminum) in the lithium extraction tailings, thereby reducing the subsequent impurity removal requirements and reducing the loss of phosphorus and iron elements. Finally, through staged leaching, the phosphorus and iron elements in the lithium extraction tailings are efficiently extracted, the acidity of the leachate is reduced, the amount of alkali used in the subsequent synthesis process is reduced, and the production cost is reduced. By adopting the above method, phosphorus and iron elements in the lithium extraction tailings can be efficiently extracted, and battery-grade iron phosphate dihydrate can be synthesized, thereby achieving harmless, resource-based, and reduced-volume disposal of the lithium extraction tailings.

[0033] Preferably, in step (1), the Fe content in the lithium extraction tailings is 15-45wt%, preferably 15-35wt%, for example, 15wt%, 20wt%, 25wt%, 30wt%, 35wt%, 40wt%, etc.

[0034] Preferably, in step (1), the content of P in the lithium extraction tailings is 8-35 wt%, preferably 8-25 wt%, for example, 8 wt%, 15 wt%, 25 wt%, 30 wt% or 35 wt%.

[0035] Preferably, in step (1), the ball milling treatment includes wet ball milling or dry ball milling.

[0036] Preferably, in step (1), the solvent used in the wet ball milling includes any one of water, acetone, ethanol or isopropanol.

[0037] Preferably, in step (1), the particle size of the lithium-extracted tailings powder after ball milling is ≤50 μm, preferably ≤40 μm, such as 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm or 40 μm, etc., but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable, and more preferably ≤30 μm.

[0038] In the present invention, the particle size of the lithium extraction tailings after ball milling treatment is preferably ≤50 μm, so that the encapsulated impurity elements are effectively exposed, thereby improving the removal efficiency of impurities.

[0039] Preferably, in step (2), the acid solution is any one of a sulfuric acid solution, a nitric acid solution, or hydrochloric acid. When the acid solution is a sulfuric acid solution, the concentration of the sulfuric acid solution is 0.01 to 1 mol / L, such as 0.01 mol / L, 0.05 mol / L, 0.1 mol / L, 0.5 mol / L, or 1 mol / L, but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable, and more preferably 0.05 to 0.5 mol / L.

[0040] Preferably, in step (2), the liquid-to-solid ratio of the acid solution to the lithium extraction tailings powder is 1-10 mL / g, preferably 3-10 mL / g, such as 3 mL / g, 4 mL / g, 5 mL / g, 6 mL / g, 7 mL / g, 8 mL / g, 9 mL / g or 10 mL / g, etc., but is not limited to the listed values. Other values ​​not listed within this numerical range are also applicable, and more preferably 3-6 mL / g.

[0041] Preferably, in step (2), the concentration of the sodium lauryl sulfate is 0.01 to 1 mol / L, such as 0.01 mol / L, 0.05 mol / L, 0.1 mol / L, 0.5 mol / L or 1 mol / L, but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable, and more preferably 0.01 to 0.5 mol / L.

[0042] Preferably, in step (2), the pickling temperature is 20-100°C, such as 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, etc., but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable, preferably 50-80°C;

[0043] Preferably, in step (2), the pickling time is 30 to 180 min, such as 30 min, 40 min, 60 min, 80 min, 100 min, 130 min or 150 min, etc., but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable, preferably 30 to 90 min;

[0044] Preferably, in step (2), the number of segmented pickling is 1 to 10 times, such as 1 time, 2 times, 3 times, 4 times or 5 times, but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable, preferably 1 to 5 times.

[0045] Preferably, in step (3), the acid solution is any one of a sulfuric acid solution, a phosphoric acid solution, or a hydrochloric acid solution. When the acid solution is a sulfuric acid solution, the concentration of the sulfuric acid solution is 1 to 3 mol / L, such as 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L, 3 mol / L, etc., but is not limited to the listed values. Other values ​​not listed within this numerical range are also applicable, and more preferably 1.5 to 2.5 mol / L.

[0046] Preferably, in step (3), the reducing agent comprises at least one of iron powder, sulfur dioxide gas, sodium sulfite, sodium thiosulfate, or sodium metabisulfite. When the reducing agent is iron powder, the molar ratio of the iron powder to the iron in the lithium extraction tailings powder is (0.01-1):1, such as 0.01:1, 0.05:1, 0.1:1, 0.5:1, 1:1, etc., but is not limited to the listed values. Other values ​​not listed within this numerical range are also applicable, and more preferably (0.01-0.2):1.

[0047] Preferably, in step (3), the leaching temperature is 20-100°C, such as 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, etc., but is not limited to the listed values. Other values ​​not listed within this numerical range are also applicable, preferably 50-80°C.

[0048] Preferably, in step (3), the leaching time is 30 to 180 min, such as 30 min, 40 min, 60 min, 80 min, 100 min, 130 min or 150 min, etc., but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable, preferably 30 to 90 min.

[0049] Preferably, in step (3), the number of segmented leaching is 1 to 10 times, such as 1, 2, 3, 4 or 5 times, but is not limited to the listed values. Other unlisted values ​​within the numerical range are also applicable, preferably 1 to 5 times.

[0050] Preferably, in step (3), the pH value of the leachate containing phosphorus and iron elements is 0-2, such as 0, 0.1, 0.5, 0.8, 1.4, 1.5, etc., but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable, and more preferably 0.1-0.8.

[0051] Preferably, in step (3), the iron powder and Fe 3+ The molar ratio is (1-1.5):1, such as 1:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1, etc., but is not limited to the listed values. Other unlisted values ​​within the numerical range are also applicable, and more preferably (1.2-1.4):1.

[0052] Preferably, in step (4), the fluoride is any one of ammonium fluoride, ammonium bifluoride, sodium fluoride or potassium fluoride. - Al in the leaching solution 3+ The molar ratio is (2-10):1, such as 2:1, 3:1, 5:1, 7:1, 10:1, etc., but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable, and more preferably (2-6):1.

[0053] Preferably, in step (5), the oxidant is any one of hydrogen peroxide, ozone, air, chlorine or sodium chlorate, preferably hydrogen peroxide.

[0054] Preferably, the iron content in the solution A is 0.35-1.2 mol / L, such as 0.35 mol / L, 0.5 mol / L, 0.75 mol / L, 1 mol / L or 1.2 mol / L, but is not limited to the listed values. Other values ​​not listed within this numerical range are also applicable, and more preferably 0.5-1.1 mol / L.

[0055] Preferably, in step (6), the phosphorus-containing solution is at least one of ammonium dihydrogen phosphate, phosphoric acid, or orthophosphate. The orthophosphate is sodium orthophosphate, potassium orthophosphate, or ammonium orthophosphate. When the phosphorus-containing solution is ammonium dihydrogen phosphate, the concentration of the ammonium dihydrogen phosphate is 1 to 3 mol / L, such as 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L, 3 mol / L, etc., but is not limited to the listed values. Other values ​​not listed within this numerical range are also applicable, and more preferably 1.5 to 2.5 mol / L.

[0056] After the ammonium dihydrogen phosphate is added, the molar ratio of total iron to total phosphorus in the system is 1: (1-1.5), such as 1:1, 1:1.1, 1:1.2, 1:1.3, 1:1.4, 1:1.5, etc., but is not limited to the listed values. Other values ​​not listed within this numerical range are also applicable, preferably 1: (1.2-1.4).

[0057] Preferably, in step (7), the pH value of the solution B is adjusted to 1.5-2.5, such as 1.5, 1.8, 2.0, 2.2, 2.5, etc., but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable, preferably 2-2.5.

[0058] Preferably, in step (7), the reaction temperature is 40-100°C, such as 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, etc., but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable, and more preferably 60-80°C.

[0059] Preferably, in step (7), the reaction time is 20 to 180 min, preferably 30 to 180 min, such as 20 min, 30 min, 40 min, 60 min, 80 min, 100 min, 130 min or 150 min, etc., but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable, and more preferably 60 to 120 min.

[0060] Preferably, in step (8), the amount of water added is such that the liquid-to-solid ratio of water to filter cake A is 1-16 mL / g, preferably 1-15 mL / g, such as 1 mL / g, 2 mL / g, 3 mL / g, 4 mL / g, 5 mL / g, 6 mL / g, 7 mL / g, 8 mL / g, 9 mL / g, 10 mL / g, 11 mL / g, 12 mL / g, 13 mL / g, 14 mL / g or 15 mL / g, etc., but is not limited to the listed values, and other values ​​not listed within this numerical range are also applicable, more preferably 3-5 mL / g.

[0061] Preferably, in step (8), the aging temperature is 40-100°C, such as 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, etc., but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable, and more preferably 80-100°C;

[0062] Preferably, in step (8), the aging time is 20 to 180 min, preferably 30 to 180 min, such as 20 min, 30 min, 40 min, 60 min, 80 min, 100 min, 130 min or 150 min, etc., but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable, and more preferably 120 to 180 min.

[0063] Preferably, in step (9), the washing is performed by stirring with pure water, the washing method is pulping washing, the liquid-to-solid ratio of each stirring washing is 1-16 mL / g, and the number of stirring washing times is 1-10 times.

[0064] Preferably, in step (9), the drying temperature is 80-150°C.

[0065] In the present invention, the staged pickling process is designed to remove some or all impurities (the main impurity element is aluminum) in the lithium extraction tailings, reducing the requirements for subsequent impurity removal and reducing the loss of phosphorus and iron elements. The staged leaching process is designed to efficiently extract phosphorus and iron elements from the lithium extraction tailings, reduce the acidity of the leachate, reduce the amount of alkali used in the subsequent synthesis process, and reduce production costs. The present invention performs staged pickling during the pickling process, controls the amount of acid and surfactant used, removes some or all impurities before leaching, and controls the amount of acid and reducing agent used during the leaching process, reducing the acidity of the leachate, significantly improving the leaching rate of iron and phosphorus, while reducing the amount of subsequent alkali used. The synthesized ferric phosphate dihydrate can meet battery-grade standards.

[0066] Compared with the prior art, the present invention has the following beneficial effects:

[0067] (1) The method of the present invention uses ball milling to effectively expose the encapsulated impurity elements, thereby improving the efficiency of impurity removal. During pickling, the impurity elements in the lithium extraction tailings are partially removed by using acid and surfactant, and the loss of phosphorus and iron elements is reduced.

[0068] (2) The present invention adopts segmented leaching to efficiently extract phosphorus and iron elements from lithium extraction tailings by controlling the acid concentration, the amount of reducing agent, the number of leaching times, the leaching temperature, and the leaching time, and reduces the acidity of the leaching solution, thereby reducing the amount of alkali used in the subsequent synthesis process and reducing production costs.

[0069] (3) The method of the present invention, through the mutual coordination of various processes, achieves a high extraction rate of the valuable element ferrophosphorus, uses less acid and alkali, and the synthesized ferric phosphate dihydrate meets battery-grade standards. It is environmentally friendly, has low equipment requirements, low energy consumption and cost, and good economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0070] Figure 1 This is a schematic flow chart of a method for recovering ferrophosphorus from lithium extraction tailings in Example 1 of the present invention. DETAILED DESCRIPTION

[0071] In order to make the technical solution of the present invention more clearly understood by those skilled in the art, the following examples are given for illustration. It should be noted that the following examples do not limit the scope of protection claimed by the present invention.

[0072] Unless otherwise specified, the raw materials, reagents, or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.

[0073] The mass fractions of the elements in the lithium extraction tailings powder (dry basis) used in the following examples and comparative examples are shown in Table 1. Table 1 mainly records the proportions of metal elements. In Table 1, the metals are calculated as oxides (the specific form was not tested), iron and phosphorus are calculated as ferric phosphate dihydrate, some of which are anhydrous ferric phosphate, and the acid-insoluble matter is mainly carbon powder and some other components. The total of each component is approximately 100%.

[0074] Table 1

[0075] Example 1

[0076] A method for recovering ferrophosphorus from lithium extraction tailings comprises the following steps:

[0077] (1) adding acid solution and surfactant to lithium extraction tailing powder with a particle size of ≤50 μm after ball milling, wherein the acid solution is 0.2 mol / L nitric acid solution, the liquid-solid ratio of acid solution to lithium extraction tailing powder is 10 mL / g, and the surfactant (sodium dodecyl sulfate) is 1 mol / L. After addition, the concentration of sodium dodecyl sulfate in the system (the system consists of lithium extraction tailing powder, nitric acid, sodium dodecyl sulfate, and water) is 0.01 mol / L, the pickling temperature is 70 °C, the pickling time is 90 min, and the number of pickling times is 1, thereby obtaining pickling residue and pickling solution (the pickling solution here is a single pickling solution);

[0078] (2) The pickling residue is added with acid solution and reducing agent for leaching, wherein the acid solution is 3 mol / L sulfuric acid solution, the reducing agent is iron powder, the molar ratio of iron powder to iron in lithium extraction tailings powder is 0.2:1, the liquid-solid ratio of acid solution to lithium extraction tailings powder is 5 mL / g, the leaching temperature is 80 °C, the leaching time is 90 min, and the leaching number is 1, to obtain a leachate containing phosphorus and iron elements (the leachate here is the 1st leachate) and a leaching residue;

[0079] (3) Iron powder is added to the leachate containing phosphorus and iron elements for reduction. The iron powder reacts with Fe 3+ The molar ratio is 1.2:1; then add ammonium fluoride to remove impurities, according to F - Al in the leaching solution 3+ Ammonium fluoride was added in a molar ratio of 6:1 and filtered to obtain a decontaminated solution;

[0080] (4) Add oxidizing agent hydrogen peroxide to the impurity removal liquid. Hydrogen peroxide can remove Fe 2+ The amount of addition calculated by weight is 1.2 times the theoretical amount, so that Fe 2+ After complete oxidation, solution A is obtained;

[0081] (5) Add 1 mol / L ammonium dihydrogen phosphate solution to solution A, and control the molar ratio of total iron to total phosphorus in solution A to be 1:1.2 to obtain solution B;

[0082] (6) Add 30 wt% ammonia water to solution B to adjust the pH value of solution B to 2.0, react at 80 °C for 2 h, and then separate the solid and liquid to obtain filter cake A;

[0083] (7) Add water to filter cake A in an amount such that the liquid-solid ratio of water to filter cake A is 5 mL / g. After aging at 90°C for 3 h, solid-liquid separation is performed to obtain filter cake B.

[0084] (8) The filter cake B was washed with pure water at a liquid-to-solid ratio of 10 mL / g each time, and the washing times were 5 times. After washing, the filter cake was filtered and dried at 100°C to obtain battery-grade ferric phosphate dihydrate. Example 2

[0085] A method for recovering ferrophosphorus from lithium extraction tailings comprises the following steps:

[0086] (1) After ball milling, the lithium extraction tailing powder with a particle size of ≤50 μm was added with acid solution and surfactant. The acid solution was 0.3 mol / L sulfuric acid solution, the liquid-solid ratio of the acid solution to the lithium extraction tailing powder was 5 mL / g, and the surfactant (sodium dodecyl sulfate) was 0.01 mol / L. After the addition, the concentration of sodium dodecyl sulfate in the system (the system consists of lithium extraction tailing powder, nitric acid, sodium dodecyl sulfate, and water) was 0.01 mol / L. The pickling temperature was 80 ° C. The total pickling time was 60 min (the time of each pickling was the same). The number of pickling times was 2 (the first pickling was to obtain 1 pickling solution and 1 pickling residue, and then the 1 pickling residue was pickled for the second time to obtain 2 pickling solutions and pickling residue). The 1 pickling solution and the 2 pickling solutions were combined to form a pickling solution.

[0087] (2) The pickling residue is added with acid solution and reducing agent for leaching, the acid solution is 1.5 mol / L sulfuric acid solution, the reducing agent is iron powder, the molar ratio of iron powder to iron in lithium extraction tailings powder is 0.2:1, the liquid-solid ratio of acid solution to lithium extraction tailings powder is 3 mL / g, the leaching temperature is 80 ° C, the total leaching time is 180 min (the time of each leaching is the same), the leaching times are 2 times (the first leaching obtains 1 leachate and 1 leach residue, and then the 1 leach residue is leached for the second time to obtain 2 leachates and leach residue), and the 1st leachate and the 2nd leachate are combined to obtain a leachate containing phosphorus and iron elements;

[0088] (3) Iron powder is added to the leachate containing phosphorus and iron elements for reduction. The iron powder reacts with Fe 3+ The molar ratio is 1.2:1; then add ammonium fluoride to remove impurities, according to F - Al in the leaching solution 3+ Ammonium fluoride was added in a molar ratio of 6:1 and filtered to obtain a decontaminated solution;

[0089] (4) Add oxidizing agent hydrogen peroxide to the impurity removal liquid. Hydrogen peroxide can remove Fe 2+ The total amount of addition is calculated to be 1.2 times the theoretical amount, so that Fe 2+ After complete oxidation, solution A is obtained;

[0090] (5) Add 1 mol / L ammonium dihydrogen phosphate solution to solution A, and control the molar ratio of total iron to total phosphorus in solution A to be 1:1.2 to obtain solution B;

[0091] (6) Add 30 wt% ammonia water to solution B to adjust the pH value of solution B to 2.0, react at 80 °C for 2 h, and then separate the solid and liquid to obtain filter cake A;

[0092] (7) Add water to filter cake A in an amount such that the liquid-solid ratio of water to filter cake A is 5 mL / g. After aging at 90°C for 3 h, solid-liquid separation is performed to obtain filter cake B.

[0093] (8) The filter cake B was washed with pure water at a liquid-to-solid ratio of 10 mL / g each time, and the washing times were 5 times. After washing, the filter cake was filtered and dried at 100°C to obtain battery-grade ferric phosphate dihydrate. Example 3

[0094] A method for recovering ferrophosphorus from lithium extraction tailings comprises the following steps:

[0095] (1) After ball milling, the lithium extraction tailing powder with a particle size of ≤50 μm was added with acid solution and surfactant, the acid solution was 0.5 mol / L sulfuric acid solution, the liquid-solid ratio of the acid solution to the lithium extraction tailing powder was 5 mL / g, the surfactant (sodium dodecyl sulfate) was 0.01 mol / L, and the concentration of sodium dodecyl sulfate in the system (the system was composed of lithium extraction tailing powder, nitric acid, sodium dodecyl sulfate, and water) was 0.01 mol / L after addition, the pickling temperature was 80 ° C, the total pickling time was 60 min (the time of each pickling was the same), the pickling times were 3 times (the first pickling to obtain 1 pickling solution and 1 pickling residue, then the 1 pickling residue was pickled for the second time to obtain 2 pickling solutions and 2 pickling residues, then the 2 pickling residue was pickled for the third time to obtain pickling residues and 3 pickling solutions), the 1 pickling solution, the 2 pickling solution and the 3 pickling solution were combined to form a pickling solution;

[0096] (2) The pickling residue is added with acid solution and reducing agent for leaching, wherein the acid solution is 1.5 mol / L sulfuric acid solution, the reducing agent is iron powder, the molar ratio of iron powder to iron in the lithium extraction tailings powder is 0.2:1, the liquid-solid ratio of acid solution to lithium extraction tailings powder is 3 mL / g, the leaching temperature is 80 ° C, the total leaching time is 180 min (the time of each leaching is the same), the number of leaching is 3 times (the first leaching obtains 1 leachate and 1 leach residue, and then the 1 leach residue is leached for the second time to obtain 2 leachate and 2 leach residue, and then the 2 leach residue is leached for the third time to obtain leach residue and 3 leachate), and the 1st leachate, the 2nd leachate and the 3rd leachate are combined to obtain a leachate containing phosphorus and iron elements;

[0097] (3) Iron powder is added to the leachate containing phosphorus and iron elements for reduction. The iron powder reacts with Fe 3+ The molar ratio is 1.2:1; then add ammonium fluoride to remove impurities, according to F - Al in the leaching solution 3+ Ammonium fluoride was added in a molar ratio of 6:1 and filtered to obtain a decontaminated solution;

[0098] (4) Add oxidizing agent hydrogen peroxide to the impurity removal liquid. Hydrogen peroxide can remove Fe 2+ The total amount of addition is calculated to be 1.2 times the theoretical amount, so that Fe 2+ After complete oxidation, solution A is obtained;

[0099] (5) Add 1 mol / L ammonium dihydrogen phosphate solution to solution A, and control the molar ratio of total iron to total phosphorus in solution A to be 1:1.2 to obtain solution B;

[0100] (6) Add 30 wt% ammonia water to solution B to adjust the pH value of solution B to 2.0, react at 80 °C for 2 h, and then separate the solid and liquid to obtain filter cake A;

[0101] (7) Add water to filter cake A in an amount such that the liquid-solid ratio of water to filter cake A is 5 mL / g. After aging at 90°C for 3 h, solid-liquid separation is performed to obtain filter cake B.

[0102] (8) The filter cake B was washed with pure water at a liquid-to-solid ratio of 10 mL / g each time, and the washing times were 5 times. After washing, the filter cake was filtered and dried at 100°C to obtain battery-grade ferric phosphate dihydrate.

[0103] Comparative Example 1

[0104] A method for recovering ferrophosphorus from lithium extraction tailings comprises the following steps:

[0105] (1) After ball milling, the lithium extraction tailing powder with a particle size of ≤50 μm was added with acid solution and surfactant, wherein the acid solution was a 0.2 mol / L nitric acid solution, the liquid-solid ratio of the acid solution to the lithium extraction tailing powder was 10 mL / g, and the surfactant (hexadecyltrimethylammonium bromide) was 1 mol / L. After the addition, the concentration of hexadecyltrimethylammonium bromide in the system (the system consisted of lithium extraction tailing powder, nitric acid, hexadecyltrimethylammonium bromide, and water) was 0.01 mol / L, the pickling temperature was 70 °C, the pickling time was 90 min, and the number of pickling times was 1, thereby obtaining pickling residue and pickling solution;

[0106] (2) The pickling residue was added with acid solution and reducing agent for leaching, wherein the acid solution was 3 mol / L sulfuric acid solution, the reducing agent was iron powder, the molar ratio of iron powder to iron in the lithium extraction tailings powder was 0.2:1, the liquid-solid ratio of acid solution to lithium extraction tailings powder was 5 mL / g, the leaching temperature was 80 °C, the leaching time was 90 min, and the leaching number was 1, to obtain a leachate containing phosphorus and iron elements;

[0107] (3) Iron powder is added to the leachate containing phosphorus and iron elements for reduction. The iron powder reacts with Fe 3+ The molar ratio is 1.2:1; then add ammonium fluoride to remove impurities, according to F- Al in the leaching solution 3+ Ammonium fluoride was added in a molar ratio of 6:1 and filtered to obtain a decontaminated solution;

[0108] (4) Add oxidizing agent hydrogen peroxide to the impurity removal liquid. Hydrogen peroxide can remove Fe 2+ The total amount of addition is calculated to be 1.2 times the theoretical amount, so that Fe 2+ After complete oxidation, solution A is obtained;

[0109] (5) Add 1 mol / L ammonium dihydrogen phosphate solution to solution A, and control the molar ratio of total iron to total phosphorus in solution A to be 1:1.2 to obtain solution B;

[0110] (6) Add 30 wt% ammonia water to solution B to adjust the pH value of solution B to 2.0, react at 80 °C for 2 h, and then separate the solid and liquid to obtain filter cake A;

[0111] (7) Add water to filter cake A in an amount such that the liquid-solid ratio of water to filter cake A is 5 mL / g. After aging at 90°C for 3 h, solid-liquid separation is performed to obtain filter cake B.

[0112] (8) The filter cake B was washed with pure water at a liquid-to-solid ratio of 10 mL / g each time, and the washing times were 5 times. After washing, the filter cake was filtered and dried at 100°C to obtain battery-grade ferric phosphate dihydrate.

[0113] Comparative Example 2

[0114] A method for recovering ferrophosphorus from lithium extraction tailings comprises the following steps:

[0115] (1) After ball milling, the lithium extraction tailing powder with a particle size of ≤50 μm was added with acid solution and surfactant, wherein the acid solution was 0.2 mol / L nitric acid solution, the liquid-solid ratio of the acid solution to the lithium extraction tailing powder was 10 mL / g, and the surfactant (sodium dodecyl sulfate) was 1 mol / L. After the addition, the concentration of sodium dodecyl sulfate in the system (the system consisted of lithium extraction tailing powder, nitric acid, sodium dodecyl sulfate, and water) was 0.01 mol / L, the pickling temperature was 70 °C, the pickling time was 90 min, and the pickling number was 1, thereby obtaining pickling residue and pickling solution;

[0116] (2) The pickling residue was added with acid solution and reducing agent for leaching, wherein the acid solution was 3 mol / L sulfuric acid solution, the reducing agent was iron powder, the molar ratio of iron powder to iron in the lithium extraction tailings powder was 0.2:1, the liquid-solid ratio of acid solution to lithium extraction tailings powder was 5 mL / g, the leaching temperature was 80 °C, the leaching time was 90 min, and the leaching number was 1, to obtain a leachate containing phosphorus and iron elements;

[0117] (3) Iron powder is added to the leachate containing phosphorus and iron elements for reduction. The iron powder reacts with Fe 3+ The molar ratio is 1.2:1; sodium hydroxide is then added to remove impurities, the pH is adjusted to 3.0, and the impurity-removed liquid is obtained after filtration;

[0118] (4) Add oxidizing agent hydrogen peroxide to the impurity removal liquid. Hydrogen peroxide can remove Fe 2+ The total amount of addition is calculated to be 1.2 times the theoretical amount, so that Fe 2+ After complete oxidation, solution A is obtained;

[0119] (5) Add 1 mol / L ammonium dihydrogen phosphate solution to solution A, and control the molar ratio of total iron to total phosphorus in solution A to be 1:1.2 to obtain solution B;

[0120] (6) Add 30 wt% ammonia water to solution B to adjust the pH value of solution B to 2.0, react at 80 °C for 2 h, and then separate the solid and liquid to obtain filter cake A;

[0121] (7) Add water to filter cake A in an amount such that the liquid-solid ratio of water to filter cake A is 5 mL / g. After aging at 90°C for 3 h, solid-liquid separation is performed to obtain filter cake B.

[0122] (8) The filter cake B was washed with pure water at a liquid-to-solid ratio of 10 mL / g each time, and the washing times were 5 times. After washing, the filter cake was filtered and dried at 100°C to obtain battery-grade ferric phosphate dihydrate.

[0123] Effect test

[0124] The leaching rate of each element is calculated as follows: leaching rate of element (%) = total mass of the element in the pickling solution or leachate / total mass of the element in the lithium extraction tailings powder * 100%.

[0125] The pickling solutions and leachates obtained in the examples and comparative examples were tested for the contents of various elements (except phosphorus) by inductively coupled plasma (ICP) spectroscopy, and for the content of phosphorus by spectrophotometry. The leaching rates of various elements were calculated, and the results are shown in Tables 2 to 5 below.

[0126] The leaching rate of the first pickling solution is the leaching rate of the pickling solution obtained by the first pickling, the leaching rate of the second pickling solution is the leaching rate of the pickling solution obtained by the second pickling, the leaching rate of the third pickling solution is the leaching rate of the pickling solution obtained by the third pickling, and the leaching rate of the pickling solution subtotal is the sum of the leaching rates corresponding to the three pickling solutions.

[0127] The leaching rate of the first leachate is the leaching rate of the leachate obtained by the first leaching, the leaching rate of the second leachate is the leaching rate of the leachate obtained by the second leaching, the leaching rate of the third leachate is the leaching rate of the leachate obtained by the third leaching, and the leaching rate of the subtotal leachate is the sum of the leaching rates corresponding to the three leachates respectively.

[0128] Table 2: Leaching rate results of Example 1

[0129]

[0130] Table 3: Leaching rate results of Example 2

[0131]

[0132] Table 4: Leaching rate results of Example 3

[0133]

[0134] Table 5: Leaching rate results of the pickling solution and leachate of Example 1 and Comparative Example 1

[0135]

[0136] Table 6: Impurity removal results of Example 1 and Comparative Example 2

[0137]

[0138] Note: Aluminum removal rate (%) = (aluminum mass in leachate - aluminum mass in impurity removal solution) / aluminum mass in leachate * 100%, total phosphorus or iron recovery (%) = phosphorus or iron mass in battery-grade ferric phosphate dihydrate / phosphorus or iron mass in lithium extraction tailings powder * 100%.

[0139] As can be seen from the results of above-mentioned Table 2 to Table 6, pickling process of the present invention needs to control the acid solution concentration, the kind of surfactant, the kind of impurity remover, the pickling number, the pickling temperature, the pickling time to be coordinated within a certain range to reach the effective removal of impurity elements, and reduce the loss of phosphorus and iron elements. Leaching process needs to control the acid solution concentration, the reducing agent dosage, the leaching number, the leaching temperature, the leaching time to be coordinated within a certain range to reach the phosphorus and iron elements in the lithium tailings to be efficiently extracted, and reduce the acidity of the leachate, reduce the alkali dosage of the subsequent synthesis process. The present invention adopts ball milling, segmented pickling, segmented leaching, realizes the effective separation of impurities in the lithium tailings, can effectively reduce the impurity removal cost of synthesis process, controls the acid consumption to realize the efficient extraction of iron and phosphorus, and reduces the consumption of subsequent alkali, improves production economic benefit, realizes the resource utilization, harmlessness, reduction disposal of the lithium tailings. The method of the present invention is simple to operate, and iron and phosphorus extraction rates are high, without pollutant discharge, environmental protection and energy saving, clean production, with significant economic benefit.

[0140] The above content describes the basic principle and main features of the present invention and the advantages of the present invention. It should be understood by those skilled in the art that protection scope of the present invention is not limited by the above-described embodiments. Without departing from the spirit and scope of the present invention, the present invention also has various changes and improvements, and these changes and improvements all fall within the scope of the present invention claimed.

Claims

1. A method for recovering ferrophosphorus from lithium extraction tailings, characterized in that: The following steps are involved: (1) adding an acid solution and a surfactant to lithium extraction tailing powder with a particle size of ≤50 μm after ball milling, wherein the acid solution is a 0.2 mol / L nitric acid solution, the liquid-to-solid ratio of the acid solution to the lithium extraction tailing powder is 10 mL / g, the surfactant is sodium dodecyl sulfate, the concentration of the surfactant is 1 mol / L, and the concentration of the sodium dodecyl sulfate in the system is 0.01 mol / L after the addition, the system is composed of lithium extraction tailing powder, nitric acid, sodium dodecyl sulfate, and water, the pickling temperature is 70° C., the pickling time is 90 min, the pickling number is 1, and the pickling residue and pickling solution are obtained, wherein the pickling solution here is a 1 pickling solution; (2) adding acid solution and reducing agent to the pickled residue for leaching, wherein the acid solution is 3 mol / L sulfuric acid solution, the reducing agent is iron powder, the molar ratio of iron powder to iron in lithium extraction tailings powder is 0.2:1, the liquid-solid ratio of acid solution to lithium extraction tailings powder is 5 mL / g, the leaching temperature is 80°C, the leaching time is 90 min, the leaching number is 1, and a leachate and leached residue containing phosphorus and iron elements are obtained, wherein the leachate here is a 1-time leachate; (3) Iron powder is added to the leaching solution containing phosphorus and iron elements for reduction. The iron powder reacts with Fe in the leaching solution. 3+ The molar ratio is 1.2:1; then add ammonium fluoride to remove impurities, according to F - Al in the leaching solution 3+ Ammonium fluoride was added in a molar ratio of 6:1, and the impurity-removing liquid was obtained after filtration; (4) Add oxidant hydrogen peroxide to the impurity removal liquid. The hydrogen peroxide is used to remove Fe 2+ The amount of addition calculated by weight is 1.2 times the theoretical amount, so that Fe 2+ After complete oxidation, solution A is obtained; (5) adding 1 mol / L diammonium dihydrogen phosphate solution to solution A to control the molar ratio of total iron to total phosphorus in solution A to be 1:1.2, thereby obtaining solution B; (6) adding 30 wt % ammonia water to solution B to adjust the pH value of solution B to 2.0, reacting at 80° C. for 2 h, and then separating the solid and the liquid to obtain filter cake A; (7) adding water to filter cake A in an amount such that the liquid-to-solid ratio of water to filter cake A is 5 mL / g, aging at 90° C. for 3 h, and then separating the solid and the liquid to obtain filter cake B; (8) The filter cake B was washed with pure water, the liquid-to-solid ratio of each washing was 10 mL / g, and the washing times were 5 times. After washing, the filter cake was filtered and dried at 100° C. to obtain battery-grade ferric phosphate dihydrate.

Citation Information

Patent Citations

  • Method for recovering valuable metals in waste lithium iron phosphate positive electrode powder

    CN115744940A

  • Method for recovering lithium iron phosphate lithium extraction slag

    CN118145611A

  • Method for recycling waste lithium iron phosphate batteries

    CN118281390A