A high-efficiency anti-corrosion mortar material and its preparation method and application
Through the combination of rare earth oxide modified graphene and urushiol acetal resin composite materials with cement, fly ash and other raw materials, the problem of poor anti-corrosion effect and easy cracking of building anti-corrosion mortar is solved, and high-efficiency anti-corrosion and anti-cracking properties are achieved. Extends the service life of building materials and reduces costs.
Patent Information
- Application Number
- CN202411017180.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-29
AI Technical Summary
Existing anti-corrosion mortars for buildings have poor anti-corrosion effects and are prone to cracking, resulting in shortened service life of building materials, complicated operations and high costs.
The composite material of rare earth oxide modified graphene and urushiol acetal resin is used as the cementing material, combined with raw materials such as cement, fly ash, slag powder and quartz sand, through the modification treatment and compounding of rare earth oxide modified graphene. The synergistic effect of materials improves the anti-corrosion and cracking resistance of mortar.
It achieves good anti-corrosion performance and anti-cracking performance of high-efficiency anti-corrosion mortar materials, extends the service life of building materials, reduces operation complexity and cost, and provides new design ideas for building materials.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building materials, and specifically discloses a high-efficiency anti-corrosion mortar material and a preparation method and application thereof. Background Art
[0002] The exterior walls and ceilings of buildings are in direct contact with the external environment and need to be treated with anti-corrosion to reduce the erosion of the concrete matrix by pollutants such as rainwater. The anti-corrosion performance of building materials directly affects the service life and safety of engineering buildings.
[0003] At present, the commonly used anticorrosive building materials are mainly anticorrosive coatings and anticorrosive mortars. The former is a protective layer in the form of a coating cover, which has insufficient durability and its service life is far lower than the engineering building to be protected. In addition, in actual operation, it is generally necessary to set a waterproof interface mortar layer between the anticorrosive coating layer and the substrate layer, which is complicated to operate and increases the cost.
[0004] The anti-corrosion mortar is generally a polymer-modified silicate cement mortar or a high-alumina cement system anti-corrosion mortar, which uses hydration to form an impermeable layer, and compounded with water-soluble glue powder to increase the gel degree of the mortar, improve the mortar's impermeability, and achieve the purpose of anti-corrosion. However, the existing anti-corrosion mortar has the problem of easy cracking after stress shrinkage. Although it can be strengthened by adding fiber materials, it only delays the time of cracking and cannot fundamentally solve the above problem.
[0005] Based on this, developing a mortar material that is low-cost, easy to operate and has long-term anti-corrosion is of great significance to the development of new building materials. Summary of the invention
[0006] In view of the problem that the building anticorrosive mortar in the prior art has poor anticorrosive effect and is prone to cracking, the present invention provides a high-efficiency anticorrosive mortar material and its preparation method and application. The high-efficiency anticorrosive mortar material is prepared by using cement and rare earth oxide modified graphene / lacquer phenol acetal resin composite material as cementitious material and anticorrosive material; fly ash, slag powder and quartz sand as aggregates; water reducer, defoamer and stabilizer as additives. The present invention utilizes the synergistic effect of each raw material component to make the obtained high-efficiency anticorrosive mortar material have good anticorrosive performance and anti-cracking performance.
[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0008] The first aspect of the present invention provides a high-efficiency anti-corrosion mortar material, comprising the following raw material components in parts by weight: 100-120 parts of cement, 30-80 parts of fly ash, 20-50 parts of slag powder, 80-100 parts of quartz sand, 1-5 parts of water reducer, 1-2 parts of defoamer, 1-2 parts of stabilizer, 20-35 parts of rare earth oxide modified graphene / lacquer phenol acetal resin composite material and 60-90 parts of water.
[0009] Graphene has a small size effect, a two-dimensional sheet structure and hydrophobic properties, and can be used as a nanofiller to improve the anti-corrosion performance of materials. However, the dispersibility and wettability of graphene are relatively poor, which makes it easy for graphene to be stratified and agglomerated when mixed with other components, greatly reducing its anti-corrosion performance. Based on this, the present invention uses rare earth oxides to modify it. Since rare earth elements have low electronegativity and high activity, they can form Re-C bonds with graphene, making the state of rare earth-modified graphene materials more stable and avoiding agglomeration of graphene-based materials.
[0010] In order to further improve the anti-corrosion effect of the mortar material, the present invention composites the rare earth oxide modified graphene with lacquer phenol acetal resin, takes the lacquer phenol acetal resin as the matrix, and the rare earth oxide modified graphene is a modifier attached to the surface and inside of the lacquer phenol acetal resin. The poor wettability of graphene is used to increase the contact angle of the lacquer phenol acetal resin, thereby achieving the purpose of improving the anti-corrosion performance of the mortar material. In addition, the addition of rare earth oxide modified graphene further fills the defects of the lacquer phenol acetal resin, further improves the cross-linking degree between the molecules of the lacquer phenol acetal resin, improves the density of the mortar material, and can better resist ion corrosion.
[0011] The present invention uses rare earth oxide modified graphene / lacquer phenol acetal resin composite material as the main anti-corrosion material, and combines cement, fly ash, slag powder, quartz sand, and raw material additives such as water reducer, defoamer and stabilizer to prepare a high-efficiency anti-corrosion mortar material. The present invention utilizes the synergistic effect of various raw material components to make the obtained high-efficiency anti-corrosion mortar material have good anti-corrosion performance and anti-cracking performance, providing a new design idea for new building materials.
[0012] Preferably, the rare earth oxide is cerium oxide or lanthanum oxide.
[0013] Preferably, the preparation method of the rare earth oxide modified graphene / urushiol acetal resin composite material comprises the following steps:
[0014] S1, dissolving urushiol and formaldehyde in a phenyl solvent, adding a catalyst, and reacting at 50-60° C. for 3-6 hours to obtain urushiol acetal resin;
[0015] S2, dispersing a rare earth oxide precursor in an alcohol solution, adding graphene, ultrasonicating, reacting at 80-120° C. for 2-5 hours to obtain a mixed system; transferring the mixed system to a reactor, performing a hydrothermal reaction at 170-190° C., solid-liquid separation, and drying to obtain rare earth oxide-modified graphene;
[0016] S3, ball-milling the rare earth oxide modified graphene, adding the urushiol acetal resin, mixing evenly, and drying to obtain the rare earth oxide modified graphene / urushiol acetal resin composite material.
[0017] Further preferably, in S1, the mass ratio of urushiol to formaldehyde is 10:2-15:4.
[0018] Further preferably, in S1, the volume ratio of the urushiol to the phenyl solvent is 1:10-2:15.
[0019] Further preferably, in S1, the amount of the catalyst added is 0.5%-1% of the mass of the phenyl solvent.
[0020] Further preferably, in S1, the phenyl solvent is xylene.
[0021] Further preferably, in S1, the catalyst is a 0.1-0.5 mol / L sodium hydroxide solution.
[0022] Further preferably, in S2, the rare earth oxide precursor is cerium nitrate or lanthanum nitrate.
[0023] Further preferably, in S2, the alcohol solution is a 55%-65% ethanol solution.
[0024] Further preferably, in S2, the mass volume ratio of the rare earth oxide precursor to the alcohol solution is 1g:5mL-1g:8mL.
[0025] Further preferably, in S2, the mass ratio of the rare earth oxide precursor to the graphene is 1:2-1:4.
[0026] Further preferably, in S2, the ultrasonic treatment time is 30 min-45 min.
[0027] Further preferably, in S2, the hydrothermal reaction time is 12-20 hours.
[0028] Further preferably, in S3, the mass ratio of the rare earth oxide modified graphene to the lacquer phenol acetal resin is 1:15-1:25.
[0029] Preferably, the cement is Portland cement.
[0030] Preferably, the particle size of the fly ash is 0.05-0.15 mm.
[0031] Preferably, the particle size of the slag powder is 0.1-0.3 mm.
[0032] Preferably, the particle size of the quartz sand is 0.2-0.8 mm.
[0033] Preferably, the water reducer is any one of a sodium lignin sulfonate water reducer, a naphthalene-based high-efficiency water reducer, an aliphatic high-efficiency water reducer, an amino high-efficiency water reducer or a polycarboxylic acid high-efficiency water reducer.
[0034] Preferably, the defoaming agent is P803 or P210z.
[0035] Preferably, the stabilizer is any one of EL0002, TAB-2 or T-386.
[0036] The second aspect of the present invention provides a method for preparing the highly efficient anti-corrosion mortar material, which is characterized by comprising the following steps: weighing each raw material component according to the designed ratio, and mixing the weighed components evenly to obtain a highly efficient anti-corrosion mortar material.
[0037] The third aspect of the present invention provides the use of the high-efficiency anti-corrosion mortar material or the high-efficiency anti-corrosion mortar material prepared by the preparation method of the high-efficiency anti-corrosion mortar material in the field of building insulation.
[0038] In summary, the present invention provides a high-efficiency anti-corrosion mortar material and a preparation method and application thereof, wherein the high-efficiency anti-corrosion mortar material is prepared using cement and rare earth oxide modified graphene / lacquer phenol acetal resin composite materials as cementitious materials and anti-corrosion materials; fly ash, slag powder and quartz sand as aggregates; and water reducer, defoamer and stabilizer as additives. The present invention utilizes the synergistic effect of each raw material component to make the obtained high-efficiency anti-corrosion mortar material have good anti-corrosion performance and anti-cracking performance, thereby effectively solving the problem that the building anti-corrosion mortar in the prior art has poor anti-corrosion effect and is prone to cracking. DETAILED DESCRIPTION
[0039] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0040] Example 1
[0041] This embodiment provides a high-efficiency anti-corrosion mortar material and a preparation method thereof, which specifically includes the following contents:
[0042] The high-efficiency anti-corrosion mortar material includes the following raw material components in parts by mass: 110 parts of silicate cement, 60 parts of fly ash, 40 parts of slag powder, 90 parts of quartz sand, 2 parts of polycarboxylic acid high-performance water reducer, 1 part of defoamer P803, 1 part of stabilizer EL0002, 25 parts of cerium oxide modified graphene / lacquer phenol acetal resin composite material and 70 parts of water.
[0043] The raw material components are weighed according to the designed proportions, and mixed evenly to obtain the high-efficiency anti-corrosion mortar material.
[0044] The preparation method of the cerium oxide modified graphene / urushiol acetal resin composite material comprises the following steps:
[0045] S1. Dissolve 500 g of urushiol and 150 g of formaldehyde in 5000 mL of xylene, add 30 g of 0.3 mol / L sodium hydroxide solution, and react at 55° C. for 4 h to obtain urushiol acetal resin;
[0046] S2, dispersing 10g of cerium nitrate in 60mL of 55% ethanol solution, adding 30g of graphene, ultrasonicating for 40min, reacting at 100°C for 3h to obtain a mixed system; transferring the mixed system to a reactor, performing a hydrothermal reaction at 180°C for 14h, separating the solid from the liquid, and drying at 100°C for 2h to obtain cerium oxide modified graphene;
[0047] S3. Ball-mill 40 g of cerium oxide modified graphene at a rotation speed of 800 rpm for 3 h, add 800 g of the lacquer phenol acetal resin, mix well, and dry to obtain the cerium oxide modified graphene / lacquer phenol acetal resin composite material.
[0048] The particle size of the fly ash is 0.1 mm; the particle size of the slag powder is 0.2 mm; and the particle size of the quartz sand is 0.5 mm.
[0049] Example 2
[0050] This embodiment provides a high-efficiency anti-corrosion mortar material and a preparation method thereof, which specifically includes the following contents:
[0051] The high-efficiency anti-corrosion mortar material includes the following raw material components in parts by mass: 120 parts of silicate cement, 80 parts of fly ash, 20 parts of slag powder, 80 parts of quartz sand, 5 parts of sodium lignin sulfonate water reducer, 2 parts of defoamer PP210z, 2 parts of stabilizer EL0002, 35 parts of cerium oxide modified graphene / lacquer phenol acetal resin composite material and 90 parts of water.
[0052] The raw material components are weighed according to the designed proportions, and mixed evenly to obtain the high-efficiency anti-corrosion mortar material.
[0053] The preparation method of the cerium oxide modified graphene / urushiol acetal resin composite material comprises the following steps:
[0054] S1. Dissolve 500 g of urushiol and 150 g of formaldehyde in 5000 mL of xylene, add 30 g of 0.3 mol / L sodium hydroxide solution, and react at 50° C. for 4 h to obtain urushiol acetal resin;
[0055] S2, dispersing 10g of cerium nitrate in 70mL of 55% ethanol solution, adding 30g of graphene, ultrasonicating for 40min, reacting at 100°C for 3h to obtain a mixed system; transferring the mixed system to a reactor, performing a hydrothermal reaction at 170°C for 16h, solid-liquid separation, and drying at 90°C for 3h to obtain cerium oxide modified graphene;
[0056] S3. Ball-mill 40 g of cerium oxide modified graphene at a rotation speed of 900 rpm for 3 h, add 800 g of the lacquer phenol acetal resin, mix well, and dry to obtain the cerium oxide modified graphene / lacquer phenol acetal resin composite material.
[0057] The particle size of the fly ash is 0.05 mm; the particle size of the slag powder is 0.3 mm; and the particle size of the quartz sand is 0.4 mm.
[0058] Example 3
[0059] This embodiment provides a high-efficiency anti-corrosion mortar material and a preparation method thereof, which specifically includes the following contents:
[0060] The high-efficiency anti-corrosion mortar material includes the following raw material components in parts by weight: 120 parts of silicate cement, 50 parts of fly ash, 50 parts of slag powder, 100 parts of quartz sand, 4 parts of naphthalene-based high-efficiency water reducer, 1 part of defoamer P210, 1 part of stabilizer TAB-2, 30 parts of lanthanum oxide modified graphene / lacquer phenol acetal resin composite material and 80 parts of water.
[0061] The raw material components are weighed according to the designed proportions, and mixed evenly to obtain the high-efficiency anti-corrosion mortar material.
[0062] The preparation method of the lanthanum oxide modified graphene / urushiol acetal resin composite material comprises the following steps:
[0063] S1. Dissolve 500 g of urushiol and 150 g of formaldehyde in 5000 mL of xylene, add 30 g of 0.2 mol / L sodium hydroxide solution, and react at 50° C. for 4 h to obtain urushiol acetal resin;
[0064] S2, dispersing 10g of lanthanum nitrate in 80mL of 55% ethanol solution, adding 30g of graphene, ultrasonicating for 40min, reacting at 100°C for 3h to obtain a mixed system; transferring the mixed system to a reactor, performing a hydrothermal reaction at 170°C for 14h, solid-liquid separation, and drying at 100°C for 3h to obtain lanthanum oxide modified graphene;
[0065] S3, ball-milling 40 g of the lanthanum oxide modified graphene at a rotation speed of 700 rpm for 3 h, adding 800 g of the lacquer phenol acetal resin, mixing evenly, and drying to obtain a lanthanum oxide modified graphene / lacquer phenol acetal resin composite material.
[0066] The particle size of the fly ash is 0.1 mm; the particle size of the slag powder is 0.1 mm; and the particle size of the quartz sand is 0.8 mm.
[0067] Comparative Example 1
[0068] This comparative example provides an anticorrosive mortar material and a preparation method thereof, which differs from Example 1 in that the cerium oxide modified graphene / urushiol acetal resin composite material is replaced with an equal amount of urushiol acetal resin, and other components and processes remain unchanged, specifically including the following contents:
[0069] The anticorrosive mortar material includes the following raw material components in parts by mass: 110 parts of silicate cement, 60 parts of fly ash, 40 parts of slag powder, 90 parts of quartz sand, 2 parts of polycarboxylic acid high-performance water reducing agent, 1 part of defoamer P803, 1 part of stabilizer EL0002, 25 parts of lacquer phenol acetal resin and 70 parts of water.
[0070] Weigh each raw material component according to the designed ratio, mix them evenly, and obtain the anti-corrosion mortar material.
[0071] The preparation method of the urushiol acetal resin comprises the following steps: dissolving 500g urushiol and 150g formaldehyde in 5000mL xylene, adding 30g 0.3mol / L sodium hydroxide solution, reacting at 55°C for 4h to obtain the urushiol acetal resin.
[0072] The particle size of the fly ash is 0.1 mm; the particle size of the slag powder is 0.2 mm; and the particle size of the quartz sand is 0.5 mm.
[0073] Comparative Example 2
[0074] This comparative example provides an anticorrosive mortar material and a preparation method thereof, which differs from Example 1 in that the cerium oxide modified graphene / lacquer phenol acetal resin composite material is replaced with an equal amount of cerium oxide modified graphene, and other components and processes remain unchanged, specifically including the following contents:
[0075] The anticorrosive mortar material includes the following raw material components in parts by mass: 110 parts of silicate cement, 60 parts of fly ash, 40 parts of slag powder, 90 parts of quartz sand, 2 parts of polycarboxylic acid high-performance water reducing agent, 1 part of defoaming agent P803, 1 part of stabilizer EL0002, 25 parts of cerium oxide modified graphene and 70 parts of water.
[0076] Weigh each raw material component according to the designed ratio, mix them evenly, and obtain the anti-corrosion mortar material.
[0077] The preparation method of cerium oxide modified graphene includes the following steps: dispersing 10g of cerium nitrate in 60mL of 55% ethanol solution, adding 30g of graphene, ultrasonicating for 40min, reacting at 100°C for 3h to obtain a mixed system; transferring the mixed system to a reactor, performing a hydrothermal reaction at 180°C for 14h, separating the solid from the liquid, and drying at 100°C for 2h to obtain cerium oxide modified graphene.
[0078] The particle size of the fly ash is 0.1 mm; the particle size of the slag powder is 0.2 mm; and the particle size of the quartz sand is 0.5 mm.
[0079] Comparative Example 3
[0080] This comparative example provides a high-efficiency anticorrosive mortar material and a preparation method thereof, which is different from Example 1 in that the cerium oxide-modified graphene / urushiol acetal resin composite material is replaced with an equal amount of graphene / urushiol acetal resin composite material, and other components and processes remain unchanged, specifically including the following contents:
[0081] The high-efficiency anti-corrosion mortar material includes the following raw material components in parts by mass: 110 parts of silicate cement, 60 parts of fly ash, 40 parts of slag powder, 90 parts of quartz sand, 2 parts of polycarboxylic acid high-performance water reducer, 1 part of defoamer P803, 1 part of stabilizer EL0002, 25 parts of graphene / lacquer phenol acetal resin composite material and 70 parts of water.
[0082] The raw material components are weighed according to the designed proportions, and mixed evenly to obtain the high-efficiency anti-corrosion mortar material.
[0083] The preparation method of the graphene / lacquer phenol acetal resin composite material comprises the following steps:
[0084] S1. Dissolve 500 g of urushiol and 150 g of formaldehyde in 5000 mL of xylene, add 30 g of 0.3 mol / L sodium hydroxide solution, and react at 55° C. for 4 h to obtain urushiol acetal resin;
[0085] S2. Ball-mill 40 g of graphene at a rotation speed of 800 rpm for 3 h, add 800 g of the lacquer phenol acetal resin, mix well, and dry to obtain the graphene / lacquer phenol acetal resin composite material.
[0086] The particle size of the fly ash is 0.1 mm; the particle size of the slag powder is 0.2 mm; and the particle size of the quartz sand is 0.5 mm.
[0087] In order to further reflect the technical effect of the present invention, the present invention conducted the following tests on the mortar materials obtained in Examples 1-3 and Comparative Examples 1-3: the mortar was poured into a mold, standardly cured for 7 days, and an SS-15 mortar impermeability tester was used to perform an impermeability test with reference to the JGJ / T70-2009 standard; a prismatic specimen with a specification of 40×40×160 mm was cast, standardly cured for 28 days, and an electronic universal testing machine was used to perform a flexural performance test. The specific test data results are shown in Table 1.
[0088] Table 1 Performance test results of various mortar materials
[0089]
[0090] The present invention refers to GB / T50082-2009 "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete" to conduct durability (resistance to sulfate erosion and resistance to chloride ion penetration) tests on the mortar materials obtained in each embodiment and each comparative example.
[0091] The test steps for sulfate corrosion resistance include: preparing test pieces with a molding size of 40 mm × 40 mm × 160 mm according to GB / T29756-2013, and curing them at 22°C and a relative humidity of 60% for 28 days; immersing the test pieces cured to the age in water and 5% sodium sulfate solution respectively, and testing the flexural strength and compressive strength of the test pieces after immersion for 30 days and 90 days; during this period, the sodium sulfate solution should be regularly replenished to ensure its concentration; and calculating the flexural or compressive corrosion resistance coefficient according to formula (1).
[0092]
[0093] Formula (1)
[0094] Where: F (f,c)s It indicates the flexural strength or compressive strength of the specimen after being immersed in sodium sulfate solution for a certain period of time, in MPa; F (f,c)w It indicates the flexural strength or compressive strength of specimens of the same age after being immersed in clean water for a certain period of time, in MPa.
[0095] The fast chloride ion migration coefficient method was used to measure the anti-chloride ion penetration performance. A cylinder with a size of ∅100 mm × 50 mm was formed and the chloride ion penetration depth was tested after curing at 20°C and 60% relative humidity for 90 days. The non-steady-state chloride ion migration coefficient D was calculated according to formula (2): RCM , unit is m 2 / s.
[0096]
[0097] Formula (2)
[0098] Where: U is the absolute value of the voltage used (V); T is the average value of the anodic solution's starting and ending temperatures (°C); L is the specimen thickness (mm); X d is the average value of chloride ion penetration depth (mm); t is the test duration (h).
[0099] The test results are shown in Table 2.
[0100] Table 2 Durability test results
[0101]
[0102] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A highly efficient anti-corrosion mortar material, characterized by: The invention comprises the following raw material components in parts by weight: 100-120 parts of cement, 30-80 parts of fly ash, 20-50 parts of slag powder, 80-100 parts of quartz sand, 1-5 parts of water reducer, 1-2 parts of defoamer, 1-2 parts of stabilizer, 20-35 parts of rare earth oxide modified graphene / lacquer phenol acetal resin composite material and 60-90 parts of water; The preparation method of the rare earth oxide modified graphene / lacquer phenol acetal resin composite material comprises the following steps: S1, dissolving urushiol and formaldehyde in a phenyl solvent, adding a catalyst, and reacting at 50-60° C. for 3-6 hours to obtain urushiol acetal resin; S2, dispersing a rare earth oxide precursor in an alcohol solution, adding graphene, ultrasonicating, reacting at 80-120° C. for 2-5 hours to obtain a mixed system; transferring the mixed system to a reactor, performing a hydrothermal reaction at 170-190° C., solid-liquid separation, and drying to obtain rare earth oxide-modified graphene; S3, ball-milling the rare earth oxide modified graphene, adding the urushiol acetal resin, mixing evenly, and drying to obtain the rare earth oxide modified graphene / urushiol acetal resin composite material.
2. The high-efficiency anticorrosive mortar material according to claim 1, characterized in that: The rare earth oxide is cerium oxide or lanthanum oxide.
3. The high-efficiency anticorrosive mortar material according to claim 1, characterized in that: In S1, the mass ratio of urushiol to formaldehyde is 10:2-15:4; and / or In S1, the volume ratio of the urushiol to the phenyl solvent is 1:10-2:15; and / or In S1, the added amount of the catalyst is 0.5%-1% of the mass of the phenyl solvent.
4. The high-efficiency anticorrosive mortar material according to claim 1, characterized in that: In S1, the phenyl solvent is xylene; and / or In S1, the catalyst is a 0.1-0.5 mol / L sodium hydroxide solution.
5. The high-efficiency anticorrosive mortar material according to claim 1, characterized in that: In S2, the rare earth oxide precursor is cerium nitrate or lanthanum nitrate; and / or In S2, the alcohol solution is a 55%-65% ethanol solution; and / or In S2, the mass volume ratio of the rare earth oxide precursor to the alcohol solution is 1g:5mL-1g:8mL; and / or In S2, the mass ratio of the rare earth oxide precursor to the graphene is 1:2-1:
4.
6. The high-efficiency anticorrosive mortar material according to claim 1, characterized in that: In S2, the ultrasonic treatment time is 30min-45min; and / or In S2, the hydrothermal reaction time is 12-20 hours.
7. The high-efficiency anticorrosive mortar material according to claim 1, characterized in that: In S3, the ball milling speed is 600-1000 rpm, and the ball milling time is 2-4 h; and / or In S3, the mass ratio of the rare earth oxide modified graphene to the lacquer phenol acetal resin is 1:15-1:
25.
8. The method for preparing a high-efficiency anticorrosive mortar material according to any one of claims 1 to 7, characterized in that: The method comprises the following steps: weighing various raw material components according to the designed proportion, and uniformly mixing the weighed components to obtain a high-efficiency anticorrosive mortar material.
9. Application of the high-efficiency anti-corrosion mortar material as described in any one of claims 1 to 7 or the high-efficiency anti-corrosion mortar material prepared by the preparation method of the high-efficiency anti-corrosion mortar material as described in claim 8 in the field of building anti-corrosion materials.