A kind of concrete gap quick repair material and preparation method thereof
Patent Information
- Application Number
- CN202411021994.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-07-29
AI Technical Summary
Calcium hydroxide produced during the hydration process of existing concrete gap repair materials will precipitate, resulting in a decrease in strength and affecting the repair effect.
It uses carbon dioxide storage material, adsorbs ammonia borane through zif-8 and then pyrolyzes it, combined with dopamine modification to improve hydrophilicity and stability, and cooperates with a special accelerating agent to absorb carbon dioxide and calcium hydroxide produced during the hydration process to prevent Its precipitation improves the strength and curing speed of concrete repair materials.
It effectively prevents the precipitation of calcium hydroxide, improves the strength and curing speed of concrete repair materials, reduces the curing time, and significantly improves the initial and long-term compressive strength of the repair materials.
Smart Images

Figure CN118545966B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of concrete gap repair materials, and in particular to a concrete gap quick repair material and a preparation method thereof. Background Art
[0002] With the rapid development of my country's national economy, the construction of various highways, bridges and municipal engineering projects has been rapid. Among them, the proportion of cement concrete pavement has increased significantly. Under the repeated effects of loads and the continuous influence of natural environmental factors such as freeze-thaw cycles, salt freezing, carbonization, and the combined effects of many factors such as design, construction, and maintenance, cement concrete pavements will inevitably suffer various damages during use, such as cracks, potholes, and cracks, which affect the speed and quality of traffic and cause traffic problems. In order to minimize traffic problems, damaged pavements must be repaired and repaired in a timely manner.
[0003] Concrete gap repair materials mainly include silicate cement, fine aggregate, coarse aggregate and other additives. Various chemical reactions will occur in the repair materials, among which the hydration reaction of cement is one of the most important reactions. Gels such as hydrated calcium silicate and hydrated calcium aluminate are formed through the hydration reaction to provide support for the strength of the concrete repair material. However, there will be side reactions in the hydration process, such as the production of calcium hydroxide. Although calcium hydroxide can provide a certain alkalinity and has a certain promoting effect on the reaction, more calcium hydroxide will precipitate and produce flaky crystals, which will have a great impact on the strength of the concrete repair material.
[0004] To this end, in response to the problems in the above-mentioned background technology, those skilled in the art have proposed a concrete repair material for solving the problem of calcium hydroxide generated during the hydration process. Summary of the invention
[0005] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a concrete crack quick repair material and a preparation method thereof to solve the problems raised in the above background technology.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] A concrete crack quick repair material comprises the following components by weight: 190-230 parts of ordinary Portland cement, 60-100 parts of special accelerating agent, 10-30 parts of high-performance expansion agent, 280-320 parts of fine aggregate, 330-370 parts of coarse aggregate, 40-70 parts of carbon dioxide storage material, 2-3 parts of polycarboxylic acid water reducing agent, 0.5-1.0 parts of high molecular polymer and 250-350 parts of water.
[0008] Furthermore, the carbon dioxide storage material is prepared by the following steps:
[0009] S101, dissolving zinc nitrate in deionized water, adding 2-methylimidazole to the deionized water containing zinc nitrate, and reacting at room temperature for 8-25 hours to obtain a mixed solution;
[0010] S102, adding dopamine to the mixed solution in step S101, stirring and mixing evenly, then dropping 25% ammonia water until the pH of the mixed solution is 8.5, and continuing the reaction for 2-12 hours. During the reaction, air is introduced into the mixed solution. After the reaction is completed, the filtered product is washed with deionized water and vacuum dried at 120-250° C. to obtain a polydopamine-modified zif-8 material;
[0011] S103, dissolving ammonia borane in deionized water, adding the polydopamine-modified zif-8 material prepared in step S102 to the deionized water containing ammonia borane, stirring and mixing for 1-8 hours, filtering the product, and calcining it in a muffle furnace at a temperature of 500-700° C. for 5-7 hours to obtain a composite material:
[0012] S104, ultrasonically dispersing the composite material obtained in step S103 into a saturated carbon dioxide aqueous solution, stirring the reaction for 1-6 hours, introducing carbon dioxide into the saturated carbon dioxide aqueous solution during the stirring and mixing process, filtering after the reaction is completed, and vacuum drying at 20-30° C. to obtain a carbon dioxide storage material.
[0013] Furthermore, in step S101, the mass ratio of zinc nitrate, 2-methylimidazole and deionized water is 1:(4-18):(40-80).
[0014] Furthermore, the mass ratio of dopamine in step S102 to zinc nitrate in step S101 is 1:(2-6).
[0015] Furthermore, the mass ratio of ammonia borane to deionized water in step S103 is 1:(10-20), and the mass ratio of ammonia borane in step S103 to zinc nitrate used in step S101 is 1:(0.2-0.5).
[0016] Furthermore, the mass ratio of the zinc nitrate in step S101 to the saturated carbon dioxide aqueous solution in step S104 is 1:(20-50).
[0017] Furthermore, the fine aggregate is river sand, the river sand is continuous grade river sand with a particle size of 1-5 mm, and the coarse aggregate is pebbles with a particle size of 10-20 mm.
[0018] Furthermore, the high molecular polymer is one of sodium polyacrylate, polyethylene oxide, and EDDHA-Na, the high-performance expansion agent is one of a calcium expansion agent, a calcium-magnesium composite expansion agent, and calcium stearate, and the special accelerating setting agent is a mixture of amorphous calcium aluminate, sodium sulfate, calcium sulfate dihydrate, and sodium aluminate, and the mass ratio of the amorphous calcium aluminate, sodium sulfate, calcium sulfate dihydrate, and sodium aluminate is 13:4:2:1.
[0019] A preparation method for preparing the above-mentioned concrete crack quick repair material comprises the following steps:
[0020] S1. Put water, carbon dioxide storage material, polycarboxylate water reducer and high molecular polymer into a mixer and mix them evenly according to the proportion to form a mixture A. Put special accelerating setting agent, ordinary Portland cement, high performance expansion agent, fine aggregate and coarse aggregate into a mixer and mix them evenly according to the proportion to form a mixture B.
[0021] S2. Slowly add the mixture B prepared in step S1 into the mixture A prepared in step S1, and stir evenly to obtain a concrete crack quick repair material.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] 1. The present invention adds a carbon dioxide storage material, which absorbs enough carbon dioxide before entering the ingredients. Combined with the autoclaving process commonly used in concrete, the carbon dioxide generated during the autoclaving process combines with the calcium hydroxide generated during the hydration process to prevent the precipitation and crystallization of excessive calcium hydroxide, effectively improving the strength of the concrete repair material;
[0024] 2. The carbon dioxide storage material in the present invention is obtained by pyrolysis of zif-8 after adsorbing ammonia borane. Zif-8 is modified by dopamine to improve its hydrophilicity and stability, and has excellent carbon dioxide adsorption capacity. Combined with the special accelerating setting agent added in the present invention, it can greatly improve the initial hydration rate of concrete and reduce the curing time. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The present invention is a process flow chart for preparing the concrete crack quick repair material;
[0026] Figure 2 This is a process flow chart for preparing the carbon dioxide storage material of the present invention. DETAILED DESCRIPTION
[0027] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] See also Figure 1-2 The present invention provides a concrete crack quick-repairing material, which includes a special accelerating setting agent, which is composed of amorphous calcium aluminate, sodium sulfate, calcium sulfate dihydrate and sodium aluminate. The specific preparation steps are as follows: 65kg of amorphous calcium aluminate, 20kg of sodium sulfate, 10kg of calcium sulfate dihydrate and 5kg of sodium aluminate are sequentially added into a mixer and mixed evenly. By adding the special accelerating setting agent, the curing speed of the concrete crack repairing material is improved.
[0029] Example 1
[0030] A concrete crack quick repair material is prepared by the following method:
[0031] S1, 32kg of water, 6kg of carbon dioxide storage material, 0.3kg of polycarboxylate water reducer and 0.1kg of sodium polyacrylate were put into a mixer and mixed evenly to form a mixture A, 8.5kg of special quick-setting agent, 21kg of ordinary Portland cement, 2.5kg of calcium expansion agent, 31kg of river sand fine aggregate with a particle size of 5mm and 34kg of pebble coarse aggregate with a particle size of 20mm were put into a mixer and mixed evenly to form a mixture B;
[0032] S2, slowly adding the mixture B prepared in step S1 into the mixture A prepared in step S1, stirring evenly, to obtain a concrete crack quick repair material;
[0033] The above carbon dioxide storage material is prepared by the following steps:
[0034] S101, dissolving 4 kg of zinc nitrate in 300 kg of deionized water, adding 35 kg of 2-methylimidazole to the deionized water containing zinc nitrate, and reacting at room temperature for 20 hours to obtain a mixed solution;
[0035] S102, adding 2 kg of dopamine to the mixed solution in step S101, stirring and mixing evenly, then dropping 25% ammonia water until the pH of the mixed solution is 8.5, and continuing the reaction for 7 hours. During the reaction, air is introduced into the mixed solution. After the reaction is completed, the filtered product is washed with deionized water and vacuum dried at 240° C. to obtain a polydopamine-modified zif-8 material;
[0036] S103, dissolving 14 kg of ammonia borane in 250 kg of deionized water, adding the polydopamine-modified zif-8 material prepared in step S102 to the deionized water containing ammonia borane, stirring and mixing for 4 hours, filtering the product, and calcining it in a muffle furnace at a temperature of 700° C. for 7 hours to obtain a composite material;
[0037] S104, ultrasonically dispersing the composite material obtained in step S103 into 120 kg of saturated carbon dioxide aqueous solution, stirring and reacting for 5 hours, introducing carbon dioxide into the saturated carbon dioxide aqueous solution during the stirring and mixing process, filtering and vacuum drying at 30° C. after the reaction is completed, to obtain a carbon dioxide storage material.
[0038] Example 2
[0039] A concrete crack quick repair material is prepared by the following method:
[0040] S1, 35kg of water, 7kg of carbon dioxide storage material, 0.3kg of polycarboxylate water reducer and 0.1kg of polyethylene oxide were put into a mixer and mixed evenly to form a mixture A, 10kg of special quick-setting agent, 23kg of ordinary Portland cement, 3kg of calcium-magnesium composite expansion agent, 32kg of river sand fine aggregate with a particle size of 5mm and 37kg of pebble coarse aggregate with a particle size of 20mm were put into a mixer and mixed evenly to form a mixture B;
[0041] S2, slowly adding the mixture B prepared in step S1 into the mixture A prepared in step S1, stirring evenly, to obtain a concrete crack quick repair material;
[0042] The above carbon dioxide storage material is prepared by the following steps:
[0043] S101, dissolving 4 kg of zinc nitrate in 320 kg of deionized water, adding 72 kg of 2-methylimidazole to the deionized water containing zinc nitrate, and reacting at room temperature for 25 hours to obtain a mixed solution;
[0044] S102, adding 0.7 kg of dopamine to the mixed solution in step S101, stirring and mixing evenly, and then dropping 25% by mass of ammonia water until the pH of the mixed solution is 8.5, and continuing the reaction for 12 hours. During the reaction, air is introduced into the mixed solution. After the reaction is completed, the filtered product is washed with deionized water and vacuum dried at 250° C. to obtain a polydopamine-modified zif-8 material;
[0045] S103, dissolving 20 kg of ammonia borane in 400 kg of deionized water, adding the polydopamine-modified zif-8 material prepared in step S102 to the deionized water containing ammonia borane, stirring and mixing for 8 hours, filtering the product, and calcining it in a muffle furnace at a temperature of 700° C. for 7 hours to obtain a composite material;
[0046] S104, ultrasonically dispersing the composite material obtained in step S103 into 200 kg of saturated carbon dioxide aqueous solution, stirring and reacting for 6 hours, introducing carbon dioxide into the saturated carbon dioxide aqueous solution during the stirring and mixing process, filtering and vacuum drying at 30° C. after the reaction is completed, to obtain a carbon dioxide storage material.
[0047] Example 3
[0048] A concrete crack quick repair material is prepared by the following method:
[0049] S1, 31kg of water, 5.5kg of carbon dioxide storage material, 0.25kg of polycarboxylate water reducer and 0.08kg of EDDHA-Na were put into a mixer and mixed evenly to form a mixture A, 7kg of special quick-setting agent, 20kg of ordinary Portland cement, 2.6kg of calcium-magnesium composite expansion agent, 30kg of river sand fine aggregate with a particle size of 4mm and 35kg of pebble coarse aggregate with a particle size of 15mm were put into a mixer and mixed evenly to form a mixture B;
[0050] S2, slowly adding the mixture B prepared in step S1 into the mixture A prepared in step S1, stirring evenly, to obtain a concrete crack quick repair material;
[0051] The above carbon dioxide storage material is prepared by the following steps:
[0052] S101, dissolving 4 kg of zinc nitrate in 250 kg of deionized water, adding 40 kg of 2-methylimidazole to the deionized water containing zinc nitrate, and reacting at room temperature for 16 hours to obtain a mixed solution;
[0053] S102, adding 1.2 kg of dopamine to the mixed solution in step S101, stirring and mixing evenly, then dropping 25% ammonia water until the pH of the mixed solution is 8.5, and continuing the reaction for 9 hours. During the reaction, air is introduced into the mixed solution. After the reaction is completed, the filtered product is washed with deionized water and vacuum dried at 200° C. to obtain a polydopamine-modified zif-8 material;
[0054] S103, dissolving 16 kg of ammonia borane in 240 kg of deionized water, adding the polydopamine-modified zif-8 material prepared in step S102 to the deionized water containing ammonia borane, stirring and mixing for 7 hours, filtering the product, and calcining it in a muffle furnace at a temperature of 650° C. for 6 hours to obtain a composite material;
[0055] S104, ultrasonically dispersing the composite material obtained in step S103 into 160 kg of saturated carbon dioxide aqueous solution, stirring and reacting for 4 hours, introducing carbon dioxide into the saturated carbon dioxide aqueous solution during the stirring and mixing process, filtering and vacuum drying at 28° C. after the reaction is completed, to obtain a carbon dioxide storage material.
[0056] Example 4
[0057] A concrete crack quick repair material is prepared by the following method:
[0058] S1, 25kg of water, 4kg of carbon dioxide storage material, 0.2kg of polycarboxylate water reducer and 0.05kg of sodium polyacrylate were put into a mixer and mixed evenly to form a mixture A, 6kg of special quick-setting agent, 19kg of ordinary Portland cement, 1kg of calcium stearate, 28kg of river sand fine aggregate with a particle size of 1mm and 33kg of pebble coarse aggregate with a particle size of 10mm were put into a mixer and mixed evenly to form a mixture B;
[0059] S2, slowly adding the mixture B prepared in step S1 into the mixture A prepared in step S1, stirring evenly, to obtain a concrete crack quick repair material;
[0060] The above carbon dioxide storage material is prepared by the following steps:
[0061] S101, dissolving 4 kg of zinc nitrate in 40 kg of deionized water, adding 16 kg of 2-methylimidazole to the deionized water containing zinc nitrate, and reacting at room temperature for 8 hours to obtain a mixed solution;
[0062] S102, adding 2 kg of dopamine to the mixed solution in step S101, stirring and mixing evenly, then dropping 25% ammonia water until the pH of the mixed solution is 8.5, and continuing the reaction for 2 h. During the reaction, air is introduced into the mixed solution. After the reaction is completed, the filtered product is washed with deionized water and vacuum dried at 120° C. to obtain a polydopamine-modified zif-8 material;
[0063] S103, dissolving 8 kg of ammonia borane in 80 kg of deionized water, adding the polydopamine-modified zif-8 material prepared in step S102 to the deionized water containing ammonia borane, stirring and mixing for 1 hour, filtering the product, and calcining it in a muffle furnace at a temperature of 500° C. for 5 hours to obtain a composite material;
[0064] S104, ultrasonically dispersing the composite material obtained in step S103 into 80 kg of saturated carbon dioxide aqueous solution, stirring and reacting for 1 hour, introducing carbon dioxide into the saturated carbon dioxide aqueous solution during the stirring and mixing process, filtering and vacuum drying at 20° C. after the reaction is completed, to obtain a carbon dioxide storage material.
[0065] Example 5
[0066] A concrete crack quick repair material is prepared by the following method:
[0067] S1, 35kg of water, 6kg of carbon dioxide storage material, 0.3kg of polycarboxylate water reducer and 0.1kg of sodium polyacrylate were put into a mixer and mixed evenly to form a mixture A, 9kg of special quick-setting agent, 22kg of ordinary Portland cement, 2.5kg of calcium-magnesium composite expansion agent, 32kg of river sand fine aggregate with a particle size of 3mm and 36kg of pebble coarse aggregate with a particle size of 15mm were put into a mixer and mixed evenly to form a mixture B;
[0068] S2, slowly adding the mixture B prepared in step S1 into the mixture A prepared in step S1, stirring evenly, to obtain a concrete crack quick repair material;
[0069] The above carbon dioxide storage material is prepared by the following steps:
[0070] S101, dissolving 4 kg of zinc nitrate in 180 kg of deionized water, adding 35 kg of 2-methylimidazole to the deionized water containing zinc nitrate, and reacting at room temperature for 20 hours to obtain a mixed solution;
[0071] S102, adding 2 kg of dopamine to the mixed solution in step S101, stirring and mixing evenly, then dropping 25% ammonia water until the pH of the mixed solution is 8.5, and continuing the reaction for 9 hours. During the reaction, air is introduced into the mixed solution. After the reaction is completed, the filtered product is washed with deionized water and vacuum dried at 230° C. to obtain a polydopamine-modified zif-8 material;
[0072] S103, dissolving 12 kg of ammonia borane in 190 kg of deionized water, adding the polydopamine-modified zif-8 material prepared in step S102 to the deionized water containing ammonia borane, stirring and mixing for 6 hours, filtering the product, and calcining it in a muffle furnace at a temperature of 600° C. for 5 hours to obtain a composite material:
[0073] S104, ultrasonically dispersing the composite material obtained in step S103 into 180 kg of saturated carbon dioxide aqueous solution, stirring and reacting for 5 hours, introducing carbon dioxide into the saturated carbon dioxide aqueous solution during the stirring and mixing process, filtering and vacuum drying at 20° C. after the reaction is completed, to obtain a carbon dioxide storage material.
[0074] Comparative Example 1
[0075] The difference between Comparative Example 1 and Example 1 is that step S102 is omitted, thereby eliminating the addition of dopamine, and the remaining steps are exactly the same as those of Example 1.
[0076] Comparative Example 2
[0077] The difference between Comparative Example 2 and Example 1 is that step S104 is omitted, thereby eliminating the process of immersing the composite material in a saturated carbon dioxide solution, and the remaining steps are exactly the same as those in Example 1.
[0078] Comparative Example 3
[0079] The difference between Comparative Example 3 and Comparative Example 2 is that step S102 is omitted, thereby canceling the addition of dopamine, and the remaining steps are exactly the same as those of Comparative Example 2.
[0080] Eight portions of concrete crack quick repair materials were prepared through the above-mentioned embodiments 1-5 and comparative examples 1-3, respectively. After initial setting, each concrete crack quick repair material was autoclaved and cured at a temperature of 60° C. The 1d compressive strength, 2d compressive strength and 20d compressive strength of each concrete crack quick repair material were measured. The measurement standard was based on GB / T 50080-2001 "Standard for Test Methods for Performance of Ordinary Concrete Mixtures". The measurement results are shown in Table 1 below:
[0081] Table 1: Test table of concrete gap quick repair material in various implementation methods
[0082]
[0083] It can be seen from the data of Examples 1-5 in Table 1 above that after adding the carbon dioxide storage material, the 1d compressive strength of the present invention under autoclaving all reaches more than 40MPa, the 2d compressive strength all reaches more than 60MPa, and the 20d compressive strength all reaches more than 100MPa. By comparing Comparative Example 2 with Example 1, it can be seen that after the composite material in the present invention is immersed in a saturated carbon dioxide solution, the concrete curing strength is improved. By comparing Comparative Example 1 with Example 1, it can be seen that the ZIF-8 material also improves the concrete curing strength after being modified by polydopamine.
[0084] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A concrete crack quick repair material, characterized in that: The following components are included by mass: 190-230 parts of ordinary Portland cement, 60-100 parts of special accelerating agent, 10-30 parts of high-performance expansion agent, 280-320 parts of fine aggregate, 330-370 parts of coarse aggregate, 40-70 parts of carbon dioxide storage material, 2-3 parts of polycarboxylate water reducer, 0.5-1.0 parts of high molecular polymer, and 250-350 parts of water; The carbon dioxide storage material is prepared by the following steps: S101, dissolving zinc nitrate in deionized water, adding 2-methylimidazole to the deionized water containing zinc nitrate, and reacting at room temperature for 8-25 hours to obtain a mixed solution; S102, adding dopamine to the mixed solution in step S101, stirring and mixing evenly, then dropping 25% ammonia water until the pH of the mixed solution is 8.5, and continuing the reaction for 2-12 hours. During the reaction, air is introduced into the mixed solution. After the reaction is completed, the filtered product is washed with deionized water and vacuum dried at 120-250° C. to obtain a polydopamine-modified zif-8 material; S103, dissolving ammonia borane in deionized water, adding the polydopamine-modified zif-8 material prepared in step S102 to the deionized water containing ammonia borane, stirring and mixing for 1-8 hours, filtering the product, and calcining it in a muffle furnace at a temperature of 500-700° C. for 5-7 hours to obtain a composite material: S104, ultrasonically dispersing the composite material obtained in step S103 into a saturated carbon dioxide aqueous solution, stirring the mixture for reaction for 1-6 hours, introducing carbon dioxide into the saturated carbon dioxide aqueous solution during the stirring and mixing process, filtering the mixture after the reaction is completed, and vacuum drying the mixture at 20-30° C. to obtain a carbon dioxide storage material; The high molecular polymer is one of sodium polyacrylate and polyethylene oxide; The high-performance expansion agent is one of a calcium expansion agent and a calcium-magnesium composite expansion agent; The special accelerating agent is formed by mixing amorphous calcium aluminate, sodium sulfate, calcium sulfate dihydrate and sodium aluminate, and the mass ratio of the amorphous calcium aluminate, sodium sulfate, calcium sulfate dihydrate and sodium aluminate is 13:4:2:1; In the step S101, the mass ratio of zinc nitrate, 2-methylimidazole and deionized water is 1:(4-18):(40-80); The mass ratio of ammonia borane in step S103 to zinc nitrate used in step S101 is 1:(0.2-0.5).
2. A concrete crack quick repair material according to claim 1, characterized in that: The mass ratio of dopamine in step S102 to zinc nitrate in step S101 is 1:(2-6).
3. A concrete crack quick repair material according to claim 1, characterized in that: In step S103, the mass ratio of ammonia borane to deionized water is 1:(10-20).
4. A concrete crack quick repair material according to claim 1, characterized in that: The mass ratio of the zinc nitrate in step S101 to the saturated carbon dioxide aqueous solution in step S104 is 1:(20-50).
5. A concrete crack quick repair material according to claim 1, characterized in that: The fine aggregate is river sand, and the river sand is continuous grade river sand with a particle size of 1-5 mm; The coarse aggregate is pebbles with a particle size of 10-20 mm.
6. A method for preparing a concrete crack quick repair material as claimed in any one of claims 1 to 5, characterized in that: Use the following steps: S1. Put water, carbon dioxide storage material, polycarboxylate water reducer and high molecular polymer into a mixer and mix them evenly according to the proportion to form a mixture A. Put special accelerating setting agent, ordinary Portland cement, high performance expansion agent, fine aggregate and coarse aggregate into a mixer and mix them evenly according to the proportion to form a mixture B. S2. Slowly add the mixture B prepared in step S1 into the mixture A prepared in step S1, and stir evenly to obtain a concrete crack quick repair material.
Citation Information
Patent Citations
Preparation method of composite lubricating material
CN113621420A
Preparation method of porous nano composite material and application of porous nano composite material in hydrogen production through hydrolysis of ammonia borane
CN115041209A
Preparation method of composite antibacterial cementing material
CN115724604A