A bio-based flame retardant toughening curing agent and its preparation method and application

By introducing a bio-based flame retardant and toughening curing agent into epoxy resin, and utilizing the chemical structure of its long-chain alkyl and phosphorus groups, the problem of flammability and brittleness of epoxy resin is solved, and its flame retardant and mechanical properties are significantly improved. , achieving efficient flame retardant modification and industrial application.

CN118546175BActive Publication Date: 2024-10-11UNIV OF SCI & TECH OF CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411014768.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-10-11
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

Existing epoxy resin materials are flammable and brittle, and the addition of flame retardants reduces their tensile and impact properties, making them difficult to be widely used in high-tech fields.

Method used

Develop a bio-based flame retardant and toughening curing agent. Its chemical structure contains long-chain alkyl and phosphorus groups, which can significantly improve the flame retardant properties of the polymer and participate in the curing reaction of epoxy resin through multiple active hydroxyl functional groups. , improve cross-linking density and mechanical properties. The curing agent is composed of a phosphorus-containing compound and 2-acrylic acid-(2-hydroxy-1,3-propylene)bis[oxy(2-hydroxy-3,1-propylene)] ester reacted under inert gas protection Preparation, suitable for flame retardant and toughening modification of epoxy resin.

Benefits of technology

It significantly improves the limiting oxygen index of epoxy resin, reaches V-0 level vertical combustion, improves its tensile and impact resistance, overcomes the shortcomings of brittleness and flame retardant properties, and is suitable for industrial production and application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118546175B_ABST
    Figure CN118546175B_ABST
Patent Text Reader

Abstract

The present invention discloses a bio-based flame retardant toughening curing agent and a preparation method and application thereof, and belongs to the technical field of flame retardant toughening curing agents. The chemical structure of the bio-based flame retardant toughening curing agent of the present invention is shown in formula (I): #imgabs0#; wherein R is a phosphorus-containing group. The long-chain alkyl group in the structure of the bio-based flame retardant toughening curing agent of the present invention has a toughening function, and the introduction of the phosphorus-containing group can significantly improve the flame retardant properties of the polymer matrix, and the phosphorus content and the number of aromatic rings can be adjusted, which is suitable for flame retardant toughening modification of epoxy resin. In addition, the curing agent structure contains multiple active hydroxyl functional groups, which can participate in the epoxy resin curing reaction as a co-curing agent, improve the cross-linking density, and thus play a role in enhancing mechanical properties. When the bio-based flame retardant toughening curing agent of the present invention is applied to epoxy resin, the limiting oxygen index is significantly improved, the vertical combustion reaches V-0 level, and it has the advantages of excellent tensile and impact resistance, high flame retardant efficiency, etc.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of flame retardant toughening curing agents, and specifically relates to a bio-based flame retardant toughening curing agent and a preparation method and application thereof. Background Art

[0002] As a commonly used thermosetting resin material, epoxy resin has low production cost and excellent electrical insulation, chemical stability, adhesion, mechanical properties and other advantages. Therefore, it has been widely used in high-tech fields such as coatings and adhesives, integrated circuits, transportation, aerospace, etc. However, as an organic polymer, epoxy resin contains a large amount of carbon, hydrogen, and oxygen elements in its structure, so it is flammable and releases a large amount of smoke during combustion, which seriously limits the expansion of its application field. At present, the most commonly used epoxy resin is bisphenol A epoxy resin (DGEBA). Although DGEBA epoxy resin has the above advantages, it still has disadvantages such as flammability and high brittleness, which limits its application range. Therefore, it is of great significance to simultaneously modify epoxy resin for flame retardancy and toughening.

[0003] In recent years, the flame retardant modification of epoxy resin using phosphorus flame retardants has become one of the research hotspots in the field of flame retardancy. Bio-based organophosphorus flame retardants have the advantages of low toxicity, low cost, and high flame retardant efficiency, and have been widely studied and developed in recent years. Wang Zhengzhou's research group at Tongji University used phytic acid, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO) and other raw materials to synthesize a bio-based organophosphorus flame retardant, and applied it to DGEBA-type epoxy resin and cyanate resin copolymers, but the addition of flame retardants will reduce the tensile and impact properties of epoxy resin and cyanate resin copolymers. Hu Yuan's research group at the University of Science and Technology of China used vanillin, DOPO and other raw materials to synthesize a bio-based phosphorus-containing flame retardant, and applied it to DGEBA-type epoxy resin for flame retardant modification. The epoxy composite material has excellent flame retardant properties at a low addition amount and low phosphorus content. However, the addition of flame retardants reduces the impact strength of epoxy composite materials and cannot overcome the disadvantage of DGEBA-type epoxy resin's brittleness.

[0004] Therefore, the development of new bio-based flame retardant curing agents that are green, environmentally friendly, highly flame retardant, and have low additive amounts for the preparation of new flame retardant epoxy resin materials with excellent flame retardancy and high toughness has become an urgent need in the field of flame retardant epoxy resin technology. Summary of the invention

[0005] In view of the above-mentioned deficiencies of the prior art, the present invention provides a bio-based flame retardant toughening curing agent and a preparation method and application thereof. When the bio-based flame retardant toughening curing agent of the present invention is applied to epoxy resin, the limiting oxygen index is significantly improved, the vertical combustion reaches V-0 level, and it has the advantages of excellent tensile and impact resistance, high flame retardant efficiency, etc.

[0006] The bio-based flame retardant toughening curing agent of the present invention has a chemical structure as shown in the following formula (I):

[0007] .

[0008] In formula (I), R is selected from any one of the following structures:

[0009] .

[0010] The long-chain alkyl in the structure of the bio-based flame retardant toughening curing agent of the present invention has a toughening function, and the introduction of phosphorus-containing groups can significantly improve the flame retardant properties of the polymer matrix, and the phosphorus content and the number of aromatic rings can be adjusted, which is suitable for flame retardant toughening modification of epoxy resin. In addition, the curing agent structure contains multiple active hydroxyl functional groups, which can participate in the epoxy resin curing reaction as a co-curing agent to increase the crosslinking density, thereby playing a role in enhancing mechanical properties. In addition, the preparation process of the bio-based flame retardant toughening curing agent is simple, the conditions are relatively mild, the yield is high, and it is suitable for industrial production and application.

[0011] The preparation method of the bio-based flame retardant toughening curing agent of the present invention comprises the following steps:

[0012] Under the protection of inert gas, the phosphorus-containing compound A and 2-acrylic acid-(2-hydroxy-1,3-propylene)di[oxy(2-hydroxy-3,1-propylene)]ester are stirred and mixed uniformly in a reactor according to a certain molar ratio, and then heated to 150-200° C. and reacted for 2-24 hours to obtain the target product.

[0013] The phosphorus-containing compound A is any one of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, diphenylphosphine, diphenyl phosphite, dibenzyl phosphite, dimethyl phosphite, diethyl phosphite, di-n-butyl phosphite and di-tert-butyl phosphite.

[0014] The molar ratio of 2-acrylic acid-(2-hydroxy-1,3-propylene)di[oxy(2-hydroxy-3,1-propylene)]ester to the phosphorus-containing compound A is 1:(1.8-2.0).

[0015] The inert gas is any one of nitrogen, argon or helium.

[0016] The application of the bio-based flame retardant toughening curing agent of the present invention is to mix the bio-based flame retardant toughening curing agent with epoxy resin, and prepare a flame retardant epoxy resin sample after curing.

[0017] The added amount of the bio-based flame retardant toughening curing agent is 2-20% of the total mass of the epoxy curing system.

[0018] During the curing process, the bio-based flame retardant toughening curing agent of the present invention can partially replace the conventional curing agent or completely replace it.

[0019] The above raw material components also include various conventional auxiliary agents.

[0020] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0021] 1. The flame retardant curing agent provided by the present invention is synthesized from bio-based raw materials, and the phosphorus content and the number of aromatic rings in the chemical structure are controllable. The introduction of phosphorus-containing groups can significantly improve the flame retardant properties of the epoxy resin matrix.

[0022] 2. The bio-based flame retardant curing agent provided by the present invention contains multiple hydroxyl functional groups in its structure, which can participate in the curing reaction of epoxy resin by covalent bonding, increase the cross-linking density, thereby playing a role in improving mechanical properties, and can overcome the shortcomings of additive flame retardants such as poor compatibility with epoxy matrices and easy migration and precipitation.

[0023] 3. The bio-based flame retardant curing agent provided by the present invention has a relatively long aliphatic molecular chain in its chemical structure, has a good plasticizing effect, and can simultaneously improve the impact resistance of epoxy resin.

[0024] Therefore, the structure of the curing agent of the present application has multiple active functional groups, long-chain alkyl groups and phosphorus elements with adjustable oxidation states, which solves the problem of simultaneously improving the strength, toughness and flame retardancy of epoxy resin. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0026] Figure 1 3 and 4 are thermogravimetric analysis curves of the samples in Example 5, Example 6, Example 7 and Comparative Example 1 of the present invention.

[0027] Figure 2 1 is the heat release rate curve of each sample in Example 5, Example 6, Example 7 and Comparative Example 1 of the present invention.

[0028] Figure 3 This is the total heat release curve of each sample in Example 5, Example 6, Example 7 and Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0029] In order to further illustrate the technical solution of the present invention, the preferred embodiments of the present invention are described below in conjunction with examples, but it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention. Based on the examples in the present invention, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention. Example 1

[0030] 2-Acrylic acid-(2-hydroxy-1,3-propylene)di[oxy(2-hydroxy-3,1-propylene)]ester and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide were mixed with magnetic stirring for 5 to 10 minutes at a molar ratio of 1:2.0 under nitrogen protection. The mixture was heated to 160°C and reacted for 24 hours to obtain the target product a, whose chemical structure is shown below:

[0031]

[0032] The target product a was analyzed by Fourier transform infrared spectroscopy (FT-IR), nuclear magnetic resonance spectroscopy ( 1 H-NMR) characterization confirmed its chemical structure as follows: FT-IR (KBr, cm -1 ): 905 (POC), 1040 (COC), 1115 (PC&P-O), 1172 (P=O), 1385 (-CH 2 -), 1625 (Ar-Ar), 1740 (C=O), 2861 (-CH 2 -), 3428 (OH). 1 H-NMR (300 MHz, DMSO-d 6 , ppm): 2.36 (s, 4H, (PC-CH 2 ) 2 ), 2.67 (s, 4H, (P-CH 2 ) 2 ), 3.87-3.19 (m, 9H, (CH 2 -O-CH 2 ) 2 &C-OC-CH), 4.31-4.00 (m, 6H, (COO-CH 2 -CH)2 ), , 3.74-3.67 (t, 2H, Ar-CH 2 -Ar), 5.09 (s, 3H, -OH), 7.97-7.20 (m, 20H, Ar-H). Example 2

[0033] 2-Acrylic acid-(2-hydroxy-1,3-propylene)di[oxy(2-hydroxy-3,1-propylene)]ester and diphenylphosphine oxide were mixed with a molar ratio of 1:2.0 under nitrogen protection and magnetic stirring for 5 to 10 minutes. The above mixture was heated to 160°C and reacted for 12 hours to obtain the target product b, whose chemical structure is shown below:

[0034]

[0035] The target product b was analyzed by Fourier transform infrared spectroscopy (FT-IR), nuclear magnetic resonance spectroscopy ( 1 H-NMR) characterization confirmed its chemical structure as follows: FT-IR (KBr, cm -1 ): 1055 (COC), 1118 (PC), 1180 (P=O), 1386 (-CH 2 -), 1615 (Ar-Ar), 1735 (C=O), 2865 (-CH 2 -), 3430 (OH). 1 H-NMR (300 MHz, DMSO-d 6 , ppm): 2.79 (m, 4H, C-CH 2 -CO), 2.95 (m, 4H, -CH 2 -P), 3.50-4.33 (m,12H, O-CH 2 -C), 4.00-4.39 (m, 3H, CH-O), 5.77 (s, 3H, -OH), 7.50-7.75 (m, 20H, Ar). Example 3

[0036] 2-Acrylic acid-(2-hydroxy-1,3-propylene)di[oxy(2-hydroxy-3,1-propylene)]ester and diphenyl phosphite were mixed with magnetic stirring for 5-10 minutes at a molar ratio of 1:2.0 under nitrogen protection. The mixture was heated to 150°C and reacted for 24 hours to obtain the target product c, whose chemical structure is shown below:

[0037]

[0038] The target product c was characterized by Fourier transform infrared spectroscopy (FT-IR), nuclear magnetic resonance spectroscopy ( 1 H-NMR) characterization confirmed its chemical structure as follows: FT-IR (KBr, cm -1 ): 908 (POC), 1046 (COC), 1115 (PC&P-O), 1164 (P=O), 1378 (-CH 2 -), 1615 (Ar-Ar), 1742 (C=O), 2865 (-CH 2 -), 3435 (OH). 1 H-NMR (300 MHz, DMSO-d 6 , ppm): 2.49 (m, 4H, C-CH 2 -CO), 2.16 (m, 4H, -CH 2 -P), 3.50-4.33 (m, 12H, O-CH 2 -C), 4.00-4.39 (m, 3H, CH-O), 5.77 (s, 3H, -OH), 7.21-7.40 (m, 20H, Ar). Example 4

[0039] 2-Acrylic acid-(2-hydroxy-1,3-propylene)di[oxy(2-hydroxy-3,1-propylene)]ester and dimethyl phosphite were mixed with magnetic stirring for 5-10 minutes at a molar ratio of 1:2.0 under nitrogen protection. The above mixture was heated to 150°C and reacted for 24 hours to obtain the target product d, whose chemical structure is shown below:

[0040]

[0041] The target product d was characterized by Fourier transform infrared spectroscopy (FT-IR), nuclear magnetic resonance spectroscopy ( 1 H-NMR) characterization confirmed its chemical structure as follows: FT-IR (KBr, cm -1 ): 907 (POC), 1052 (COC), 1118 (PC&P-O), 1188 (P=O), 1385 (-CH 2 -), 1738 (C=O), 2861 (-CH 2 -), 2960 (-CH 3 ), 3455 (OH). 1 H-NMR (300 MHz, DMSO-d 6, ppm): 2.49 (m, 4H, C-CH 2 -CO), 2.16 (m, 4H, -CH 2 -P), 3.50-4.33 (m, 12H, O-CH 2 -C), 3.65 (s, 12H, -O-CH 3 ), 4.00-4.39 (m, 3H, CH-O), 5.77 (s, 3H, -OH). Example 5

[0042] 100.0 g of DGEBA epoxy resin (brand: E-44) and 8.1 g of flame retardant toughening agent curing agent a were added to a three-necked flask, heated to 150°C, mechanically stirred and mixed for 20 minutes to obtain an epoxy resin dispersion; 20.2 g of curing agent 4, 4'-diaminodiphenylmethane was added to the above epoxy resin dispersion, heated to 80°C, mechanically stirred and mixed for 10 minutes, and immediately poured into the mold. The curing conditions were 100°C / 2 hours + 150°C / 2 hours. After demolding, it was naturally cooled to room temperature to obtain a flame retardant epoxy resin sample. Example 6

[0043] 100.0 g of DGEBA epoxy resin (brand: E-44) and 17.1 g of flame retardant toughening agent curing agent a were added to a three-necked flask, heated to 150°C, mechanically stirred and mixed for 20 minutes to obtain an epoxy resin dispersion; 18.5 g of curing agent 4, 4'-diaminodiphenylmethane was added to the above epoxy resin dispersion, heated to 80°C, mechanically stirred and mixed for 10 minutes, and immediately poured into the mold. The curing conditions were 100°C / 2 hours + 150°C / 2 hours. After demolding, it was naturally cooled to room temperature to obtain a flame retardant epoxy resin sample. Example 7

[0044] 100.0 g of DGEBA epoxy resin (brand: E-44) and 27.1 g of flame retardant toughening agent curing agent a were added to a three-necked flask, heated to 150°C, mechanically stirred and mixed for 20 minutes to obtain an epoxy resin dispersion; 16.6 g of curing agent 4, 4'-diaminodiphenylmethane was added to the above epoxy resin dispersion, heated to 80°C, mechanically stirred and mixed for 10 minutes, and immediately poured into the mold. The curing conditions were 100°C / 2 hours + 150°C / 2 hours. After demolding, it was naturally cooled to room temperature to obtain a flame retardant epoxy resin sample. Example 8

[0045] 100.0 g of DGEBA epoxy resin (brand: E-44) and 16.4 g of flame retardant toughening agent curing agent b were added to a three-necked flask, heated to 150°C, mechanically stirred and mixed for 20 minutes to obtain an epoxy resin dispersion; 18.5 g of curing agent 4, 4'-diaminodiphenylmethane was added to the above epoxy resin dispersion, heated to 80°C, mechanically stirred and mixed for 10 minutes, and immediately poured into the mold. The curing conditions were 100°C / 2 hours + 150°C / 2 hours. After demolding, it was naturally cooled to room temperature to obtain a flame retardant epoxy resin sample. Example 9

[0046] 100.0 g of DGEBA epoxy resin (brand: E-44) and 18.0 g of flame retardant toughening agent curing agent c were added to a three-necked flask, heated to 150°C, mechanically stirred and mixed for 20 minutes to obtain an epoxy resin dispersion; 18.5 g of curing agent 4, 4'-diaminodiphenylmethane was added to the above epoxy resin dispersion, heated to 80°C, mechanically stirred and mixed for 10 minutes, and immediately poured into a mold. The curing conditions were 100°C / 2 hours + 150°C / 2 hours. After demolding, it was naturally cooled to room temperature to obtain a flame retardant epoxy resin sample. Example 10

[0047] 100.0 g of DGEBA epoxy resin (brand: E-44) and 12.0 g of flame retardant toughening agent curing agent d were added to a three-necked flask, heated to 150°C, mechanically stirred and mixed for 20 minutes to obtain an epoxy resin dispersion; 18.6 g of curing agent 4, 4'-diaminodiphenylmethane was added to the above epoxy resin dispersion, heated to 80°C, mechanically stirred and mixed for 10 minutes, and immediately poured into a mold. The curing conditions were 100°C / 2 hours + 150°C / 2 hours. After demolding, it was naturally cooled to room temperature to obtain a flame retardant epoxy resin sample. Comparative Example 1

[0048] 100.0 g of DGEBA epoxy resin (brand: E-44) and 21.8 g of curing agent 4, 4'-diaminodiphenylmethane were added to a three-necked flask, heated to 80°C, mechanically stirred and mixed for 10 minutes, and immediately poured into the mold. The curing conditions were 100°C / 2 hours + 150°C / 2 hours. After demolding, the mixture was naturally cooled to room temperature to obtain an epoxy resin sample. Comparative Example 2

[0049] 100.0 g of DGEBA epoxy resin (brand: E-44) and 30.5 g of aluminum hydroxide powder were added to a three-necked flask, heated to 100°C, and mechanically stirred for 30 minutes; then 21.8 g of curing agent 4, 4'-diaminodiphenylmethane was added, and mechanical stirring was continued for 10 minutes, and immediately poured into the mold, and the curing conditions were 100°C / 2 hours + 150°C / 2 hours. After demolding, it was naturally cooled to room temperature to obtain a flame-retardant epoxy resin sample. Comparative Example 3

[0050] 100.0 g of DGEBA epoxy resin (brand: E-44) and 13.7 g of 10-(2, 5-dihydroxyphenyl)-10-hydrogen-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO-HQ) were added to a three-necked flask, heated to 100°C, and mechanically stirred for 30 minutes; then 17.6 g of curing agent 4, 4'-diaminodiphenylmethane was added, and mechanical stirring was continued for 10 minutes, and immediately poured into the mold, and the curing conditions were 100°C / 2 hours + 150°C / 2 hours. After demolding, it was naturally cooled to room temperature to obtain a flame-retardant epoxy resin sample.

[0051] The performance test results of the epoxy resins obtained in the above embodiments and comparative examples are as follows:

[0052] Table 1 Oxygen index, vertical combustion, tensile and impact test results of flame retardant epoxy resin

[0053]

[0054] The flame retardant test results of each sample in Table 1 show that the oxygen index of the unmodified DGEBA epoxy resin is 23.5%, the UL-94 vertical combustion test has no level, and the tensile strength is 41.9 MPa (Comparative Example 1). The oxygen index of the epoxy resin with flame retardant curing agent a with 0.5 wt% phosphorus content (Example 5), 1.0 wt% phosphorus content (Example 6) and 1.5 wt% phosphorus content (Example 7) respectively increased to 31.5%, 34.0% and 35.0%, and the results of the UL-94 vertical combustion test were V-1, V-0 and V-0 respectively. The tensile strength of the samples in Examples 5, 6 and 7 reached 70.6, 85.5 and 76.6 MPa respectively, which were greatly improved compared with the unmodified epoxy resin (Comparative Example 1). This is because the molecular structure of flame retardant curing agent a contains multiple hydroxyl groups, which participate in the curing reaction and improve the crosslinking density of the system. The impact strengths of the samples in Examples 5, 6 and 7 were 23.6, 25.4 and 30.0 kJ / m respectively. 2, which is significantly improved compared with the unmodified epoxy resin (Comparative Example 1). This is because the flame retardant curing agent a contains a long alkyl molecular chain in its molecular structure, which has a good toughening effect. In addition, by changing the type of flame retardant curing agent, the oxygen index of the epoxy resin of adding 1.0 wt% phosphorus content of flame retardant curing agent b (Example 8), flame retardant curing agent c (Example 9) and flame retardant curing agent d (Example 10) respectively increased to 32.5%, 33.0% and 31.0%, and all of them can pass the UL-94 vertical combustion test V-0 level. Similarly, the tensile strength and impact strength are greatly improved compared with the unmodified epoxy resin (Comparative Example 1).

[0055] Compared with the commonly used commercial flame retardants aluminum hydroxide (Comparative Example 2) and 10-(2, 5-dihydroxyphenyl)-10-hydrogen-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO-HQ) (Comparative Example 3), although the oxygen index and UL-94 combustion rating of the flame-retardant epoxy resin obtained in Comparative Example 2 have been improved to a certain extent, the higher amount of flame retardant added (20 wt%) has caused the tensile strength and impact strength of the material to deteriorate significantly; at the same phosphorus content addition ratio, the oxygen index and UL-94 combustion rating of the flame-retardant epoxy resin obtained in Comparative Example 3 have also been improved to a certain extent, but its flame retardant rating, tensile strength and impact strength are all lower than the performance of the epoxy resin modified by the bio-based flame retardant curing agent a, b, c and d provided by the present invention. Replacing different types of epoxy resins, curing agents and curing accelerators, the epoxy resin modified by the bio-based flame retardant curing agent provided by the present invention also has a similar flame retardant effect.

[0056] In summary, the bio-based flame retardant curing agent provided by the present invention can not only significantly improve the flame retardant properties of epoxy resin, but also significantly improve the tensile strength and impact strength of the material, and is suitable for applications that require simultaneous improvement of flame retardancy and mechanical properties.

[0057] The thermogravimetric analysis curves of the samples in Examples 5, 6, 7 and Comparative Example 1 under nitrogen atmosphere are as follows: Figure 1 It can be seen that the epoxy resin (Examples 5, 6, and 7) with the addition of flame retardant curing agent a (phosphorus content of 0.5 wt%, 1.0 wt%, and 1.5 wt%, respectively) can promote the formation of a carbon layer in the epoxy matrix during thermal decomposition, and the amount of carbon formed is higher than that of the unmodified epoxy resin, thereby exerting a condensed phase flame retardant effect.

[0058] The heat release rate curves of the samples in Examples 5, 6, 7 and Comparative Example 1 are as follows: Figure 2 As shown. It can be seen that the peak heat release rate of the unmodified epoxy resin (Comparative Example 1) is about 1360 kW / m 2The peak heat release rates of the epoxy resins (Examples 5, 6, and 7) added with flame retardant curing agent a (with phosphorus contents of 0.5 wt%, 1.0 wt%, and 1.5 wt%, respectively) were reduced to 1116, 975, and 723 kW / m 2 , decreased by 18%, 28% and 47% compared with the unmodified epoxy resin, indicating that flame retardant curing agent a can effectively inhibit the heat release rate during the combustion of epoxy resin.

[0059] The total heat release curves of the samples in Examples 5, 6, 7 and Comparative Example 1 are as follows: Figure 3 It can be seen that within 0~230s, the total heat release value of the unmodified epoxy resin is about 84.2 MJ / m 2 The total heat release of epoxy resin (Examples 5, 6, and 7) with the addition of flame retardant curing agent a (phosphorus content of 0.5 wt%, 1.0 wt%, and 1.5 wt%, respectively) was reduced to 65.9, 64.6, and 52.8 MJ / m 2 , decreased by 22%, 23% and 37% compared with the unmodified epoxy resin, indicating that flame retardant curing agent a can promote charring and effectively inhibit the heat release during the combustion of epoxy resin.

Claims

1. A bio-based flame retardant toughening curing agent, characterized in that Its chemical structure is shown in the following formula (I): ; In formula (I), R is selected from any one of the following structures: 。 2. The method for preparing the bio-based flame retardant toughening curing agent according to claim 1, characterized in that The following steps are involved: Under the protection of inert gas, the phosphorus-containing compound A and 2-acrylic acid-(2-hydroxy-1,3-propylene)di[oxy(2-hydroxy-3,1-propylene)]ester are stirred and mixed uniformly in a reactor, and heated to react to obtain the target product; The phosphorus-containing compound A is any one of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, diphenylphosphine, diphenyl phosphite, dibenzyl phosphite, dimethyl phosphite, diethyl phosphite, di-n-butyl phosphite and di-tert-butyl phosphite.

3. The preparation method according to claim 2, characterized in that: The molar ratio of 2-acrylic acid-(2-hydroxy-1,3-propylene)di[oxy(2-hydroxy-3,1-propylene)]ester to the phosphorus-containing compound A is 1:(1.8-2.0).

4. The preparation method according to claim 2, characterized in that: The inert gas is any one of nitrogen, argon or helium.

5. The preparation method according to claim 2, characterized in that: The reaction temperature is 150~200°C and the reaction time is 2~24 hours.

6. Use of the bio-based flame retardant toughening curing agent according to claim 1 in epoxy resin curing.

7. The use according to claim 6, characterized in that: The added amount of the bio-based flame retardant toughening curing agent is 2-20% of the total mass of the epoxy curing system.