Impact-resistant rubber composition for dust cover and preparation method thereof

By using butyl rubber, natural rubber, glass fiber and specific compounds in the rubber dust cover, the problem of poor compatibility of glass fibers is solved, the impact resistance and tensile strength of the rubber composition are improved, and the more High impact resistance and strength.

CN118546441BActive Publication Date: 2024-11-29HEBEI HUAMI RUBBER
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411025389.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-29
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

The poor compatibility of glass fibers and matrix materials in existing rubber dustproof covers leads to insufficient impact resistance and difficult to meet the needs of high impact resistance and tensile strength.

Method used

Compositions using butyl rubber, natural rubber, glass fiber, compounds containing carbon-carbon double bonds and butoxy groups, fillers, activators, anti-aging agents, vulcanizing agents and accelerators, and through specific mass ratios and processes, the The impact resistance and tensile strength of the rubber composition.

Benefits of technology

The impact resistance and tensile strength of the rubber composition are significantly improved, and the dustproof cover produced has good impact resistance and high strength, meeting higher usage requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention relates to the field of rubber technology, and proposes an impact-resistant rubber composition for dust covers and a preparation method thereof. An impact-resistant rubber composition for dust covers comprises the following components by mass: 80 parts of butadiene rubber, 20 parts of natural rubber, 5 to 15 parts of glass fiber, 1 to 7 parts of a compound containing a carbon-carbon double bond and a butoxy group, 10 to 30 parts of a filler, 3 to 8 parts of an activator, 1 to 3 parts of an antioxidant, 2 to 4 parts of a vulcanizing agent, and 1 to 3 parts of an accelerator. Through the above technical solution, the problem of poor impact resistance of rubber materials prepared from glass fibers in the related art is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rubber, and in particular to an impact-resistant rubber composition for a dust cover and a preparation method thereof. Background Art

[0002] Dust covers are used to protect the surface of objects from corrosion and damage from the outside world. They come in a variety of shapes, including round, square, and polygonal. They are made of a variety of materials, including fiberglass, rubber, and canvas. Different materials correspond to different performances and different usage scenarios. Among the many types of dust covers, rubber dust covers are the most commonly used because they not only have good elasticity and are suitable for occasions that require frequent bending and extension, but also have good sealing properties, which can effectively prevent corrosion and damage from the outside world.

[0003] At present, butadiene rubber and natural rubber are commonly used as the base materials of rubber dust covers. The impact resistance of the rubber material is improved by adding glass fiber, thereby improving the impact resistance of the dust cover. However, the compatibility of glass fiber with the base material is poor, resulting in the impact resistance of the rubber material to be further improved. Summary of the invention

[0004] The invention provides an impact-resistant rubber composition for a dust cover and a preparation method thereof, which solves the problem of poor impact resistance of rubber materials prepared from glass fibers in the related art.

[0005] The technical solution of the present invention is as follows:

[0006] A shock-resistant rubber composition for a dust cover comprises the following components in parts by mass: 80 parts of butadiene rubber, 20 parts of natural rubber, 5-15 parts of glass fiber, 1-7 parts of a compound containing a carbon-carbon double bond and a butoxy group, 10-30 parts of a filler, 3-8 parts of an activator, 1-3 parts of an antioxidant, 2-4 parts of a vulcanizer, and 1-3 parts of an accelerator.

[0007] As a further technical solution, the mass of the glass fiber is ≤0.6 times the mass of the filler.

[0008] In the present invention, the mass of the glass fiber is ≤0.6 times the mass of the filler, which further improves the impact resistance and tensile strength of the rubber composition.

[0009] As a further technical solution, the mass ratio of the glass fiber to the filler is 4-5:10.

[0010] The present invention limits the mass ratio of glass fiber to filler to 4-5:10, thereby further improving the impact resistance and tensile strength of the rubber composition.

[0011] As a further technical solution, the filler includes hydrophilic silica and / or hydrophobic silica.

[0012] As a further technical solution, the filler includes hydrophobic silica and hydrophilic silica in a mass ratio of 1:1-3.

[0013] The filler of the present invention is limited to hydrophobic white carbon black and hydrophilic white carbon black in a mass ratio of 1:1-3. The impact resistance and tensile strength of the rubber composition are synergistically improved by combining the two.

[0014] As a further technical solution, the mass ratio of the compound containing carbon-carbon double bonds and butoxy group to the glass fiber is 3-5:10.

[0015] The invention limits the mass ratio of the compound containing carbon-carbon double bonds and butoxy groups to the glass fiber to 3-5:10, thereby further improving the impact resistance and tensile strength of the rubber composition.

[0016] As a further technical solution, the compound containing a carbon-carbon double bond and a butoxy group can be any compound containing a carbon-carbon double bond and a butoxy group, preferably one or more of di-n-butyl squarate, N-(butoxymethyl)acrylamide, 3-butoxy-2-cyclohexene-1-one, and 2-butoxyethyl methacrylate.

[0017] As a further technical solution, the activator includes one or both of stearic acid and zinc oxide.

[0018] As a further technical solution, the antioxidant includes one or two of antioxidant RD and antioxidant 4010NA.

[0019] As a further technical solution, the vulcanizing agent includes one or two of sulfur and peroxide;

[0020] The accelerator includes one or both of accelerator CZ and accelerator H.

[0021] As a further technical solution, the peroxide can be any one or more peroxides with vulcanization and crosslinking effects in the art, preferably one or two of diisopropylbenzene peroxide and 1,1-di-tert-butylperoxide-3,3,5-trimethylcyclohexane.

[0022] The present invention also provides a method for preparing an impact-resistant rubber composition for a dust cover, comprising the following steps: mixing butadiene rubber and natural rubber, plasticizing, adding other components, mixing, and vulcanizing to obtain a rubber composition.

[0023] The working principle and beneficial effects of the present invention are:

[0024] The addition of a compound containing a carbon-carbon double bond and a butoxy group in the present invention improves the impact resistance of the rubber composition. The reason is that during the processing of the rubber composition, the compound containing a carbon-carbon double bond and a butoxy group can react with the hydroxyl group on the surface of the glass fiber on the one hand, and on the other hand, the carbon-carbon double bond can also react with the rubber matrix, thereby improving the compatibility of the glass fiber and the rubber matrix, achieving the effect of improving the impact resistance and tensile strength of the rubber composition. The obtained dust cover has good impact resistance and high strength. DETAILED DESCRIPTION

[0025] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] The raw material parameters in the following examples and comparative examples are as follows:

[0027] Butadiene rubber is butadiene rubber BR9000;

[0028] The natural rubber is natural rubber SVRCV60;

[0029] The length of the glass fiber is 3 mm;

[0030] The hydrophilic white carbon black is the hydrophilic Cabot fumed silica M-5;

[0031] The hydrophobic silica is R972 hydrophobic fumed silica.

[0032] Example 1

[0033] 80 parts of butadiene rubber and 20 parts of natural rubber were added into a mixer and mixed evenly, and then plasticized at 45°C for 5 minutes. 15 parts of glass fiber, 1 part of 3-butoxy-2-cyclohexene-1-one, 20 parts of hydrophobic silica, 2 parts of stearic acid, 4 parts of zinc oxide, and 2 parts of antioxidant RD were added, and the mixture was mixed at 120°C and 35 r / min for 10 minutes. The mixture was cooled to 80°C, 3 parts of sulfur and 2 parts of accelerator H were added, and the mixture was mixed for 10 minutes. The mixture was vulcanized at 160°C and 8 MPa for 50 minutes to obtain a rubber composition.

[0034] Example 2

[0035] 80 parts of cis-1,4-dibutyl rubber and 20 parts of natural rubber were added into a mixer and mixed evenly, and then plasticized at 45°C for 5 minutes. 15 parts of glass fiber, 1 part of di-n-butyl squarate, 10 parts of hydrophobic silica, 1 part of stearic acid, 2 parts of zinc oxide and 1 part of antioxidant 4010NA were added and mixed at 120°C and 35 r / min for 10 minutes. The temperature was lowered to 80°C, 2 parts of diisopropyl peroxide and 1 part of accelerator CZ were added and mixed for 10 minutes. The mixture was vulcanized at 160°C and 8 MPa for 50 minutes to obtain a rubber composition.

[0036] Example 3

[0037] 80 parts of butadiene rubber and 20 parts of natural rubber were added into a mixer and mixed evenly, and then plasticized at 45°C for 5 minutes. 15 parts of glass fiber, 1 part of 2-butoxyethyl methacrylate, 30 parts of hydrophobic silica, 2 parts of stearic acid, 6 parts of zinc oxide, and 3 parts of antioxidant 4010NA were added and mixed at 120°C and 35 r / min for 10 minutes. The temperature was lowered to 80°C, 4 parts of 1,1-di-tert-butylperoxy-3,3,5-trimethylcyclohexane, 1 part of accelerator CZ, and 2 parts of accelerator H were added and mixed for 10 minutes. The rubber composition was vulcanized at 160°C and 8 MPa for 50 minutes to obtain a rubber composition.

[0038] Example 4

[0039] 80 parts of butadiene rubber and 20 parts of natural rubber were added into a mixer and mixed evenly, and then plasticized at 45°C for 5 minutes. 12 parts of glass fiber, 1 part of 3-butoxy-2-cyclohexene-1-one, 20 parts of hydrophobic silica, 2 parts of stearic acid, 4 parts of zinc oxide, and 2 parts of antioxidant RD were added, and the mixture was mixed at 120°C and 35 r / min for 10 minutes. The mixture was cooled to 80°C, 3 parts of sulfur and 2 parts of accelerator H were added, and the mixture was mixed for 10 minutes. The mixture was vulcanized at 160°C and 8 MPa for 50 minutes to obtain a rubber composition.

[0040] Example 5

[0041] 80 parts of butadiene rubber and 20 parts of natural rubber were added into a mixer and mixed evenly, and then plasticized at 45°C for 5 minutes. 10 parts of glass fiber, 1 part of 3-butoxy-2-cyclohexene-1-one, 20 parts of hydrophobic silica, 2 parts of stearic acid, 4 parts of zinc oxide, and 2 parts of antioxidant RD were added, and the mixture was mixed at 120°C and 35 r / min for 10 minutes. The mixture was cooled to 80°C, 3 parts of sulfur and 2 parts of accelerator H were added, and the mixture was mixed for 10 minutes. The mixture was vulcanized at 160°C and 8 MPa for 50 minutes to obtain a rubber composition.

[0042] Example 6

[0043] 80 parts of butadiene rubber and 20 parts of natural rubber were added into a mixer and mixed evenly, and then plasticized at 45°C for 5 minutes. 8 parts of glass fiber, 1 part of 3-butoxy-2-cyclohexene-1-one, 20 parts of hydrophobic silica, 2 parts of stearic acid, 4 parts of zinc oxide, and 2 parts of antioxidant RD were added, and the mixture was mixed at 120°C and 35 r / min for 10 minutes. The mixture was cooled to 80°C, 3 parts of sulfur and 2 parts of accelerator H were added, and the mixture was mixed for 10 minutes. The mixture was vulcanized at 160°C and 8 MPa for 50 minutes to obtain a rubber composition.

[0044] Example 7

[0045] 80 parts of butadiene rubber and 20 parts of natural rubber were added into a mixer and mixed evenly, and then plasticized at 45°C for 5 minutes. 5 parts of glass fiber, 1 part of 3-butoxy-2-cyclohexene-1-one, 20 parts of hydrophobic silica, 2 parts of stearic acid, 4 parts of zinc oxide, and 2 parts of antioxidant RD were added, and the mixture was mixed at 120°C and 35 r / min for 10 minutes. The mixture was cooled to 80°C, 3 parts of sulfur and 2 parts of accelerator H were added, and the mixture was mixed for 10 minutes. The mixture was vulcanized at 160°C and 8 MPa for 50 minutes to obtain a rubber composition.

[0046] Example 8

[0047] 80 parts of butadiene rubber and 20 parts of natural rubber were added into a mixer and mixed evenly, and then plasticized at 45°C for 5 minutes. 10 parts of glass fiber, 1 part of 3-butoxy-2-cyclohexene-1-one, 20 parts of hydrophilic silica, 2 parts of stearic acid, 4 parts of zinc oxide, and 2 parts of antioxidant RD were added, and the mixture was mixed at 120°C and 35 r / min for 10 minutes. The mixture was cooled to 80°C, 3 parts of sulfur and 2 parts of accelerator H were added, and the mixture was mixed for 10 minutes. The mixture was vulcanized at 160°C and 8 MPa for 50 minutes to obtain a rubber composition.

[0048] Example 9

[0049] 80 parts of butadiene rubber and 20 parts of natural rubber were added into a mixer and mixed evenly, and then plasticized at 45°C for 5 minutes. 10 parts of glass fiber, 1 part of 3-butoxy-2-cyclohexene-1-one, 2 parts of hydrophobic silica, 18 parts of hydrophilic silica, 2 parts of stearic acid, 4 parts of zinc oxide, and 2 parts of antioxidant RD were added, and the mixture was mixed at 120°C and 35 r / min for 10 minutes. The mixture was cooled to 80°C, 3 parts of sulfur and 2 parts of accelerator H were added, and the mixture was mixed for 10 minutes. The mixture was vulcanized at 160°C and 8 MPa for 50 minutes to obtain a rubber composition.

[0050] Example 10

[0051] 80 parts of butadiene rubber and 20 parts of natural rubber were added into a mixer and mixed evenly, and then plasticized at 45°C for 5 minutes. 10 parts of glass fiber, 1 part of 3-butoxy-2-cyclohexene-1-one, 5 parts of hydrophobic silica, 15 parts of hydrophilic silica, 2 parts of stearic acid, 4 parts of zinc oxide, and 2 parts of antioxidant RD were added, and the mixture was mixed at 120°C and 35 r / min for 10 minutes. The mixture was cooled to 80°C, 3 parts of sulfur and 2 parts of accelerator H were added, and the mixture was mixed for 10 minutes. The mixture was vulcanized at 160°C and 8 MPa for 50 minutes to obtain a rubber composition.

[0052] Embodiment 11

[0053] 80 parts of butadiene rubber and 20 parts of natural rubber were added into a mixer and mixed evenly, and then plasticized at 45°C for 5 minutes. 10 parts of glass fiber, 1 part of 3-butoxy-2-cyclohexene-1-one, 8 parts of hydrophobic silica, 12 parts of hydrophilic silica, 2 parts of stearic acid, 4 parts of zinc oxide, and 2 parts of antioxidant RD were added, and the mixture was mixed at 120°C and 35 r / min for 10 minutes. The mixture was cooled to 80°C, 3 parts of sulfur and 2 parts of accelerator H were added, and the mixture was mixed for 10 minutes. The mixture was vulcanized at 160°C and 8 MPa for 50 minutes to obtain a rubber composition.

[0054] Example 12

[0055] 80 parts of butadiene rubber and 20 parts of natural rubber were added into a mixer and mixed evenly, and then plasticized at 45°C for 5 minutes. 10 parts of glass fiber, 1 part of 3-butoxy-2-cyclohexene-1-one, 10 parts of hydrophobic silica, 10 parts of hydrophilic silica, 2 parts of stearic acid, 4 parts of zinc oxide, and 2 parts of antioxidant RD were added, and the mixture was mixed at 120°C and 35 r / min for 10 minutes. The mixture was cooled to 80°C, 3 parts of sulfur and 2 parts of accelerator H were added, and the mixture was mixed for 10 minutes. The mixture was vulcanized at 160°C and 8 MPa for 50 minutes to obtain a rubber composition.

[0056] Embodiment 13

[0057] 80 parts of butadiene rubber and 20 parts of natural rubber were added into a mixer and mixed evenly, and then plasticized at 45°C for 5 minutes. 10 parts of glass fiber, 1 part of 3-butoxy-2-cyclohexene-1-one, 13 parts of hydrophobic silica, 7 parts of hydrophilic silica, 2 parts of stearic acid, 4 parts of zinc oxide, and 2 parts of antioxidant RD were added, and the mixture was mixed at 120°C and 35 r / min for 10 minutes. The mixture was cooled to 80°C, 3 parts of sulfur and 2 parts of accelerator H were added, and the mixture was mixed for 10 minutes. The mixture was vulcanized at 160°C and 8 MPa for 50 minutes to obtain a rubber composition.

[0058] Embodiment 14

[0059] 80 parts of butadiene rubber and 20 parts of natural rubber were added into a mixer and mixed evenly, and then plasticized at 45°C for 5 minutes. 10 parts of glass fiber, 3 parts of 3-butoxy-2-cyclohexene-1-one, 8 parts of hydrophobic silica, 12 parts of hydrophilic silica, 2 parts of stearic acid, 4 parts of zinc oxide, and 2 parts of antioxidant RD were added, and the mixture was mixed at 120°C and 35 r / min for 10 minutes. The mixture was cooled to 80°C, 3 parts of sulfur and 2 parts of accelerator H were added, and the mixture was mixed for 10 minutes. The mixture was vulcanized at 160°C and 8 MPa for 50 minutes to obtain a rubber composition.

[0060] Embodiment 15

[0061] 80 parts of butadiene rubber and 20 parts of natural rubber were added into a mixer and mixed evenly, and then plasticized at 45°C for 5 minutes. 10 parts of glass fiber, 5 parts of 3-butoxy-2-cyclohexene-1-one, 8 parts of hydrophobic silica, 12 parts of hydrophilic silica, 2 parts of stearic acid, 4 parts of zinc oxide, and 2 parts of antioxidant RD were added, and the mixture was mixed at 120°C and 35 r / min for 10 minutes. The mixture was cooled to 80°C, 3 parts of sulfur and 2 parts of accelerator H were added, and the mixture was mixed for 10 minutes. The mixture was vulcanized at 160°C and 8 MPa for 50 minutes to obtain a rubber composition.

[0062] Example 16

[0063] 80 parts of cis-1,4-dimethylformamide and 20 parts of natural rubber were added into a mixer and mixed evenly, and then plasticized at 45°C for 5 min. 10 parts of glass fiber, 7 parts of 3-butoxy-2-cyclohexene-1-one, 8 parts of hydrophobic silica, 12 parts of hydrophilic silica, 2 parts of stearic acid, 4 parts of zinc oxide and 2 parts of antioxidant RD were added, and the mixture was mixed at 120°C and 35 r / min for 10 min. The mixture was cooled to 80°C, 3 parts of sulfur and 2 parts of accelerator H were added, and the mixture was mixed for 10 min. The mixture was vulcanized at 160°C and 8 MPa for 50 min to obtain a rubber composition.

[0064] Embodiment 17

[0065] 80 parts of butadiene rubber and 20 parts of natural rubber were added into a mixer and mixed evenly, and then plasticized at 45°C for 5 minutes. 10 parts of glass fiber, 5 parts of N-(butoxymethyl)acrylamide, 8 parts of hydrophobic silica, 12 parts of hydrophilic silica, 2 parts of stearic acid, 4 parts of zinc oxide, and 2 parts of antioxidant RD were added, and the mixture was mixed at 120°C and 35 r / min for 10 minutes. The mixture was cooled to 80°C, 3 parts of sulfur and 2 parts of accelerator H were added, and the mixture was mixed for 10 minutes. The mixture was vulcanized at 160°C and 8 MPa for 50 minutes to obtain a rubber composition.

[0066] Comparative Example 1

[0067] 80 parts of butadiene rubber and 20 parts of natural rubber were added into a mixer and mixed evenly, and then plasticized at 45°C for 5 minutes. 15 parts of glass fiber, 20 parts of hydrophobic white carbon black, 2 parts of stearic acid, 4 parts of zinc oxide, and 2 parts of antioxidant RD were added and mixed at 120°C and 35 r / min for 10 minutes. The temperature was lowered to 80°C, 3 parts of sulfur and 2 parts of accelerator H were added, and mixing was continued for 10 minutes. The rubber composition was vulcanized at 160°C and 8 MPa for 50 minutes to obtain a rubber composition.

[0068] The rubber compositions obtained in Examples 1 to 17 and Comparative Example 1 were tested for Izod notched impact strength according to the method in GB / T 1843-2008, and for 1A dumbbell tensile strength according to the method in GB / T 528-2009. The test results are recorded in Table 1.

[0069] Table 1 Izod notched impact strength and tensile strength of rubber compositions

[0070]

[0071] It can be seen from Table 1 that the Izod notched impact strength of the rubber composition provided by the present invention is 54.9 kJ / m 2 The above, the tensile strength is above 18.6MPa, with good impact resistance and high tensile strength.

[0072] Compared with Comparative Example 1, Examples 1 to 17 add compounds containing carbon-carbon double bonds and butoxy groups, while Comparative Example 1 does not add compounds containing carbon-carbon double bonds and butoxy groups. The Izod notched impact strength and tensile strength of the rubber compositions obtained in Examples 1 to 17 are higher than those in Comparative Example 1, indicating that the addition of compounds containing carbon-carbon double bonds and butoxy groups can improve the impact resistance and tensile strength of the rubber composition.

[0073] The Izod notched impact strength and tensile strength of the rubber compositions obtained in Examples 4 to 17 are higher than those in Example 1, indicating that the mass of the glass fiber is ≤0.6 times the mass of the filler, which can further improve the impact resistance and tensile strength of the rubber composition. In addition, the Izod notched impact strength and tensile strength of the rubber compositions obtained in Examples 5 to 6 are higher than those in Examples 4 and 7, indicating that the mass ratio of the glass fiber to the filler is 4 to 5:10, which can further improve the impact resistance and tensile strength of the rubber composition.

[0074] The Izod notched impact strength and tensile strength of the rubber compositions obtained in Examples 10 to 12 are higher than those in Examples 5, 8 to 9, and 13, indicating that when the filler is hydrophobic silica and hydrophilic silica in a mass ratio of 1:1 to 3, the two synergistically improve the impact resistance and tensile strength of the rubber composition.

[0075] The notched Izod impact strength and tensile strength of the rubber compositions obtained in Examples 14 to 15 are higher than those in the other examples, indicating that the mass ratio of the compound containing a carbon-carbon double bond and a butoxy group to the glass fiber is 3 to 5:10, which can further improve the impact resistance and tensile strength of the rubber composition.

[0076] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. An impact-resistant rubber composition for a dust cover, characterized in that: The invention comprises the following components in parts by mass: 80 parts of cis-1,4-butadiene rubber, 20 parts of natural rubber, 5-15 parts of glass fiber, 1-7 parts of a compound containing a carbon-carbon double bond and a butoxy group, 10-30 parts of a filler, 3-8 parts of an activator, 1-3 parts of an antioxidant, 2-4 parts of a vulcanizing agent, and 1-3 parts of an accelerator. The compound containing a carbon-carbon double bond and a butoxy group is one or more of di-n-butyl squarate, N-(butoxymethyl)acrylamide, 3-butoxy-2-cyclohexene-1-one, and 2-butoxyethyl methacrylate.

2. The impact-resistant rubber composition for a dust cover according to claim 1, characterized in that: The mass of the glass fiber is ≤0.6 times the mass of the filler.

3. The impact-resistant rubber composition for a dust cover according to claim 2, characterized in that: The mass ratio of the glass fiber to the filler is 4-5:

10.

4. The impact-resistant rubber composition for a dust cover according to claim 3, characterized in that: The filler includes hydrophilic white carbon black and / or hydrophobic white carbon black.

5. The impact-resistant rubber composition for a dust cover according to claim 4, characterized in that: The filler includes hydrophobic white carbon black and hydrophilic white carbon black in a mass ratio of 1:1-3.

6. The impact-resistant rubber composition for a dust cover according to claim 1, characterized in that: The mass ratio of the compound containing carbon-carbon double bonds and butoxy group to the glass fiber is 3-5:

10.

7. The impact-resistant rubber composition for a dust cover according to claim 1, characterized in that: The activator comprises one or both of stearic acid and zinc oxide.

8. The impact-resistant rubber composition for a dust cover according to claim 1, characterized in that: The antioxidant includes one or both of antioxidant RD and antioxidant 4010NA.

9. The impact-resistant rubber composition for a dust cover according to claim 1, characterized in that: The vulcanizing agent includes one or two of sulfur and peroxide; The accelerator includes one or both of accelerator CZ and accelerator H.

10. The method for preparing an impact-resistant rubber composition for a dust cover according to any one of claims 1 to 9, characterized in that: The following steps are involved: The butadiene rubber and the natural rubber are mixed and then plasticized, and the remaining components are added, kneaded, and vulcanized to obtain a rubber composition.

Citation Information

Patent Citations

  • Anti-aging cable sheath material

    CN105237821A

  • Preparation method of carboxyl polysulfide modified rubber composite material

    CN117986702A