A special interface agent for crack-resistant aluminum formwork concrete and preparation method thereof

Through the combination of base and top layer coatings, nanomaterials and acidic substances are used to emulsify and decompose residual mold release agents, and combine organic polymers and inorganic materials to form a mosaic body, which solves the poor adhesion and insufficient bonding strength of the aluminum mold concrete surface. The problem is to achieve efficient interface processing and crack resistance.

CN118546571BActive Publication Date: 2024-11-26湖南国彩新材料有限公司
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411009943.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-26
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

Existing interfacial agents cannot effectively solve the problems of poor adhesion, insufficient bonding strength, prone to cracking and hollowing caused by residual mold release agent on aluminum mold concrete surface, and lack of special interfacial agents.

Method used

The base coating is used to combine the base coating and the top coating. The base coating contains acidic substances such as nano aluminum sulfate, nano iron chloride, sodium dodecyl sulfonate, and is combined with the permeable alkali-resistant bottom cover emulsion to emulsify and decompose residual mold release agent; The top coating uses organic polymers and inorganic materials, containing alkali-resistant penetration agents and nanomaterials, forming a mosaic to improve adhesion and bonding strength.

Benefits of technology

It significantly improves the adhesion and bonding strength of the aluminum mold concrete surface, prevents cracking, reduces the harm of residual mold release agent, improves the tensile strength and durability of the interface agent, and achieves the effect of quick drying and early strength. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118546571B_ABST
    Figure CN118546571B_ABST
Patent Text Reader

Abstract

The invention provides a special interface agent for crack-resistant aluminum formwork concrete and a preparation method thereof. The interface agent comprises a primer and a surface coating. The primer is composed of the following raw materials in parts by weight: 20-30 parts of water, 0.1-0.2 parts of hydroxypropyl methylcellulose, 2-4 parts of nano aluminum sulfate, 2-4 parts of nano ferric chloride, 1-2 parts of nano carbon fiber, 0.5-1 parts of sulfated castor oil, 2-4 parts of sodium dodecyl sulfonate, 20-30 parts of penetrating anti-alkali bottom sealing emulsion, 20-30 parts of self-made polyvinyl alcohol glutinous rice glue emulsion, 5-10 parts of waste tile powder modified by lime water, 1-2 parts of strong acid-resistant penetrant, 2-3 parts of anti-corrosion and moisture-proof modified bamboo fiber, 2-3 parts of anti-corrosion and moisture-proof modified loofah fiber and 0.3-0.5 parts of defoamer; and the surface coating is a two-component coating composed of component A and component B. The combined use of primer and surface coating not only solves the problem of residual release agent on the surface of aluminum formwork concrete, but also improves the bonding strength and anti-cracking effect of the interface agent, and can also achieve the functions of quick drying, improved efficacy, and comprehensive utilization of waste.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, and in particular to a special interface agent for crack-resistant aluminum formwork concrete and a preparation method thereof. Background Art

[0002] The incidents of building exterior walls falling off happen from time to time. Most of the reasons are caused by the lack of good interface treatment between the wall and the decorative layer. Building interface agents are mainly used to treat the interface of concrete, aerated concrete and the coating surface of old buildings to solve the problems of weak bonding, easy hollowing, cracking, and even peeling caused by the high water absorption, poor strength, smooth surface, looseness and other reasons of these surface layers. In particular, most existing buildings use aluminum alloy formwork to replace the traditional wood formwork for pouring concrete. The aluminum formwork climbing frame technology has been widely used due to its advantages of convenient installation and disassembly, recyclable reuse, labor saving and time saving. However, the base surface of concrete poured with aluminum molds is very smooth, and there are residual release agents. These residual release agents will seriously affect the adhesion of the surface coating. In particular, some construction sites use oily release agents for good demoulding. If putty or mortar is directly scraped without good interface treatment, it is easy to cause hollowing and cracking. However, traditional interface agents cannot meet the interface treatment requirements of aluminum formwork concrete. Currently, no special interface agent for aluminum formwork concrete has been found on the market, so it is imperative to develop a special interface agent for aluminum formwork concrete. Summary of the invention

[0003] In view of the above, the purpose of the present invention is to provide a special interface agent for anti-cracking aluminum formwork concrete and a preparation method thereof, which has strong bonding force, anti-cracking, good adhesion, can decompose residual release agent, has good affinity with aluminum formwork concrete, and dries quickly, in order to solve the technical problems that the existing interface agents have poor adhesion, insufficient bonding strength, easy cracking and hollowing, slow drying, etc. when applied to aluminum formwork concrete walls.

[0004] The technical solution of the present invention:

[0005] The invention provides a special interface agent for crack-resistant aluminum formwork concrete, comprising a primer and a surface coating;

[0006] The bottom coating is composed of the following raw materials by weight: 20-30 parts of water, 0.1-0.2 parts of hydroxypropyl methylcellulose, 2-4 parts of nano aluminum sulfate, 2-4 parts of nano ferric chloride, 1-2 parts of nano carbon fiber, 0.5-1 parts of sulfated castor oil, 2-4 parts of sodium dodecyl sulfonate, 20-30 parts of penetrating anti-alkali bottom sealing emulsion, 20-30 parts of self-made polyvinyl alcohol glutinous rice glue emulsion, 5-10 parts of waste tile powder modified by lime water, 1-2 parts of strong acid resistant penetrant, 2-3 parts of anti-corrosion and moisture-proof modified bamboo fiber, 2-3 parts of anti-corrosion and moisture-proof modified loofah fiber, and 0.3-0.5 parts of defoaming agent;

[0007] The surface coating is a two-component coating consisting of component A and component B, and the mixing weight ratio of component A to component B is 1:3-3.5;

[0008] Component A is composed of the following materials by weight: 30-40 parts of water, 0.1-0.2 parts of hydroxypropyl methylcellulose, 1-2 parts of nano silicon dioxide, 20-30 parts of organosilicon modified polyurethane emulsion, 20-30 parts of penetrating anti-alkali backing emulsion, 3-5 parts of lime milk solution, and 1-2 parts of strong alkali resistant penetrating wetting agent;

[0009] Component B is composed of the following materials by weight: 30-40 parts of sulphoaluminate cement, 30-40 parts of lime water modified waste tile powder, 10-20 parts of quartz sand, 1-2 parts of borax, 1-2 parts of trisodium phosphate, 3-5 parts of nano alumina, 3-5 parts of microsilica powder, 2-3 parts of anti-corrosion and moisture-proof modified bamboo fiber, and 2-3 parts of anti-corrosion and moisture-proof modified loofah fiber.

[0010] Preferably, the nano-silicon dioxide is a nano-silicon dioxide solution with a particle size of 20-30 nanometers and a content of 10%.

[0011] Preferably, the nano-carbon fiber is carbon fiber with a particle size of 80-100 nanometers.

[0012] Preferably, the nano aluminum sulfate is nano aluminum sulfate with a particle size of 30-50 nanometers; the nano ferric chloride is nano ferric chloride with a particle size of 30-50 nanometers.

[0013] The preparation method of the above-mentioned special interface agent for crack-resistant aluminum mold concrete and the preparation method of the base coating are as follows: hydroxypropyl methylcellulose, nano aluminum sulfate, nano ferric chloride and nano carbon fiber are slowly added into water in sequence, dispersed and stirred at a speed of 800-100 rpm for 30 minutes, and then sulfated castor oil, sodium dodecyl sulfate, penetrating anti-alkali bottom sealing emulsion, homemade polyvinyl alcohol glutinous rice glue emulsion, anti-corrosion and moisture-proof modified bamboo fiber, anti-corrosion and moisture-proof modified loofah fiber, lime water modified waste tile powder, strong acid-resistant penetrant and defoaming agent are added in sequence at a speed of 200-300 rpm and stirred evenly.

[0014] The preparation method of the above-mentioned interface agent and the preparation method of the surface coating are as follows: Component A is to add hydroxypropyl methylcellulose and nano-silicon dioxide into water in sequence, disperse them at a speed of 800-100 rpm for 30 minutes, then disperse them at a speed of 200-300 rpm, and add silicone-modified polyurethane emulsion, penetrating anti-alkali bottom sealing emulsion, lime milk solution, and strong alkali-resistant penetrating wetting agent in sequence and stir evenly; Component B is to mix all the components thoroughly and evenly. When using, first pour 3-3.5 parts of component B into one part of material A and stir evenly before use.

[0015] The preparation method of the above-mentioned interface agent, the modification treatment of waste tile powder: first clean the waste tiles and then soak them in 10% lime water solution for 10 hours, then dry and crush them into 80-100 mesh tile powder particles.

[0016] The preparation method of the above-mentioned interface agent and the modification treatment of bamboo fiber are as follows: first, the bamboo is cut into small pieces of 2-5 mm in length, and after being steamed, it is put into a hot grinder and ground into bamboo fiber, and after drying, a mixed aqueous solution of elastic polyurethane emulsion and VAE emulsion that can be cured into a film is evenly sprayed on it, and the solution is fully coated on the bamboo fiber. After it is completely cured into a film and dried, it can be made into 2-5 mm fiber.

[0017] The preparation method of the above-mentioned interface agent and the modification treatment of the loofah fiber are as follows: the loofah is first cut into small segments of 2-5 mm, and then immersed in a 30% elastic polyurethane aqueous solution that can be cured into a film, allowing the solution to fully coat the loofah fiber, and then dried to form a loofah fiber with a length of 2-5 mm.

[0018] The preparation method of the above-mentioned interface agent and the production method of homemade polyvinyl alcohol glutinous rice glue emulsion are as follows: 10 parts of pure water are added to 2 parts of glutinous rice flour, 0.5 parts of sweet potato flour, and 0.5 parts of 17-99 model polyvinyl alcohol powder, stirred evenly, heated to 95-100 degrees for gelatinization for 40-50 minutes, then cooled to 50-70 degrees, slowly added with 0.3 parts of hydrochloric acid, and reacted for 30 minutes, then cooled to 40 degrees, added with 0.3 parts of silane coupling agent, 0.7 parts of 10% lime milk solution, and 3 parts of VAE emulsion, and reacted for 30 minutes.

[0019] Beneficial effects of the present invention:

[0020] The invention of this application adopts the combination of primer and surface coating, which are applied to the surface of aluminum mold concrete. Since the primer contains multiple acidic substances such as nano aluminum sulfate, nano ferric chloride, sodium dodecyl sulfonate, sulfated castor oil, etc., under the synergistic effect of strong acid-resistant penetrant and penetrating bottom-sealing anti-alkali emulsion, these acidic substances can penetrate into the aluminum mold concrete wall, and play the role of emulsification, decomposition and degradation of the release agent remaining on the surface of the aluminum mold concrete, thereby reducing the influence of the remaining release agent on the adhesion. At the same time, the penetrating anti-alkali bottom-sealing emulsion is used in combination with the strong acid-resistant penetrant, which can cooperate with nano aluminum sulfate, nano ferric chloride, and nano carbon fiber to penetrate into the capillary channel of the aluminum mold concrete to form a gel, which is embedded in the aluminum mold concrete like a rivet, playing the role of waterproof, anti-seepage and firm bonding. Homemade polyvinyl alcohol glutinous rice glue latex can firmly bond lime water modified waste tile powder, anti-corrosion and moisture-proof modified bamboo fiber, and anti-corrosion and moisture-proof modified loofah fiber to aluminum mold concrete, forming an uneven rough surface, which is conducive to the adhesion of the surface coating and can also play a role in crack resistance and crack prevention. In addition, the surface coating uses organic polymer materials and inorganic materials in combination. After mixing evenly, it is sprayed on the bottom coating. The alkaline substances formed will decompose the remaining release agent again, which not only solves the harm of the remaining release agent, but also greatly improves the adhesion and bonding strength of the product. Its tensile strength can reach 1-1.3mpa. Organic polymer modified polyurethane emulsion and VAE emulsion can improve the brittleness of cement paste and improve the bonding strength of cement paste, so that cement polymer can achieve the effect of both rigidity and flexibility and prevent cracking; the alkali-resistant penetrant contained in the surface coating, nano-silicon dioxide and nano-alumina can penetrate into the base coating and aluminum mold concrete under the action of the penetrant to form a mosaic to improve adhesion and bonding strength, and improve the density and durability of cement paste. The borax solution contained in the surface coating can cross-link with the polyvinyl alcohol in the homemade polyvinyl alcohol glutinous rice glue emulsion in the base coating, which can improve adhesion and bonding strength, and can also play a role in regulating the setting time of cement. The trisodium phosphate contained in it can also react with the hydration products in cement to form a stable complex, which can effectively inhibit the shrinkage and expansion of cement products, improve the crack resistance of cement, and improve the fluidity of cement mortar. By modifying bamboo fiber and loofah fiber and then replacing traditional short glass fiber (traditional short glass fiber cannot prevent cracking under alkaline conditions), it can prevent cracking. Modified waste tile powder is used to replace traditional quartz sand. The reuse of waste tile powder effectively reduces the exploitation of natural resources, reduces environmental pressure, and promotes the development of a circular economy. In addition, the cost of obtaining waste tile powder is low, which reduces production costs and improves economic benefits.

[0021] The present application invents a special interface agent for crack-resistant aluminum formwork concrete and a preparation method thereof. The interface agent adopts the combined use of a base coating and a surface coating, which not only solves the problem of residual release agent on the surface of aluminum formwork concrete, but also improves the bonding strength and anti-cracking effect of the interface agent, and can also achieve the functions of quick drying, early strength, improved efficacy, and comprehensive utilization of waste.

[0022] The preferred embodiments of the present invention and their beneficial effects will be further described in detail in conjunction with specific implementation methods. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present invention, but should not be construed as limiting the present invention. In the accompanying drawings:

[0024] Figure 1 The following is a comparison of the cement board substrates after being soaked in water for two days using a certain brand of interface agent (left) and the interface agent of the present invention (right).

[0025] Figure 2 The following is a comparison of the actual objects after a certain brand of interface agent (left) and the interface agent of the present invention (right) were soaked in water for two days on the base surface of the ceramic tile.

[0026] Figure 3 The following is a comparison of the glass surfaces after being soaked in water for two days using a certain brand of interface agent (left) and the interface agent of the present invention (right). DETAILED DESCRIPTION

[0027] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention. Embodiment 1:

[0028] This embodiment provides a special interface agent for crack-resistant aluminum formwork concrete, which is composed of a base coating and a surface coating.

[0029] The primer is composed of the following materials by weight: 30 parts of water, 0.1 parts of hydroxypropyl methylcellulose, 3 parts of nano-aluminum sulfate, 2 parts of nano-ferric chloride, 1 part of nano-carbon fiber, 0.5 parts of sulfated castor oil, 3 parts of sodium dodecyl sulfate, 20 parts of penetrating anti-alkali bottom sealing emulsion, 29 parts of homemade polyvinyl alcohol glutinous rice glue latex, 7 parts of waste tile powder modified by lime water, 1 part of strong acid resistant penetrant, 1.5 parts of anti-corrosion and moisture-proof modified bamboo fiber, 1.5 parts of anti-corrosion and moisture-proof modified loofah fiber, and 0.4 parts of defoaming agent.

[0030] Production preparation method of base coating: slowly add hydroxypropyl methylcellulose, nano aluminum sulfate, nano ferric chloride, and nano carbon fiber into water in turn and disperse at high speed (800-100 rpm) and stir for 30 minutes, then add sulfated castor oil, sodium dodecyl sulfate, penetrating anti-alkali bottom sealing emulsion, homemade polyvinyl alcohol glutinous rice glue emulsion, anti-corrosion and moisture-proof modified bamboo fiber, anti-corrosion and moisture-proof modified loofah fiber, lime water modified waste tile powder, strong acid-resistant penetrant, and defoaming agent in turn at low speed (200-300 rpm) and stir evenly.

[0031] The surface coating is a two-component coating consisting of component A (liquid) and component B (powder), and the mixing weight ratio of component A to component B is 1:3.

[0032] Component A (liquid material) is composed of the following materials by weight: 33.8 parts of water, 0.2 parts of hydroxypropyl methylcellulose, 2 parts of nano-silicon dioxide, 30 parts of silicone-modified polyurethane emulsion, 30 parts of penetrating alkali-resistant bottom sealing emulsion, 3 parts of lime milk solution, and 1 part of strong alkali-resistant penetrating wetting agent.

[0033] Component B (powder) is composed of the following materials by weight: 33 parts of sulphoaluminate cement, 40 parts of lime water modified waste tile powder, 15 parts of quartz sand, 1 part of borax, 1 part of trisodium phosphate, 3 parts of nano alumina, 3 parts of microsilica powder, 2 parts of anti-corrosion and moisture-proof modified bamboo fiber, and 2 parts of anti-corrosion and moisture-proof modified loofah fiber.

[0034] Production and preparation method of surface coating:

[0035] The production method of component A (liquid material) is to add hydroxypropyl methylcellulose and nano silicon dioxide in water in turn, disperse at high speed (800-100 rpm) for 30 minutes and then disperse at low speed (200-300 rpm), add silicone modified polyurethane emulsion, penetrating anti-alkali bottom emulsion, lime milk solution and strong alkali resistant penetrating wetting agent in turn and stir evenly.

[0036] The production method of component B (powder) is to mix all the components thoroughly and evenly. When using, first pour 3 parts of component B into 1 part of material A and stir evenly before use.

[0037] In this embodiment, the water is purified water;

[0038] In this embodiment, the hydroxypropyl methylcellulose is the hydroxypropyl methylcellulose commonly used in water-based coatings;

[0039] In this embodiment, the nano aluminum sulfate used is nano aluminum sulfate with a particle size of 50 nanometers;

[0040] In this embodiment, the nano ferric chloride used is nano ferric chloride with a particle size of 30 nanometers;

[0041] In this embodiment, the sulfated castor oil used is sulfated castor oil produced by Wuhan Huaxiang Kejie Biotechnology Co., Ltd.;

[0042] In this embodiment, the sodium dodecyl sulfonate is produced by Kunshan Shengan Company;

[0043] In this embodiment, the penetrating anti-alkali backing emulsion is RS-64 penetrating anti-eluviation emulsion produced by Badford Company. The emulsion has a strong penetrating power and can penetrate into the capillary channel of aluminum mold concrete. The penetration depth can reach 10-20mm.

[0044] In this embodiment, the lime milk solution is a 10% lime milk solution;

[0045] In this embodiment, the nano carbon fiber is a carbon fiber with a particle size of 80 nanometers.

[0046] In this embodiment, the strong acid resistant penetrant selected is OE-35 produced by Haian Guoli Chemical Co., Ltd.;

[0047] In this embodiment, the anti-corrosion and moisture-proof modified bamboo fiber is bamboo fiber that has been treated with anti-corrosion and moisture-proof modification;

[0048] In this embodiment, the anti-corrosion and moisture-proof modified loofah fiber is a loofah fiber that has been treated with anti-corrosion and moisture-proof modification;

[0049] In this embodiment, the defoamer is a water-based paint defoamer commonly used in the market;

[0050] In this embodiment, the organosilicon-modified polyurethane emulsion is 8081 produced by Evonik of Germany. The emulsion has good permeability and high flexibility, which can make the cement paste have good flexibility, prevent cracking, and improve the bonding strength and mechanical properties of the cement polymer. It can also penetrate into the capillary channels of aluminum mold concrete.

[0051] In this embodiment, the nano-alumina has a particle size of 30 nanometers;

[0052] In this embodiment, the nano aluminum sulfate has a particle size of 20 nanometers;

[0053] In this embodiment, the nano-silica solution is a nano-silica solution with a particle size of 30 nanometers and a content of 10%. It can improve the fluidity of cement mortar, and can penetrate and fill the capillary channels of aluminum mold concrete, thereby greatly improving the density of the cement slurry and improving the durability and strength of the interface agent product.

[0054] In this embodiment, the alkali-resistant wetting penetrant is OE-46 produced by Haian Guoli Chemical Co., Ltd. This penetrant has good permeability and can penetrate into the pores of aluminum mold concrete to a penetration depth of 10-20 mm;

[0055] In this embodiment, the sulphoaluminate cement is 425 type sulphoaluminate cement;

[0056] In this embodiment, the quartz sand is 100 mesh dry quartz sand.

[0057] In this embodiment, the modification treatment of waste tile powder is as follows: the waste tiles are first cleaned and then soaked in a 10% lime solution for 10 hours, and then dried and crushed into 80 mesh tile powder particles.

[0058] Modification of bamboo fiber: first cut the bamboo into small pieces of 2mm in length, then put it into a hot grinder after steaming and grind it into bamboo fiber. After drying, evenly spray a mixed aqueous solution of elastic polyurethane emulsion and VAE emulsion that can be cured into a film, allow the solution to fully cover the bamboo fiber, and wait for it to be completely cured into a film and dried to make 2mm fibers. The bamboo fiber modified by this method has good flexibility and anti-cracking function, and can also be anti-corrosive and anti-mildew.

[0059] Modification of loofah fiber: first cut the loofah into small sections of 5mm, then soak it in a 30% elastic polyurethane aqueous solution that can be cured into a film, allow the solution to fully coat the loofah fiber, and then dry it to make loofah fiber with a length of 5mm. The loofah fiber modified by this method has good flexibility and anti-cracking function, and can also resist corrosion and mildew.

[0060] The production method of homemade polyvinyl alcohol glutinous rice glue emulsion: use 10 parts of pure water to add 2 parts of glutinous rice flour, 0.5 parts of sweet potato flour, and 0.5 parts of 17-99 polyvinyl alcohol powder, stir evenly, heat to 100 degrees for gelatinization for 40 minutes, then cool to about 60 degrees, slowly add 0.3 parts of hydrochloric acid and react for 30 minutes, then cool to 40 degrees, add 0.3 parts of silane coupling agent, 0.7 parts of 10% lime milk solution, and 3 parts of VAE emulsion, and react for 30 minutes.

[0061] The method of using the primer and the surface coating together: first apply the primer to the aluminum formwork concrete wall by spraying or roller coating, and then roller or spray the mixed surface coating onto the primer.

[0062] Embodiment 2:

[0063] This embodiment provides a special interface agent for crack-resistant aluminum formwork concrete and a preparation method thereof, which is composed of a base coating and a surface coating and is used in combination;

[0064] The primer is composed of the following materials by weight: 21.2 parts of water, 0.2 parts of hydroxypropyl methylcellulose, 4 parts of nano-aluminum sulfate, 4 parts of nano-ferric chloride, 1.5 parts of nano-carbon fiber, 0.6 parts of sulfated castor oil, 4 parts of sodium dodecyl sulfate, 30 parts of penetrating anti-alkali sealing emulsion, 20 parts of homemade polyvinyl alcohol glutinous rice glue latex, 8 parts of waste tile powder modified by lime water, 2 parts of strong acid-resistant penetrant, 2 parts of anti-corrosion and moisture-proof modified bamboo fiber, 2 parts of anti-corrosion and moisture-proof modified loofah fiber, and 0.5 parts of defoaming agent.

[0065] Production preparation method of base coating: slowly add hydroxypropyl methylcellulose, nano aluminum sulfate, nano ferric chloride, and nano carbon fiber into water in turn and disperse at high speed (800-100 rpm) and stir for 30 minutes, then add sulfated castor oil, sodium dodecyl sulfate, penetrating anti-alkali bottom sealing emulsion, homemade polyvinyl alcohol glutinous rice glue emulsion, anti-corrosion and moisture-proof modified bamboo fiber, anti-corrosion and moisture-proof modified loofah fiber, lime water modified waste tile powder, strong acid-resistant penetrant, and defoaming agent in turn at low speed (200-300 rpm) and stir evenly.

[0066] The surface coating is a two-component coating consisting of component A (liquid) and component B (powder), and the mixing weight ratio of component A to component B is 1:3.

[0067] Component A (liquid material) is composed of the following materials by weight: 38.9 parts of water, 0.1 parts of hydroxypropyl methylcellulose, 1 part of nano-silicon dioxide, 25 parts of silicone-modified polyurethane emulsion, 28 parts of penetrating alkali-resistant bottom sealing emulsion, 5 parts of lime milk solution, and 2 parts of strong alkali-resistant penetrating wetting agent.

[0068] Component B (powder) is composed of the following materials by weight: 33 parts of sulphoaluminate cement, 35 parts of lime water modified waste tile powder, 15.5 parts of quartz sand, 1.5 parts of borax, 1.5 parts of trisodium phosphate, 4 parts of nano alumina, 3.5 parts of microsilica powder, 3 parts of anti-corrosion and moisture-proof modified bamboo fiber, and 3 parts of anti-corrosion and moisture-proof modified loofah fiber.

[0069] Production and preparation method of surface coating:

[0070] The production method of component A (liquid material) is to add hydroxypropyl methylcellulose and nano silicon dioxide in water in turn, disperse at high speed (800-100 rpm) for 30 minutes and then disperse at low speed (200-300 rpm), add silicone modified polyurethane emulsion, penetrating anti-alkali bottom emulsion, lime milk solution and strong alkali resistant penetrating wetting agent in turn and stir evenly.

[0071] The production method of component B (powder) is to mix all the components thoroughly and evenly. When using, pour 3.5 parts of component B into 1 part of material A and stir evenly before use.

[0072] In this embodiment, the water is purified water;

[0073] In this embodiment, the hydroxypropyl methylcellulose is the hydroxypropyl methylcellulose commonly used in water-based coatings;

[0074] In this embodiment, the nano aluminum sulfate used is nano aluminum sulfate with a particle size of 30 nanometers;

[0075] In this embodiment, the nano ferric chloride used is nano ferric chloride with a particle size of 50 nanometers;

[0076] In this embodiment, the sulfated castor oil used is sulfated castor oil produced by Wuhan Huaxiang Kejie Biotechnology Co., Ltd.;

[0077] In this embodiment, the sodium dodecyl sulfonate is produced by Kunshan Shengan Company;

[0078] In this embodiment, the penetrating anti-alkali backing emulsion is RS-64 penetrating anti-eluviation emulsion produced by Badford Company. The emulsion has a strong penetrating power and can penetrate into the capillary channel of aluminum mold concrete. The penetration depth can reach 10-20mm.

[0079] In this embodiment, the lime milk solution is a 10% high-quality lime milk solution;

[0080] In this embodiment, the nano carbon fiber is a carbon fiber with a particle size of 100 nanometers.

[0081] In this embodiment, the strong acid resistant penetrant selected is OE-35 produced by Haian Guoli Chemical Co., Ltd.;

[0082] In this embodiment, the anti-corrosion and moisture-proof modified bamboo fiber is bamboo fiber that has been treated with anti-corrosion and moisture-proof modification;

[0083] In this embodiment, the anti-corrosion and moisture-proof modified loofah fiber is a loofah fiber that has been treated with anti-corrosion and moisture-proof modification;

[0084] In this embodiment, the defoamer is a water-based paint defoamer commonly used in the market;

[0085] In this embodiment, the organosilicon-modified polyurethane emulsion is 8081 produced by Evonik of Germany. The emulsion has good permeability and high flexibility, which can make the cement paste have good flexibility, prevent cracking, and improve the bonding strength and mechanical properties of the cement polymer. It can also penetrate into the capillary channels of aluminum mold concrete.

[0086] In this embodiment, the nano-alumina has a particle size of 20 nanometers;

[0087] In this embodiment, the nano aluminum sulfate has a particle size of 30 nanometers;

[0088] In this embodiment, the nano-silica solution is a nano-silica solution with a particle size of 20 nanometers and a content of 10%. It can improve the fluidity of cement mortar, and can penetrate and fill the capillary channels of aluminum mold concrete, thereby greatly improving the density of the cement slurry and improving the durability and strength of the interface agent product.

[0089] In this embodiment, the alkali-resistant wetting penetrant is OE-46 produced by Haian Guoli Chemical Co., Ltd. This penetrant has good permeability and can penetrate into the pores of aluminum mold concrete to a penetration depth of 10-20 mm;

[0090] In this embodiment, the sulphoaluminate cement is 425 type sulphoaluminate cement;

[0091] In this embodiment, the quartz sand is 80 mesh dry quartz sand.

[0092] In this embodiment, the modification treatment of waste tile powder is as follows: the waste tiles are first cleaned and then soaked in a 10% lime solution for 10 hours, and then dried and crushed into 100-mesh tile powder particles.

[0093] Modification of bamboo fiber: first cut the bamboo into small pieces of 5mm in length, then put it into a hot grinder after steaming and grind it into bamboo fiber. After drying, evenly spray a mixed aqueous solution of elastic polyurethane emulsion and VAE emulsion that can be cured into a film, allow the solution to fully cover the bamboo fiber, and wait for it to be completely cured into a film and dried to make 5mm fibers. The bamboo fiber modified by this method has good flexibility and anti-cracking function, and can also be anti-corrosive and anti-mildew.

[0094] Modification of loofah fiber: first cut the loofah into small sections of 2 mm, then soak it in a 30% elastic polyurethane aqueous solution that can be cured into a film, allow the solution to fully coat the loofah fiber, and then dry it to make loofah fiber with a length of 5 mm. The loofah fiber modified by this method has good flexibility and anti-cracking function, and can also resist corrosion and mildew.

[0095] The production method of homemade polyvinyl alcohol glutinous rice glue emulsion: use 10 parts of pure water to add 2 parts of glutinous rice flour, 0.5 parts of sweet potato flour, and 0.5 parts of 17-99 polyvinyl alcohol powder, stir evenly, heat to 95 degrees for gelatinization for 50 minutes, then cool to about 60 degrees, slowly add 0.3 parts of hydrochloric acid and react for 30 minutes, then cool to 40 degrees, add 0.3 parts of silane coupling agent, 0.7 parts of 10% lime milk solution, and 3 parts of VAE emulsion, and react for 30 minutes.

[0096] The method of using the primer and the surface coating together: first apply the primer to the aluminum formwork concrete wall by spraying or roller coating, and then apply the mixed surface coating to the primer by roller coating or spraying.

[0097] Embodiment 3:

[0098] This embodiment provides a special interface agent for crack-resistant aluminum formwork concrete and a preparation method thereof, which is composed of a base coating and a surface coating and is used in combination;

[0099] The primer is composed of the following materials by weight: 26 parts of water, 0.15 parts of hydroxypropyl methylcellulose, 3 parts of nano-aluminum sulfate, 3 parts of nano-ferric chloride, 1.2 parts of nano-carbon fiber, 0.7 parts of sulfated castor oil, 3 parts of sodium dodecyl sulfate, 26 parts of penetrating anti-alkali sealing emulsion, 25 parts of homemade polyvinyl alcohol glutinous rice glue latex, 7 parts of lime water modified waste tile powder, 1.5 parts of strong acid resistant penetrant, 2.5 parts of anti-corrosion and moisture-proof modified bamboo fiber, 2.6 parts of anti-corrosion and moisture-proof modified loofah fiber, and 0.4 parts of defoaming agent.

[0100] Production preparation method of base coating: slowly add hydroxypropyl methylcellulose, nano aluminum sulfate, nano ferric chloride, and nano carbon fiber into water in turn and disperse at high speed (800-100 rpm) and stir for 30 minutes, then add sulfated castor oil, sodium dodecyl sulfate, penetrating anti-alkali bottom sealing emulsion, homemade polyvinyl alcohol glutinous rice glue emulsion, anti-corrosion and moisture-proof modified bamboo fiber, anti-corrosion and moisture-proof modified loofah fiber, lime water modified waste tile powder, strong acid-resistant penetrant, and defoaming agent in turn at low speed (200-300 rpm) and stir evenly.

[0101] The surface coating is a two-component coating consisting of component A (liquid) and component B (powder), and the mixing weight ratio of component A to component B is 1:3.

[0102] Component A (liquid material) is composed of the following materials by weight: 36 parts of water, 0.15 parts of hydroxypropyl methylcellulose, 1.5 parts of nano-silicon dioxide, 28 parts of silicone-modified polyurethane emulsion, 22 parts of penetrating alkali-resistant bottom sealing emulsion, 4 parts of lime milk solution, and 1.5 parts of strong alkali-resistant penetrating wetting agent.

[0103] Component B (powder) is composed of the following materials by weight: 32 parts of sulphoaluminate cement, 32 parts of lime water modified waste tile powder, 12 parts of quartz sand, 1.2 parts of borax, 1.3 parts of trisodium phosphate, 4 parts of nano alumina, 3.2 parts of microsilica powder, 2.3 parts of anti-corrosion and moisture-proof modified bamboo fiber, and 2.6 parts of anti-corrosion and moisture-proof modified loofah fiber.

[0104] Production and preparation method of surface coating:

[0105] The production method of component A (liquid material) is to add hydroxypropyl methylcellulose and nano silicon dioxide in water in turn, disperse at high speed (800-100 rpm) for 30 minutes and then disperse at low speed (200-300 rpm), add silicone modified polyurethane emulsion, penetrating anti-alkali bottom emulsion, lime milk solution and strong alkali resistant penetrating wetting agent in turn and stir evenly.

[0106] The production method of component B (powder) is to mix all the components thoroughly and evenly. When using, pour 3.5 parts of component B into 1 part of material A and stir evenly before use.

[0107] In this embodiment, the water is purified water;

[0108] In this embodiment, the hydroxypropyl methylcellulose is the hydroxypropyl methylcellulose commonly used in water-based coatings;

[0109] In this embodiment, the nano aluminum sulfate used is nano aluminum sulfate with a particle size of 40 nanometers;

[0110] In this embodiment, the nano ferric chloride used is nano ferric chloride with a particle size of 40 nanometers;

[0111] In this embodiment, the sulfated castor oil used is sulfated castor oil produced by Wuhan Huaxiang Kejie Biotechnology Co., Ltd.;

[0112] In this embodiment, the sodium dodecyl sulfonate is produced by Kunshan Shengan Company;

[0113] In this embodiment, the penetrating anti-alkali backing emulsion is RS-64 penetrating anti-eluviation emulsion produced by Badford Company. The emulsion has a strong penetrating power and can penetrate into the capillary channel of aluminum mold concrete. The penetration depth can reach 10-20mm.

[0114] In this embodiment, the lime milk solution is a 10% high-quality lime milk solution;

[0115] In this embodiment, the nano carbon fiber is a carbon fiber with a particle size of 90 nanometers.

[0116] In this embodiment, the strong acid resistant penetrant selected is OE-35 produced by Haian Guoli Chemical Co., Ltd.;

[0117] In this embodiment, the anti-corrosion and moisture-proof modified bamboo fiber is bamboo fiber that has been treated with anti-corrosion and moisture-proof modification;

[0118] In this embodiment, the anti-corrosion and moisture-proof modified loofah fiber is a loofah fiber that has been treated with anti-corrosion and moisture-proof modification;

[0119] In this embodiment, the defoamer is a water-based paint defoamer commonly used in the market;

[0120] In this embodiment, the organosilicon-modified polyurethane emulsion is 8081 produced by Evonik of Germany. The emulsion has good permeability and high flexibility, which can make the cement paste have good flexibility, prevent cracking, and improve the bonding strength and mechanical properties of the cement polymer. It can also penetrate into the capillary channels of aluminum mold concrete.

[0121] In this embodiment, the nano-alumina has a particle size of 26 nanometers;

[0122] In this embodiment, the nano aluminum sulfate has a particle size of 28 nanometers;

[0123] In this embodiment, the nano-silica solution is a nano-silica solution with a particle size of 23 nanometers and a content of 10%. It can improve the fluidity of cement mortar, and can penetrate and fill the capillary channels of aluminum mold concrete, thereby greatly improving the density of the cement slurry and improving the durability and strength of the interface agent product.

[0124] In this embodiment, the alkali-resistant wetting penetrant is OE-46 produced by Haian Guoli Chemical Co., Ltd. This penetrant has good permeability and can penetrate into the pores of aluminum mold concrete to a penetration depth of 10-20 mm;

[0125] In this embodiment, the sulphoaluminate cement is 425 type sulphoaluminate cement;

[0126] In this embodiment, the quartz sand is 90 mesh dry quartz sand.

[0127] In this embodiment, the modification treatment of waste tile powder is as follows: the waste tiles are first cleaned and then soaked in a 10% lime solution for 10 hours, and then dried and crushed into 90 mesh tile powder particles.

[0128] Modification of bamboo fiber: first cut the bamboo into small pieces of 4mm in length, then put it into a hot grinder after steaming and grind it into bamboo fiber. After drying, evenly spray a mixed aqueous solution of elastic polyurethane emulsion and VAE emulsion that can be cured into a film, allow the solution to fully cover the bamboo fiber, and wait for it to be completely cured into a film and dried to make 4mm fibers. The bamboo fiber modified by this method has good flexibility and anti-cracking function, and can also be anti-corrosive and anti-mildew.

[0129] Modification of loofah fiber: first cut the loofah into small sections of 3mm, then soak it in a 30% elastic polyurethane aqueous solution that can be cured into a film, allow the solution to fully coat the loofah fiber, and then dry it to make loofah fiber with a length of 3mm. The loofah fiber modified by this method has good flexibility and anti-cracking function, and can also resist corrosion and mildew.

[0130] The production method of homemade polyvinyl alcohol glutinous rice glue emulsion: use 10 parts of pure water to add 2 parts of glutinous rice flour, 0.5 parts of sweet potato flour, and 0.5 parts of 17-99 polyvinyl alcohol powder, stir evenly, heat to 98 degrees for gelatinization for 50 minutes, then cool to about 60 degrees, slowly add 0.3 parts of hydrochloric acid and react for 30 minutes, then cool to 40 degrees, add 0.3 parts of silane coupling agent, 0.7 parts of 10% lime milk solution, and 3 parts of VAE emulsion, and react for 30 minutes.

[0131] The method of using the primer and the surface coating together: first apply the primer to the aluminum formwork concrete wall by spraying or roller coating, and then apply the mixed surface coating to the primer by roller coating or spraying.

[0132] Comparative Example 1: The primer in Example 1 of the present invention was applied twice on the aluminum formwork concrete wall.

[0133] Comparative Example 2: The surface coating in Example 1 of the present invention was applied twice on the aluminum formwork concrete wall.

[0134] Comparative Example 3: A well-known brand of single-component concrete interface agent commonly used in the market was selected and applied twice on the aluminum formwork concrete wall.

[0135] Comparative Example 4: A well-known brand of single-component or double-component concrete interface agent commonly used in the market was selected and applied twice on the aluminum formwork concrete wall.

[0136] The performance of the interface agent of the embodiment and the comparative example is tested as shown in the following table:

[0137]

[0138]

[0139] It can be seen from the experimental data in Comparative Table 1 that the interface agent of the present invention is superior to the comparative product in terms of tensile bonding strength, adhesion, alkali resistance and degradation effect on residual release agent.

[0140] It can be seen from Comparative Table 2 that the interface agent embodiment of the present invention has a good degradation effect on the release agent, and no peeling, hollowing and cracking will occur. However, Comparative Examples 1 and 2 have a certain degradation effect on the release agent, but it is not thorough. Comparative Example 3 has a poor degradation effect on the release agent, resulting in a large amount of blistering, peeling, hollowing and cracking. Comparative Example 4 has a poor degradation effect on the release agent, resulting in blistering, a small amount of peeling, hollowing and cracking.

[0141] In order to further demonstrate the excellent performance of the interface agent of the present invention, actual comparison pictures of an interface agent of a certain brand and the interface agent of the present invention on cement board, ceramic tile and glass base surfaces are provided.

[0142] Figure 1 This is a comparison of the actual objects after a certain brand of interface agent (left) and the interface agent of the present invention (right) were soaked in water for two days on the cement board base surface. Figure 1 It can be seen that a certain brand of interface agent has a small amount of peeling phenomenon, while the interface agent of the present invention does not have the peeling phenomenon.

[0143] Figure 2 The following is a comparison of the actual objects after a certain brand of interface agent (left) and the interface agent of the present invention (right) were soaked in water for two days on the base surface of the ceramic tile. Figure 2 It can be seen that the interface agent of a certain brand has a shedding phenomenon, while the interface agent of the present invention does not have a shedding phenomenon.

[0144] Figure 3 The following is a comparison of the glass substrate after being soaked in water for two days using a certain brand of interface agent (left) and the interface agent of the present invention (right). Figure 3 It can be seen that a certain brand of interface agent has hollowing and wrinkling phenomena, while the interface agent of the present invention does not have hollowing and wrinkling phenomena.

[0145] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A special interface agent for crack-resistant aluminum formwork concrete. It is characterized in that Including primer and topcoat; The bottom coating is composed of the following raw materials by weight: 20-30 parts of water, 0.1-0.2 parts of hydroxypropyl methylcellulose, 2-4 parts of nano aluminum sulfate, 2-4 parts of nano ferric chloride, 1-2 parts of nano carbon fiber, 0.5-1 parts of sulfated castor oil, 2-4 parts of sodium dodecyl sulfonate, 20-30 parts of penetrating anti-alkali bottom sealing emulsion, 20-30 parts of self-made polyvinyl alcohol glutinous rice glue emulsion, 5-10 parts of waste tile powder modified by lime water, 1-2 parts of strong acid resistant penetrant, 2-3 parts of anti-corrosion and moisture-proof modified bamboo fiber, 2-3 parts of anti-corrosion and moisture-proof modified loofah fiber, and 0.3-0.5 parts of defoaming agent; The surface coating is a two-component coating consisting of component A and component B, and the mixing weight ratio of component A to component B is 1:3-3.5; Component A is composed of the following materials by weight: 30-40 parts of water, 0.1-0.2 parts of hydroxypropyl methylcellulose, 1-2 parts of nano silicon dioxide, 20-30 parts of organosilicon modified polyurethane emulsion, 20-30 parts of penetrating anti-alkali backing emulsion, 3-5 parts of lime milk solution, and 1-2 parts of strong alkali resistant penetrating wetting agent; Component B is composed of the following materials by weight: 30-40 parts of sulphoaluminate cement, 30-40 parts of lime water modified waste tile powder, 10-20 parts of quartz sand, 1-2 parts of borax, 1-2 parts of trisodium phosphate, 3-5 parts of nano-alumina, 3-5 parts of microsilica powder, 2-3 parts of anti-corrosion and moisture-proof modified bamboo fiber, and 2-3 parts of anti-corrosion and moisture-proof modified loofah fiber; Modification of waste tile powder: First, clean the waste tiles and soak them in 10% lime water solution for 10 hours, then dry and crush them into 80-100 mesh tile powder particles; Modification of bamboo fiber: first cut the bamboo into small pieces of 2-5mm in length, put them into a hot grinder after steaming and grind them into bamboo fiber, and then evenly spray a mixed aqueous solution of elastic polyurethane emulsion and VAE emulsion that can be cured into a film on them after drying, so that the solution can be fully coated on the bamboo fiber, and after the film is completely cured and dried, it can be made into 2-5mm fiber; Modification of loofah fiber: first cut the loofah into small pieces of 2-5 mm, then soak it in a 30% elastic polyurethane aqueous solution that can be cured into a film, let the solution fully coat the loofah fiber, and then dry it to make a loofah fiber with a length of 2-5 mm; The production method of homemade polyvinyl alcohol glutinous rice glue emulsion: use 10 parts of pure water to add 2 parts of glutinous rice flour, 0.5 parts of sweet potato flour, and 0.5 parts of 17-99 model polyvinyl alcohol powder, stir evenly, heat to 95-100 degrees for gelatinization for 40-50 minutes, then cool to 50-70 degrees, slowly add 0.3 parts of hydrochloric acid and react for 30 minutes, then cool to 40 degrees, add 0.3 parts of silane coupling agent, 0.7 parts of 10% lime milk solution, and 3 parts of VAE emulsion, and react for 30 minutes.

2. The special interface agent for crack-resistant aluminum formwork concrete according to claim 1, It is characterized in that The nano silicon dioxide is selected from a nano silicon dioxide solution with a particle size of 20-30 nanometers and a content of 10%.

3. The special interface agent for crack-resistant aluminum formwork concrete according to claim 1, It is characterized in that The nano carbon fiber is carbon fiber with a particle size of 80-100 nanometers.

4. The special interface agent for crack-resistant aluminum formwork concrete according to claim 1, It is characterized in that The nano aluminum sulfate is nano aluminum sulfate with a particle size of 30-50 nanometers; the nano ferric chloride is nano ferric chloride with a particle size of 30-50 nanometers.

5. The special interface agent for anti-cracking aluminum formwork concrete according to any one of claims 1 to 4, It is characterized in that Preparation method of base coating: slowly add hydroxypropyl methylcellulose, nano aluminum sulfate, nano ferric chloride, and nano carbon fiber into water in sequence, disperse and stir at a speed of 800-100 rpm for 30 minutes, then add sulfated castor oil, sodium dodecyl sulfate, penetrating anti-alkali bottom sealing emulsion, homemade polyvinyl alcohol glutinous rice glue emulsion, anti-corrosion and moisture-proof modified bamboo fiber, anti-corrosion and moisture-proof modified loofah fiber, lime water modified waste tile powder, strong acid-resistant penetrant, and defoaming agent in sequence at a speed of 200-300 rpm and stir evenly.

6. The special interface agent for anti-cracking aluminum formwork concrete according to any one of claims 1 to 4, It is characterized in that Preparation method of surface coating: Component A is to add hydroxypropyl methylcellulose and nano silicon dioxide in water in sequence, disperse at a speed of 800-100 rpm for 30 minutes, then disperse at a speed of 200-300 rpm, add silicone modified polyurethane emulsion, penetrating anti-alkali bottom emulsion, lime milk solution, and strong alkali-resistant penetrating wetting agent in sequence and stir evenly; Component B is to mix all the components thoroughly and evenly. When using, first pour 3-3.5 parts of component B into one part of component A, stir evenly and it can be used.

Citation Information

Patent Citations

  • Architectural transparent colored alkali-resistant primer

    CN105176271A

  • Fabricated building wet joint concrete interface agent and preparation method

    CN112341140A

  • Direct coating type multifunctional interface agent

    CN112812633A

  • Aluminum mold concrete interface agent and preparation method thereof

    CN115216167A

  • Sound-insulation anti-crack damping floor coating and preparation method thereof

    CN118064012A