A method for preparing durable flame-retardant polyester / cotton blended fabric by in-situ deposition

By using dicyandiamide and tetrahydroxymethylphosphorus chloride in polyester blended fabrics with cyclic phosphate flame retardant FRC-1, an insoluble precipitate was generated, which solved the long-lasting flame retardant properties of polyester/cotton blended fabrics. The problem of poor performance has achieved efficient flame retardant performance and water washing resistance, which is suitable for industrial applications.

CN118547503BActive Publication Date: 2024-11-19JIANGSU HENGLI CHEM FIBER
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411020277.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-19
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

The flame retardant properties of existing polyester/cotton blended fabrics have poor durability and low wash resistance, making them difficult to widely use in clothing and decoration fields.

Method used

The system is composed of dicyandiamide aqueous solution, which is composed of tetrahydroxymethylphosphorus phosphorus chloride and cyclic phosphate flame retardant FRC-1 and polyester/cotton blended fabric. After oscillation, pre-baking and baking treatment, an insoluble precipitate is generated to ensure that The surface and interior of cotton fiber and polyester fiber are dispersed and precipitated to enhance flame retardant properties.

Benefits of technology

The produced long-lasting flame retardant polyester/cotton blended fabric is still less than 14.3cm after 55 washes, and the ultimate oxygen index is no less than 28.5%. It has excellent flame retardant and water-resistant properties, and is suitable for large-scale industrial applications. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118547503B_ABST
    Figure CN118547503B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of polyester / cotton blended fabric modification, and relates to a durable flame-retardant polyester / cotton blended fabric and an in-situ deposition preparation method. The durable flame-retardant polyester / cotton blended fabric is mainly composed of a polyester / cotton blended fabric and an insoluble precipitate dispersed on the surface and inside of a cotton fiber and a polyester fiber at the same time, and the insoluble precipitate is generated by combining a cyclic phosphate flame retardant FRC-1 and a tetrakis(hydroxymethyl)phosphonium chloride-dicyandiamide condensate through electrostatic attraction. The in-situ deposition preparation method is: tetrakis(hydroxymethyl)phosphonium chloride, a cyclic phosphate flame retardant FRC-1 and a polyester / cotton blended fabric are simultaneously added to an aqueous solution of dicyandiamide to obtain a system consisting of a flame retardant liquid and a polyester / cotton blended fabric, and after oscillation, the system is pre-baked and baked in sequence to obtain a durable flame-retardant polyester / cotton blended fabric. The durable flame-retardant polyester / cotton blended fabric of the present invention has excellent flame retardant properties and water washability, mild preparation conditions, simple process, and is suitable for large-scale industrial applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polyester / cotton blended fabric modification, and in particular relates to a durable flame-retardant polyester / cotton blended fabric and an in-situ deposition preparation method. Background Art

[0002] Polyester / cotton blended fabrics not only have the advantages of high strength, good abrasion resistance, high color fastness, good acid and heat resistance, but also have excellent moisture absorption, breathability, soft and comfortable feel and other wearing properties, and are widely used in the clothing industry and decoration field. However, polyester / cotton blended fabrics are extremely flammable and easy to cause fires due to the "wick effect" during combustion, which limits their application. It is necessary to modify polyester / cotton blended fabrics to be flame retardant.

[0003] The difficulty of durable flame retardant finishing of polyester / cotton fabric is much more difficult than that of pure cotton and pure polyester fabric. It is not possible to achieve durable flame retardant effect by mixing cotton fabric durable flame retardant finishing agent and polyester durable flame retardant finishing agent. For example, Reference 1 ("Durable flame retardant finishing process of polyester-cotton fabric", Miao Yuzhen, Printing and Dyeing, 2003, 29(2):18-19) uses pure cotton durable flame retardant finishing agent FK-103 and polyester durable flame retardant finishing agent FK-106 mixed, and then achieves flame retardant effect through resin finishing. However, this flame retardant polyester-cotton fabric loses its flame retardant effect after two washings, and the damaged length exceeds 15cm.

[0004] There are also some studies on flame retardant finishing of polyester / cotton blended fabrics in the prior art. For example, Reference 2 (“Durable halogen-free flame retardant finishing of polyester / cotton blended fabrics”, Li Qianglin et al., Printing and Dyeing, 2015, 41(11):5-9) uses hydrophobic phosphorus nitrogen silicon flame retardant PNSI, water-based polyurethane, etc. as raw materials to prepare a flame retardant coating agent, and coats polyester and cotton. However, the flame retardant effect is lost after washing, and the burning rate is high in the horizontal combustion test. Reference 3 (“Application performance of new flame retardants on polyester-cotton 70 / 30 knitted fabrics”, Wang Fei et al., Dyeing and Finishing Technology, 2021, 43(5):39-41) uses two organic phosphorus flame retardants 1# and 2# and a crosslinking agent 3# to perform flame retardant finishing on polyester-cotton 70 / 30 knitted fabrics. However, this flame retardant finished fabric can only withstand 20 washes.

[0005] It can be seen from this that the shortcomings of the polyester / cotton blended fabric in the prior art are: low water washing resistance and poor flame retardant durability.

[0006] Therefore, it is necessary to develop a new flame retardant polyester / cotton blended fabric to improve the flame retardant durability of the polyester / cotton blended fabric. Summary of the invention

[0007] The purpose of the present invention is to solve the problems existing in the prior art and provide a method for preparing a durable flame-retardant polyester / cotton blended fabric by in-situ deposition.

[0008] To achieve the above object, the technical solution adopted by the present invention is as follows:

[0009] A method for preparing a durable flame-retardant polyester / cotton blended fabric by in-situ deposition, comprising: adding tetrakis(hydroxymethyl)phosphonium chloride, cyclic phosphate flame retardant FRC-1 and polyester / cotton blended fabric to an aqueous solution of dicyandiamide to obtain a system consisting of a flame-retardant liquid and the polyester / cotton blended fabric, shaking the system at 60-70°C, pre-baking the system at 70-80°C and baking the system at 150-165°C to obtain a durable flame-retardant polyester / cotton blended fabric.

[0010] The following changes occur during the above “oscillation” process:

[0011] ① Dicyandiamide, tetrakis(hydroxymethyl)phosphonium chloride, and cyclic phosphate flame retardant FRC-1 adhere to the surface of cotton fiber and polyester fiber and diffuse into the inside of cotton fiber and polyester fiber;

[0012] ② On the surface of cotton fiber and polyester fiber or inside of cotton fiber and polyester fiber, the hydroxymethyl group of tetrakis(hydroxymethyl)phosphonium chloride reacts with the amino group and cyano group of dicyandiamide to generate tetrakis(hydroxymethyl)phosphonium chloride-dicyandiamide condensation product rich in cationic amino groups;

[0013] ③ On the surface of cotton fiber and polyester fiber or inside of cotton fiber and polyester fiber, the acidic substance cyclic phosphate flame retardant FRC-1 (FRC-1 is synthesized using phosphorus oxychloride and the like during the synthesis process and is acidic, indicating that its structure contains anionic phosphate) and tetrakis(hydroxymethyl)phosphonium chloride-dicyandiamide condensation product combine through electrostatic attraction to form an insoluble precipitate;

[0014] ④ The surface of the insoluble precipitate is rich in cyclic phosphate structures, which have a strong affinity with polyester fibers, and the two are combined through the principle of "like dissolves like";

[0015] The following changes will occur during the above-mentioned "pre-baking" and "baking" processes:

[0016] ① Dicyandiamide, tetrakis(hydroxymethyl)phosphonium chloride, and cyclic phosphate flame retardant FRC-1 attached to the surface of cotton and polyester fibers diffuse into the interior of cotton and polyester fibers;

[0017] ② On the surface of cotton fiber and polyester fiber or inside of cotton fiber and polyester fiber, the hydroxymethyl group of tetrakis(hydroxymethyl)phosphonium chloride reacts with the amino group and cyano group of dicyandiamide to generate tetrakis(hydroxymethyl)phosphonium chloride-dicyandiamide condensation product rich in cationic amino groups;

[0018] ③ On the surface of cotton fiber and polyester fiber or inside of cotton fiber and polyester fiber, the acidic substance cyclic phosphate flame retardant FRC-1 and tetrakis(hydroxymethyl)phosphonium chloride-dicyandiamide condensation product combine through electrostatic attraction to form an insoluble precipitate;

[0019] ④ The surface of the insoluble precipitate is rich in cyclic phosphate structures, which have a strong affinity with polyester fibers, and the two are combined through the principle of "like dissolves like";

[0020] Therefore, in the final durable flame-retardant polyester / cotton blended fabric, insoluble precipitates are dispersed on the surface and inside of the cotton fiber and the polyester fiber. The insoluble precipitates inside the cotton fiber and the polyester fiber are difficult to separate from the fiber due to size reasons. In particular, the insoluble precipitates inside the polyester fiber can also combine with the polyester fiber, so it is more difficult to separate from the fiber. Although the insoluble precipitates outside the cotton fiber and the polyester fiber are exposed, they can combine with the polyester fiber, so they will not be easily separated from the fiber. At the same time, the phosphate structure and the dicyandiamide nitrogen-containing structure in the insoluble precipitate can produce a synergistic flame retardant effect, with high flame retardant efficiency, so the durable flame-retardant polyester / cotton blended fabric has excellent flame retardant properties and water-resistant properties.

[0021] As the preferred technical solution:

[0022] In the above-mentioned method for preparing a durable flame-retardant polyester / cotton blended fabric by in-situ deposition, in the flame retardant liquid, the concentration of tetrakishydroxymethylphosphonium chloride is 100-200 g / L, the concentration of dicyandiamide is 50-100 g / L, and the concentration of cyclic phosphate flame retardant FRC-1 is 80-120 g / L.

[0023] In the above-mentioned method for preparing durable flame-retardant polyester / cotton blended fabric by in-situ deposition, the ratio of polyester / cotton blended fabric to flame-retardant liquid is 1g:30-40mL. The larger the bath ratio, the more conducive it is to uniformly treat the polyester / cotton blended fabric, but too high a bath ratio will result in waste.

[0024] In the above-mentioned method for preparing durable flame-retardant polyester / cotton blended fabric by in-situ deposition, the content of polyester in the polyester / cotton blended fabric is 20-80wt%.

[0025] In the above-mentioned method for preparing durable flame-retardant polyester / cotton blended fabric by in-situ deposition, the oscillation treatment adopts XW-ZDR oscillating dyeing machine (Jingjiang Xinwang), the oscillation treatment time is 30-50 minutes, and the oscillation treatment frequency is 80-100 times / minute.

[0026] In the above-mentioned method for preparing durable flame-retardant polyester / cotton blended fabric by in-situ deposition, the pre-drying time is 2-3 minutes.

[0027] In the above-mentioned method for preparing durable flame-retardant polyester / cotton blended fabric by in-situ deposition, the baking time is 3-5 minutes.

[0028] The present invention also provides a durable flame retardant polyester / cotton blended fabric prepared by the method for preparing a durable flame retardant polyester / cotton blended fabric by in-situ deposition as described in any of the above items, which mainly consists of the polyester / cotton blended fabric and an insoluble precipitate dispersed on the surface and inside of the cotton fiber and the polyester fiber at the same time, and the insoluble precipitate is generated by combining the cyclic phosphate flame retardant FRC-1 and the tetrakishydroxymethylphosphonium chloride-dicyandiamide condensation product through electrostatic attraction.

[0029] As the preferred technical solution:

[0030] The durable flame retardant polyester / cotton blended fabric as described above has a limiting oxygen index of not less than 28.5%, a damaged length of not more than 11.1 cm, and after 55 times of washing, the damaged length is still less than 14.3 cm, and has excellent flame retardant properties and washability.

[0031] Beneficial effects:

[0032] 1. In the durable flame-retardant polyester / cotton blended fabric prepared by the present invention, insoluble precipitates are dispersed on the surface and inside of the cotton fiber and the polyester fiber. The surface of the insoluble precipitate is rich in cyclic phosphate structures. These cyclic phosphate structures have a strong affinity with the polyester fiber. The two are firmly combined through the "like dissolves like" principle, thereby producing excellent water washing resistance. At the same time, the phosphate structure and the dicyandiamide nitrogen-containing structure in the insoluble precipitate can produce a synergistic flame retardant effect, thereby producing excellent flame retardant performance.

[0033] 2. The long-lasting flame-retardant polyester / cotton blended fabric prepared by the present invention has a limiting oxygen index of not less than 28.5%, a damaged length of not more than 11.1 cm, and a damaged length of still less than 14.3 cm after 55 times of washing.

[0034] 3. The present invention uses water as a solvent when preparing the flame retardant liquid, and the baking conditions are relatively mild, the operation is simple, and it is suitable for large-scale industrial applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is a surface morphology of the durable flame retardant polyester / cotton blended fabric of Example 1 of the present invention;

[0036] Figure 2 This is a result diagram of a vertical burning test (damage length) of a polyester / cotton blended fabric according to Example 3 of the present invention;

[0037] Figure 3 This is a result diagram of a vertical burning test (damage length) of a durable flame retardant polyester / cotton blended fabric according to Example 3 of the present invention;

[0038] Figure 4 This is the infrared spectrum of the insoluble precipitate of Example 1 of the present invention. DETAILED DESCRIPTION

[0039] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0040] The following are the test methods for the relevant performance indicators in each embodiment and comparative example:

[0041] Limiting oxygen index: Tested in accordance with GB / T 5454-1997 "Oxygen Index Method for Textile Combustion Performance Test".

[0042] Damage length: Tested in accordance with GB / T 5455-2014 “Determination of vertical damage length, smoldering and afterflaming time of textile combustion performance”.

[0043] Damaged length of fabric after 55 washes: first wash the fabric 55 times with reference to AATCC 61-2013 "Accelerated test for color fastness to household and commercial washing" standard, and then test the damaged length of the fabric with reference to GB / T 5455-2014 "Determination of damage length in vertical direction, smoldering and afterflaming time of textile combustion performance" standard.

[0044] Example 1

[0045] A method for preparing a durable flame-retardant polyester / cotton blended fabric by in-situ deposition, the specific steps are as follows:

[0046] (1) Preparation of raw materials;

[0047] An aqueous solution of dicyandiamide;

[0048] Tetrakis hydroxymethyl phosphonium chloride;

[0049] Cyclic phosphate flame retardant FRC-1 (manufacturer: Changzhou Inreg New Materials Co., Ltd.);

[0050] Polyester / cotton blended fabric: The content of polyester is 65wt%;

[0051] (2) Tetrakis(hydroxymethyl)phosphonium chloride, cyclic phosphate flame retardant FRC-1 and polyester / cotton blended fabric were simultaneously added to an aqueous solution of dicyandiamide to obtain a system consisting of a flame retardant liquid and a polyester / cotton blended fabric, and then the system was subjected to an oscillation treatment at a temperature of 65°C and a frequency of 90 times / min for 40 min, and then pre-baked at 75°C for 2.5 min and baked at 160°C for 4 min to obtain a durable flame retardant polyester / cotton blended fabric; wherein the concentration of tetrakis(hydroxymethyl)phosphonium chloride in the flame retardant liquid was 150 g / L, the concentration of dicyandiamide was 75 g / L, and the concentration of cyclic phosphate flame retardant FRC-1 was 100 g / L; and the ratio of the polyester / cotton blended fabric to the flame retardant liquid was 1 g:40 mL.

[0052] The surface morphology of the finally obtained durable flame retardant polyester / cotton blended fabric is as follows: Figure 1 As shown; the durable flame retardant polyester / cotton blended fabric is mainly composed of polyester / cotton blended fabric and insoluble precipitates dispersed on the surface and inside of cotton fiber and polyester fiber, and the insoluble precipitates are generated by the combination of cyclic phosphate flame retardant FRC-1 and tetrakis(hydroxymethyl)phosphonium chloride-dicyandiamide condensate through electrostatic attraction; the limiting oxygen index of the durable flame retardant polyester / cotton blended fabric is 30.9%, and the damaged length is 10.1cm; the damaged length of the durable flame retardant polyester / cotton blended fabric after 55 times of washing is 13.4cm.

[0053] In order to prove that insoluble precipitates are indeed generated during the above oscillation process, the following experiment is conducted:

[0054] After adding tetrakis(hydroxymethyl)phosphonium chloride and cyclic phosphate flame retardant FRC-1 to an aqueous solution of dicyandiamide to obtain a flame retardant liquid, the solution was first subjected to oscillation treatment at a temperature of 65°C and a frequency of 90 times / min for 40 minutes, and then freeze-dried to obtain a precipitate, which was then purified and dried to obtain an insoluble precipitate; wherein, in the flame retardant liquid, the concentration of tetrakis(hydroxymethyl)phosphonium chloride was 150 g / L, the concentration of dicyandiamide was 75 g / L, and the concentration of cyclic phosphate flame retardant FRC-1 was 100 g / L;

[0055] The infrared spectrum of the insoluble precipitate obtained above is as follows Figure 4 As shown, it can be seen that the insoluble precipitate is indeed generated by the combination of the acidic substance cyclic phosphate flame retardant FRC-1 and tetrakis(hydroxymethyl)phosphonium chloride-dicyandiamide condensate through electrostatic attraction, and the surface is indeed rich in cyclic phosphate structures.

[0056] Comparative Example 1

[0057] A method for preparing a flame retardant polyester / cotton blended fabric is basically the same as that in Example 1, except that the temperature of the oscillation treatment in step (2) is 45°C.

[0058] The damaged length of the flame-retardant polyester / cotton blended fabric finally obtained was 11.8 cm, and the damaged length was 30 cm after 55 times of washing.

[0059] Compared with Example 1, the flame retardant and durable performance of Comparative Example 1 is significantly worse. This is because the temperature of the oscillation treatment in Comparative Example 1 is too low, resulting in the inability of dicyandiamide, tetrakis(hydroxymethyl)phosphonium chloride, and cyclic phosphate flame retardant FRC-1 to fully adhere to the surface of cotton fiber and polyester fiber and diffuse into the fiber interior, and only insoluble precipitates are generated on the surface of polyester / cotton blended fabrics. In the washing process, the insoluble precipitates are easily taken away by the washing liquid, resulting in the loss of flame retardant effect; at the same time, the temperature is too low to slow down the condensation reaction rate between the hydroxymethyl of tetrakis(hydroxymethyl)phosphonium chloride and the amino and cyano groups of dicyandiamide, and the amount of tetrakis(hydroxymethyl)phosphonium chloride-dicyandiamide condensate rich in cationic amino groups is reduced; in addition, the too low temperature condition is not conducive to the acidic substance cyclic phosphate flame retardant FRC-1 and the tetrakis(hydroxymethyl)phosphonium chloride-dicyandiamide condensate to fully combine through electrostatic attraction to form an insoluble precipitate, thereby affecting the amount of insoluble precipitates generated on the fiber surface and inside, resulting in a decrease in flame retardant performance, and ultimately resulting in a significant increase in the damaged length of the flame-retardant polyester / cotton blended fabric after 55 washings.

[0060] Comparative Example 2

[0061] A method for preparing a flame retardant polyester / cotton blended fabric is basically the same as Example 1, except that the cyclic phosphate flame retardant FRC-1 is replaced by an equal mass of trimethyl phosphate.

[0062] The damaged length of the flame-retardant polyester / cotton blended fabric finally obtained was 10.7 cm, and the damaged length was 30 cm after 55 times of washing.

[0063] Compared with Example 1, the flame retardant and durable performance of Comparative Example 2 is significantly deteriorated. This is because trimethyl phosphate cannot react with tetrakis(hydroxymethyl)phosphonium chloride-dicyandiamide condensation product to form an insoluble precipitate, cannot produce precipitation inside and on the surface of the fiber, and has poor affinity with the fiber. After 55 times of water washing, the damaged length is significantly increased, and the flame retardant and durable performance is deteriorated.

[0064] Example 2

[0065] A method for preparing a durable flame-retardant polyester / cotton blended fabric by in-situ deposition, the specific steps are as follows:

[0066] (1) Preparation of raw materials;

[0067] Aqueous solution of dicyandiamide

[0068] Tetrakis hydroxymethyl phosphonium chloride;

[0069] Cyclic phosphate flame retardant FRC-1 (manufacturer: Changzhou Inreg New Materials Co., Ltd.);

[0070] Polyester / cotton blended fabric: the content of polyester is 80wt%;

[0071] (2) Tetrakis(hydroxymethyl)phosphonium chloride, cyclic phosphate flame retardant FRC-1 and polyester / cotton blended fabric were simultaneously added to an aqueous solution of dicyandiamide to obtain a system consisting of a flame retardant liquid and a polyester / cotton blended fabric, and then the system was subjected to an oscillation treatment at a temperature of 62°C and a frequency of 85 times / min for 45 min, and then pre-baked at 73°C for 2.7 min and baked at 155°C for 4.5 min to obtain a durable flame retardant polyester / cotton blended fabric; wherein the concentration of tetrakis(hydroxymethyl)phosphonium chloride in the flame retardant liquid was 130 g / L, the concentration of dicyandiamide was 60 g / L, and the concentration of cyclic phosphate flame retardant FRC-1 was 90 g / L; and the ratio of the polyester / cotton blended fabric to the flame retardant liquid was 1 g:35 mL.

[0072] The finally obtained durable flame retardant polyester / cotton blended fabric is mainly composed of polyester / cotton blended fabric and insoluble precipitates dispersed on the surface and inside of cotton fiber and polyester fiber. The insoluble precipitates are generated by the combination of cyclic phosphate flame retardant FRC-1 and tetrakis(hydroxymethyl)phosphonium chloride-dicyandiamide condensation product through electrostatic attraction; the limiting oxygen index of the durable flame retardant polyester / cotton blended fabric is 29.8%, and the damaged length is 10.5 cm; the damaged length of the durable flame retardant polyester / cotton blended fabric after 55 times of washing is 13.8 cm.

[0073] Example 3

[0074] A method for preparing a durable flame-retardant polyester / cotton blended fabric by in-situ deposition, the specific steps are as follows:

[0075] (1) Preparation of raw materials;

[0076] Aqueous solution of dicyandiamide

[0077] Tetrakis hydroxymethyl phosphonium chloride;

[0078] Cyclic phosphate flame retardant FRC-1 (manufacturer: Changzhou Inreg New Materials Co., Ltd.);

[0079] Polyester / cotton blended fabric: Limiting oxygen index is 20.1%, damage length is 30cm, polyester content is 50wt%;

[0080] (2) Tetrakis(hydroxymethyl)phosphonium chloride, cyclic phosphate flame retardant FRC-1 and polyester / cotton blended fabric were simultaneously added to an aqueous solution of dicyandiamide to obtain a system consisting of a flame retardant liquid and a polyester / cotton blended fabric, and then the system was subjected to an oscillation treatment at a temperature of 60°C and a frequency of 80 times / min for 50 min, and then pre-baked at 70°C for 3 min and baked at 150°C for 5 min to obtain a durable flame retardant polyester / cotton blended fabric; wherein the concentration of tetrakis(hydroxymethyl)phosphonium chloride in the flame retardant liquid was 100 g / L, the concentration of dicyandiamide was 50 g / L, and the concentration of cyclic phosphate flame retardant FRC-1 was 80 g / L; and the ratio of the polyester / cotton blended fabric to the flame retardant liquid was 1 g:30 mL.

[0081] The finally obtained durable flame retardant polyester / cotton blended fabric is mainly composed of polyester / cotton blended fabric and insoluble precipitates dispersed on the surface and inside of cotton fibers and polyester fibers. The insoluble precipitates are generated by the combination of cyclic phosphate flame retardant FRC-1 and tetrakis(hydroxymethyl)phosphonium chloride-dicyandiamide condensation product through electrostatic attraction; the limiting oxygen index of the durable flame retardant polyester / cotton blended fabric is 28.5%, and the damaged length is 11.1 cm; the damaged length of the durable flame retardant polyester / cotton blended fabric after 55 times of washing is 14.3 cm.

[0082] The vertical burning test results of the raw materials (polyester / cotton blended fabric) used in this example are as follows: Figure 2 As shown, the vertical combustion test results of the durable flame retardant polyester / cotton blended fabric prepared in this embodiment are as follows Figure 3 As shown, from Figure 2 It can be seen that the raw polyester / cotton blended fabric was completely destroyed after the vertical burning test, while Figure 3 The durable flame retardant polyester / cotton blended fabric prepared in this embodiment showed good flame retardant effect in the vertical burning test, and the degree of damage was significantly reduced, which fully demonstrated the effectiveness of the in-situ deposition preparation method adopted in this embodiment in improving the flame retardant properties of polyester / cotton blended fabric.

[0083] Example 4

[0084] A method for preparing a durable flame-retardant polyester / cotton blended fabric by in-situ deposition, the specific steps are as follows:

[0085] (1) Preparation of raw materials;

[0086] Aqueous solution of dicyandiamide

[0087] Tetrakis hydroxymethyl phosphonium chloride;

[0088] Cyclic phosphate flame retardant FRC-1 (manufacturer: Changzhou Inreg New Materials Co., Ltd.);

[0089] Polyester / cotton blended fabric: The content of polyester is 65wt%;

[0090] (2) Tetrakis(hydroxymethyl)phosphonium chloride, cyclic phosphate flame retardant FRC-1 and polyester / cotton blended fabric were simultaneously added to an aqueous solution of dicyandiamide to obtain a system consisting of a flame retardant liquid and a polyester / cotton blended fabric, and then the system was subjected to an oscillation treatment at a temperature of 67°C and a frequency of 95 times / min for 35 min, and then pre-baked at 78°C for 2.2 min and baked at 165°C for 3.5 min to obtain a durable flame retardant polyester / cotton blended fabric; wherein the concentration of tetrakis(hydroxymethyl)phosphonium chloride in the flame retardant liquid was 175 g / L, the concentration of dicyandiamide was 90 g / L, and the concentration of cyclic phosphate flame retardant FRC-1 was 110 g / L; and the ratio of the polyester / cotton blended fabric to the flame retardant liquid was 1 g:35 mL.

[0091] The finally obtained durable flame retardant polyester / cotton blended fabric is mainly composed of polyester / cotton blended fabric and insoluble precipitates dispersed on the surface and inside of cotton fiber and polyester fiber. The insoluble precipitates are generated by the combination of cyclic phosphate flame retardant FRC-1 and tetrakis(hydroxymethyl)phosphonium chloride-dicyandiamide condensation product through electrostatic attraction; the limiting oxygen index of the durable flame retardant polyester / cotton blended fabric is 31.7%, and the damaged length is 9.7 cm; the damaged length of the durable flame retardant polyester / cotton blended fabric after 55 times of washing is 12.9 cm.

[0092] Example 5

[0093] A method for preparing a durable flame-retardant polyester / cotton blended fabric by in-situ deposition, the specific steps are as follows:

[0094] (1) Preparation of raw materials;

[0095] Aqueous solution of dicyandiamide

[0096] Tetrakis hydroxymethyl phosphonium chloride;

[0097] Cyclic phosphate flame retardant FRC-1 (manufacturer: Changzhou Inreg New Materials Co., Ltd.);

[0098] Polyester / cotton blended fabric: the content of polyester is 20wt%;

[0099] (2) Tetrakis(hydroxymethyl)phosphonium chloride, cyclic phosphate flame retardant FRC-1 and polyester / cotton blended fabric were simultaneously added to an aqueous solution of dicyandiamide to obtain a system consisting of a flame retardant liquid and a polyester / cotton blended fabric, and then the system was subjected to an oscillation treatment at a temperature of 70°C and a frequency of 100 times / min for 30 min, and then pre-baked at 80°C for 2 min and baked at 165°C for 3 min to obtain a durable flame retardant polyester / cotton blended fabric; wherein the concentration of tetrakis(hydroxymethyl)phosphonium chloride in the flame retardant liquid was 200 g / L, the concentration of dicyandiamide was 100 g / L, and the concentration of cyclic phosphate flame retardant FRC-1 was 120 g / L; and the ratio of the polyester / cotton blended fabric to the flame retardant liquid was 1 g:40 mL.

[0100] The finally obtained durable flame retardant polyester / cotton blended fabric is mainly composed of polyester / cotton blended fabric and insoluble precipitates dispersed on the surface and inside of cotton fiber and polyester fiber. The insoluble precipitates are generated by the combination of cyclic phosphate flame retardant FRC-1 and tetrakis(hydroxymethyl)phosphonium chloride-dicyandiamide condensation product through electrostatic attraction; the limiting oxygen index of the durable flame retardant polyester / cotton blended fabric is 32.2%, and the damaged length is 9.4 cm; the damaged length of the durable flame retardant polyester / cotton blended fabric after 55 times of washing is 12.7 cm.

Claims

1. A method for preparing durable flame-retardant polyester / cotton blended fabric by in-situ deposition, characterized in that: Tetrakis(hydroxymethyl)phosphonium chloride, cyclic phosphate flame retardant FRC-1 and polyester / cotton blended fabric are simultaneously added to an aqueous solution of dicyandiamide to obtain a system consisting of a flame retardant liquid and a polyester / cotton blended fabric, and then the system is shaken at 60-70°C, and then pre-dried at 70-80°C and baked at 150-165°C to obtain a durable flame retardant polyester / cotton blended fabric. The oscillation treatment time is 30-50 minutes, and the oscillation treatment frequency is 80-100 times / minute; The durable flame retardant polyester / cotton blended fabric mainly consists of the polyester / cotton blended fabric and insoluble precipitates dispersed on the surface and inside of the cotton fiber and the polyester fiber at the same time, and the insoluble precipitates are generated by combining the cyclic phosphate flame retardant FRC-1 and the tetrakis(hydroxymethyl)phosphonium chloride-dicyandiamide condensate through electrostatic attraction.

2. The method for preparing durable flame-retardant polyester / cotton blended fabric by in-situ deposition according to claim 1, characterized in that: In the flame retardant liquid, the concentration of tetrakis(hydroxymethyl)phosphonium chloride is 100-200 g / L, the concentration of dicyandiamide is 50-100 g / L, and the concentration of cyclic phosphate flame retardant FRC-1 is 80-120 g / L.

3. The method for preparing durable flame-retardant polyester / cotton blended fabric by in-situ deposition according to claim 2, characterized in that: The ratio of polyester / cotton blended fabric to flame retardant liquid is 1g:30-40mL.

4. The method for preparing durable flame-retardant polyester / cotton blended fabric by in-situ deposition according to claim 1, characterized in that: In polyester / cotton blended fabrics, the content of polyester is 20-80wt%.

5. The method for preparing durable flame-retardant polyester / cotton blended fabric by in-situ deposition according to claim 1, characterized in that: The pre-baking time is 2-3 minutes.

6. The method for preparing durable flame-retardant polyester / cotton blended fabric by in-situ deposition according to claim 1, characterized in that: The baking time is 3-5 minutes.

7. A durable flame retardant polyester / cotton blended fabric prepared by the method for preparing a durable flame retardant polyester / cotton blended fabric by in-situ deposition as claimed in any one of claims 1 to 6, characterized in that: The limiting oxygen index of the durable flame retardant polyester / cotton blended fabric is not less than 28.5%, the damaged length is not higher than 11.1cm, and the damaged length is still less than 14.3cm after 55 washes.

Citation Information

Patent Citations

  • Flame-proof treatment method of pure cotton or cotton blended fabric

    CN104611928A

  • Preparation method of phosphorus-nitrogen leather flame-retardant retanning agent

    CN107245537A

  • Acid-methylol compound reaction products for flame resistance

    US20040039085A1