A silicon carbide power device and a method for preparing the same

By using in-situ doping and patterned mask technology during epitaxy in SiC MOSFET power devices to form the sidewalls of the silicon carbide epitaxial layer, the problem of P-well surface roughness is solved, device performance and reliability are improved, and more uniformity is achieved channel area and higher performance consistency.

CN118553620BActive Publication Date: 2024-10-29XINLIAN POWER TECH (SHAOXING) CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410993137.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-10-29
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

The surface of existing SiC MOSFET power devices is rough due to multiple high-energy ion injections during the P-well formation process, which affects carrier mobility, device performance and reliability.

Method used

The silicon carbide epitaxial layer is formed by in-situ doping during epitaxy, and sidewalls are formed on the sidewalls through patterned mask technology. Conductive type ion implantation is performed to form the JFET region and body region, reducing surface roughness and improving the channel. area size and doping concentration uniformity.

Benefits of technology

It improves the performance and reliability of silicon carbide power devices, reduces the performance differences between different devices, and reduces the risk of exposure equipment identification errors and alarms.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118553620B_ABST
    Figure CN118553620B_ABST
Patent Text Reader

Abstract

The present invention provides a silicon carbide power device and a method for preparing the same. The method for preparing the silicon carbide power device comprises: providing a substrate having a silicon carbide epitaxial layer doped in situ to a first conductivity type during epitaxy; forming a first patterned mask on the silicon carbide epitaxial layer, forming a first sidewall on the sidewall of the opening of the first patterned mask, and using the silicon carbide epitaxial layer under the first sidewall as a channel region; using the first patterned mask and the first sidewall, performing a first ion implantation of a second conductivity type to form a JFET region in the silicon carbide epitaxial layer between the first sidewalls, and using other regions of the silicon carbide epitaxial layer as a body region, and then removing the first patterned mask. In the present invention, the body region is formed by epitaxial in-situ doping to reduce the roughness of the channel surface to improve the performance and reliability of the silicon carbide power device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor technology, and in particular to a silicon carbide power device and a preparation method thereof. Background Art

[0002] SiC MOSFET (Metal Oxide Semiconductor Field Effect Transistor) power devices are widely used in new energy vehicles, transportation rails, photovoltaics and other industries due to their advantages such as high voltage and high temperature resistance, high frequency, low power loss and high switching speed. SiC MOSFET power devices can be divided into planar type (DMOSFET) and trench type (Trench MOSFET) according to their gate structure.

[0003] Taking the N-type planar MOSFET power device as an example, in the related art, its body region (P-well) is usually formed by implanting P-type ions (such as Al ions). Due to the characteristics of silicon carbide materials (Al ions diffuse weakly in silicon carbide materials), ion implantation can only be performed through high-energy ion implantation, and in order to ensure the depth distribution of its ion implantation, multiple Al ion implantations are required to form the required P-well, and then form a channel region in the P-well. However, the above-mentioned multiple high-energy ion implantations make the surface of the formed P-well relatively rough, increase channel scattering, and seriously affect the improvement of the carrier mobility of the channel. In particular, the above-mentioned part of the P-well is located below the gate structure, that is, as the gate oxide channel region, and the surface roughness of the gate oxide channel region will seriously affect the performance and reliability of the device (reliability of the gate oxide). Summary of the invention

[0004] The object of the present invention is to provide a silicon carbide power device and a preparation method thereof, which are used to improve the performance and reliability of the silicon carbide power device by reducing the roughness of the body region surface.

[0005] In order to solve the above technical problems, the present invention provides a method for preparing a silicon carbide power device, comprising:

[0006] Providing a substrate having a silicon carbide epitaxial layer in-situ doped to a first conductivity type during epitaxy;

[0007] Forming a first patterned mask on the silicon carbide epitaxial layer, and forming a first sidewall spacer on the sidewall of the opening of the first patterned mask, and using the silicon carbide epitaxial layer under the first sidewall spacer as a channel region;

[0008] The first patterned mask and the first sidewalls are used to perform a first ion implantation of a second conductivity type to form a JFET region in the silicon carbide epitaxial layer between the first sidewalls, and other regions of the silicon carbide epitaxial layer are used as body regions, and then the first patterned mask is removed.

[0009] Optionally, the silicon carbide power device includes an NMOS device, the first conductivity type is P-type, and the second conductivity type is N-type.

[0010] Optionally, an ion implantation protection layer is further provided between the silicon carbide epitaxial layer and the first patterned mask, and the opening of the first patterned mask exposes the surface of the corresponding ion implantation protection layer.

[0011] Optionally, after removing the first patterned mask, a second sidewall spacer is further formed between the first sidewall spacers, wherein the second sidewall spacer covers the JFET region and exposes the silicon carbide epitaxial layer outside the first sidewall spacer;

[0012] A second ion implantation of the second conductivity type is performed by using the first sidewall spacer and the second sidewall spacer to form a source region in the silicon carbide epitaxial layer, wherein the implantation depth of the source region is less than the thickness of the silicon carbide epitaxial layer.

[0013] Optionally, removing the first side wall and the second side wall;

[0014] forming a second patterned mask, wherein an opening of the second patterned mask exposes a region of the source region away from the JFET region;

[0015] Using the second patterned mask, performing a third ion implantation of the first conductivity type to form a body diode region in the source region;

[0016] A termination structure is formed in a peripheral region of the silicon carbide epitaxial layer.

[0017] Optional,

[0018] Before forming the first patterned mask, forming a third patterned mask to expose a portion of the surface of the silicon carbide epitaxial layer;

[0019] performing a second ion implantation of the second conductivity type to form a source region in the silicon carbide epitaxial layer;

[0020] The third patterned mask is removed, and the first patterned mask, the first sidewall and the JFET region are formed in sequence.

[0021] Optionally, the method further includes forming a gate structure on the surfaces of the JFET region, the channel region and a portion of the source region.

[0022] Optionally, the opening of the first patterned mask exposes an area for forming a terminal structure in addition to an area for forming a JFET area, and when performing the first ion implantation of the second conductivity type, the JFET area and the terminal structure are simultaneously formed in the silicon carbide epitaxial layer.

[0023] According to another aspect of the present invention, there is also provided a silicon carbide power device, comprising a substrate;

[0024] A silicon carbide epitaxial layer disposed on the surface of the substrate has a first conductivity type and is formed by in-situ doping during epitaxy;

[0025] A body region, a JFET region and a channel region are arranged in the silicon carbide epitaxial layer, the JFET region has a second conductivity type, the channel region is arranged in the body region and connected to the JFET region, and the body region and the channel region are composed of part of the silicon carbide epitaxial layer.

[0026] Optionally, the silicon carbide power device includes an NMOS device, the first conductivity type is P-type, the second conductivity type is N-type, and the surface roughness of the channel region is less than or equal to 10 nanometers.

[0027] In summary, the method for preparing a silicon carbide power device provided by the present invention includes providing a substrate having a silicon carbide epitaxial layer doped in situ to a first conductivity type during epitaxy; forming a first patterned mask on the silicon carbide epitaxial layer, forming a first sidewall on the sidewall of the opening of the first patterned mask, and using the silicon carbide epitaxial layer under the first sidewall as a channel region; using the first patterned mask and the first sidewall, performing a first ion implantation of a second conductivity type to form a JFET region in the silicon carbide epitaxial layer between the first sidewalls, and using other regions of the silicon carbide epitaxial layer as a body region, and then removing the first patterned mask. Compared with the silicon carbide layer formed by epitaxy followed by ion implantation, the present invention uses a silicon carbide epitaxial layer formed by in-situ doping during epitaxy, so that it has a lower surface roughness, and the first sidewall of the first patterned mask sidewall is used to self-align and define a channel region in the above silicon carbide epitaxial layer, so that the channel region has better size (length, width and thickness) and uniformity in doping concentration. Therefore, the channel region as a part of the silicon carbide epitaxial layer (directly composed of a part of the silicon carbide epitaxial layer) also has the above advantages. The channel region with lower surface roughness can improve the reliability of the gate dielectric layer located on the channel region to improve the performance and reliability of the power device. The channel region with better size and uniformity of doping concentration can reduce the performance difference between different power devices. In addition, the silicon carbide epitaxial layer with lower surface roughness in the present invention is also conducive to the exposure equipment to identify the lithography mark set on the silicon carbide epitaxial layer, so as to improve the alignment accuracy and reduce the risk of alarm caused by abnormal alignment of the exposure equipment. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Those skilled in the art should understand that the drawings are provided for a better understanding of the present invention, but do not constitute any limitation on the scope of the present invention.

[0029] Figure 1 A flow chart of a method for preparing a silicon carbide power device provided in Example 1;

[0030] Figure 2a A schematic diagram of providing a substrate according to Embodiment 1;

[0031] Figure 2b is a schematic diagram of forming a first patterned mask on a substrate according to Embodiment 1;

[0032] Figure 2c It is a schematic diagram of forming a first sidewall in Embodiment 1;

[0033] Figure 2d It is a schematic diagram of forming a JFET region in Example 1;

[0034] Figure 2e It is a schematic diagram after removing the first patterned mask of Embodiment 1;

[0035] Figure 2f It is a schematic diagram of forming a second sidewall in Embodiment 1;

[0036] Figure 2g is a schematic diagram of forming a source region in Embodiment 1;

[0037] Figure 2h is a schematic diagram of forming a body diode region in Embodiment 1;

[0038] Figure 2i is a schematic diagram of forming a gate structure according to Embodiment 1;

[0039] Figure 2j It is a schematic diagram of forming a silicon carbide power device according to the first embodiment.

[0040] In the accompanying drawings: 10-substrate; 11-first silicon carbide epitaxial layer; 12-second silicon carbide epitaxial layer; 13-third silicon carbide epitaxial layer; 21-first patterned mask; 22-ion implantation protection layer; 23-first side wall; 24-channel region; 25-JFET region; 26-second side wall; 27-source region; 28-body diode region; 29-source; 30-gate structure; 31-gate dielectric layer; 32-gate conductive layer; 33-interlayer dielectric layer; 34-front metal layer; 35-back metal layer. DETAILED DESCRIPTION

[0041] In order to make the purpose, advantages and features of the present invention clearer, the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be noted that the drawings are all in a very simplified form and are not drawn to scale, and are only used to conveniently and clearly assist in explaining the purpose of the embodiments of the present invention. In addition, the structure shown in the drawings is often a part of the actual structure. In particular, the emphasis of each drawing is different, and sometimes different scales are used.

[0042] It should be understood that when an element or layer is referred to as "on...", "connected to" other elements or layers, it can be directly on other elements or layers, connected to other elements or layers, or there can be intervening elements or layers. On the contrary, when an element is referred to as "directly on...", "directly connected to" other elements or layers, there is no intervening element or layer. Although the terms first, second, third, etc. can be used to describe various elements, components, regions, layers and / or parts, these elements, components, regions, layers and / or parts should not be limited by these terms. These terms are only used to distinguish an element, component, region, layer or part from another element, component, region, layer or part. Therefore, without departing from the teachings of the present invention, the first element, component, region, layer or part discussed below can be expressed as a second element, component, region, layer or part. Spatial relationship terms such as "under...", "below", "below", "above...", "above", "above", etc., can be used here for the convenience of description to describe the relationship between an element or feature shown in the figure and other elements or features. It should be understood that, in addition to the orientation shown in the figure, the spatial relationship terms are intended to include different orientations of the devices in use and operation. For example, if the device in the accompanying drawings is turned over, then, the elements or features described as "under...", "below", "below" will be oriented to be "on" other elements or features. The device can be oriented in other ways (rotated 90 degrees or other orientations) and the spatial descriptors used here are interpreted accordingly. The purpose of the terms used here is only to describe specific embodiments and is not intended to be a limitation of the present invention. When used here, the singular forms of "one", "one" and "said / the" are also intended to include plural forms, unless the context clearly indicates another way. It should also be understood that the term "including" is used to determine the existence of features, steps, operations, elements and / or parts, but does not exclude the existence or addition of one or more other features, steps, operations, elements, parts and / or groups. When used here, the term "and / or" includes any and all combinations of the relevant listed items.

[0043] Embodiment 1

[0044] Embodiment 1 provides a method for preparing a silicon carbide power device.

[0045] Figure 1 This is a flow chart of the method for preparing a silicon carbide power device provided in Example 1.

[0046] like Figure 1 As shown, the method for preparing a silicon carbide power device provided in this embodiment includes:

[0047] S01: providing a substrate having a silicon carbide epitaxial layer in-situ doped to a first conductivity type during epitaxy;

[0048] S02: forming a first patterned mask on the silicon carbide epitaxial layer, and forming a first sidewall spacer on the sidewall of the opening of the first patterned mask;

[0049] S03: Using the first patterned mask and the first side wall, perform a first ion implantation of a second conductivity type to form a JFET region in the silicon carbide epitaxial layer between the first side walls, use the silicon carbide epitaxial layer under the first side wall as a channel region, and use other areas of the silicon carbide epitaxial layer as a body region, and then remove the first patterned mask.

[0050] Figures 2a to 2j The structural schematic diagram corresponding to the corresponding steps of the method for preparing the silicon carbide power device provided in this embodiment, next, Figures 2a to 2j The preparation method of the silicon carbide power device is described in detail.

[0051] First, execute step S01, please refer to Figure 2a A substrate 10 is provided, on which a silicon carbide epitaxial layer 13 is in-situ doped to a first conductivity type during epitaxy.

[0052] The material of the substrate 10 can be any suitable base material for epitaxially growing silicon carbide, such as silicon, sapphire or silicon carbide. A silicon carbide epitaxial layer 13 is provided on the surface of the substrate 10, which is epitaxially grown and in-situ doped to a first conductivity type. The first conductivity type is opposite to the conductivity type of the device formed on the silicon carbide epitaxial layer 13. For example, when used to form an N-type power device, the first conductivity type is P-type, and when used to form a P-type power device, the first conductivity type is N-type.

[0053] Between the substrate 10 and the first conductive type silicon carbide epitaxial layer 13, several layers of silicon carbide epitaxial layers of other types are also formed by epitaxial growth and in-situ doping, as or for forming other functional film layers of power devices. In this embodiment, for example, it can be used to form an N-type power device. Three layers of silicon carbide epitaxial layers are sequentially arranged on the substrate 10, namely, the first to third silicon carbide epitaxial layers 11 to 13 that are sequentially away from the substrate 10. The conductivity type of the first silicon carbide epitaxial layer 11 can be N-type and used as a buffer layer, the conductivity type of the second silicon carbide epitaxial layer 12 can be N-type and used as a drift layer, and the conductivity type of the third silicon carbide epitaxial layer 13 can be P-type and used to form a body region. If there is no special explanation, the silicon carbide epitaxial layer mentioned below is the third silicon carbide epitaxial layer 13.

[0054] Next, step S02 is performed to form a first patterned mask 21 on the silicon carbide epitaxial layer 13, and to form a first sidewall spacer 23 on the sidewall of the opening of the first patterned mask 21, and to use the silicon carbide epitaxial layer 13 under the first sidewall spacer 23 as a channel region 24 (corresponding to the A1 region).

[0055] For details, please refer to Figure 2b , a first patterned mask 21 is formed on the silicon carbide epitaxial layer 13, the opening of the first patterned mask 21 exposes the surface of the silicon carbide epitaxial layer 13, and the width is the sum of the width of the JFET region of the power device and the width of the channel region 24 on both sides of the JFET region. The material of the first patterned mask 21 can be any material suitable for being used as a mask, which can be, for example, a film layer composed of one of silicon, silicon nitride, silicon oxide or silicon oxynitride, or a composite film layer composed of multiple materials. In a preferred example, the first patterned mask 21 can be a composite film layer composed of at least two materials, and the opening of the first patterned mask 21 exposes a film layer closest to the silicon carbide epitaxial layer 13, that is, the JFET region to be formed (corresponding to the B1 region) and the surface of the channel region 24 are covered with a film layer as an ion implantation protection layer 22, which is used to reduce the damage of ion implantation to the surface of the silicon carbide epitaxial layer 13 during subsequent ion implantation. Of course, the above-mentioned ion implantation protection layer 22 can also be regarded as a film layer outside the first patterned mask 21.

[0056] Please refer to Figure 2c , a first sidewall 23 is formed on the sidewall of the opening of the first patterned mask 21, and the silicon carbide epitaxial layer 13 under the first sidewall 23 is used as the channel region 24. The step of forming the first sidewall 23 may include: forming a first sidewall 23 material layer to conformally cover the surface of the first patterned mask 21 and the inner wall of the opening, and then performing a dry etching process to remove the first sidewall 23 material layer on the surface of the first patterned mask 21 and the bottom of the opening, and using the remaining first sidewall 23 material layer located on the sidewall of the opening as the first sidewall 23. The silicon carbide epitaxial layer 13 in the area below the bottom of the opening covered by the first sidewall 23 (the bottom edge area of ​​the opening) can be the channel region 24, and the middle area of ​​the first sidewall 23 exposing the bottom of the opening can be the JFET region 25, so the thickness of the first sidewall 23 material layer (or the width of the first sidewall 23) is the width of the channel region 24 on one side. Of course, the channel region 24 is a part of the body region (the silicon carbide epitaxial layer 13 ), and has been actually formed when the first sidewall spacer 23 is defined, while the JFET region 25 is actually formed only after ion implantation.

[0057] It should be noted that, compared with the silicon carbide layer formed by epitaxy and then ion implantation, the present embodiment adopts the silicon carbide epitaxial layer 13 formed by in-situ doping during epitaxy, so that it has a lower surface roughness, and the first sidewall 23 of the sidewall of the first patterned mask 21 is used to self-align and define the channel region 24 on the silicon carbide epitaxial layer 13, so that the channel region 24 has a better size (length, width and thickness) and uniformity in doping concentration. Therefore, the channel region 24 as a part of the silicon carbide epitaxial layer 13 (directly formed by a part of the silicon carbide epitaxial layer 13) also has the above advantages, the channel region 24 with a lower surface roughness can improve the reliability of the gate dielectric layer 31 located on the channel region 24 to improve the performance and reliability of the power device, and the channel region 24 with a better size and uniformity in doping concentration can reduce the performance difference between different power devices. In addition, the silicon carbide epitaxial layer 13 with lower surface roughness in this embodiment is also beneficial for the exposure equipment to identify the photolithography marks provided on the silicon carbide epitaxial layer 13, so as to improve the alignment accuracy and reduce the risk of alarm caused by abnormal alignment of the exposure equipment.

[0058] Next, step S03 is performed to perform a first ion implantation of a second conductivity type using the first patterned mask 21 and the first sidewall 23 to form a JFET region 25 in the silicon carbide epitaxial layer 13 between the first sidewalls 23 and use other regions of the silicon carbide epitaxial layer 13 as body regions, and then remove the first patterned mask 21.

[0059] For details, please refer to Figure 2d , using the first patterned mask 21 and the first sidewall 23, a first ion implantation of the second conductivity type is performed to form a JFET region 25 between the channel regions 24. The conductivity type of the first ion implantation is opposite to the conductivity type of the silicon carbide epitaxial layer 13, that is, the second conductivity type, and the implantation depth of the first ion implantation is greater than or equal to the thickness of the silicon carbide epitaxial layer 13 (the third silicon carbide epitaxial layer 13) to ensure that the JFET region 25 is connected to the second silicon carbide epitaxial layer 13. In this embodiment, the conductivity type of the silicon carbide epitaxial layer 13 may be P type, and the conductivity type of the first ion implantation may be N type.

[0060] Please refer to Figure 2e , remove the first patterned mask 21 to expose the surface of the silicon carbide epitaxial layer 13 or the surface of the ion implantation protection layer 22 , and retain the first sidewall spacer 23 .

[0061] Please refer to Figure 2f, a second sidewall 26 is formed between the first sidewalls 23, the second sidewall 26 covers the JFET region 25, and exposes the silicon carbide epitaxial layer 13 or the ion implantation protection layer 22 outside the first sidewall 23. The step of forming the second sidewall 26 may include: forming a second sidewall material layer to conformally cover the surface of the ion implantation protection layer 22 and the outer wall of the first sidewall 23, until the second sidewall material layer is closed (merged) in the area between the first sidewalls 23, and then performing a dry etching process to etch the second sidewall material layer, remove the second sidewall material layer outside the first sidewall 23, and retain the second sidewall material layer covering the first sidewall 23 and the JFET region 25, and serve as the second sidewall 26. Of course, if the remaining second sidewall material layer does not completely cover the JFET region 25 after performing a second sidewall material layer formation process and a dry etching process, the second sidewall material layer formation process (deposition process) and a dry etching process may be continued at least once. It should be particularly noted here that, in practice, after etching the second sidewall material layer, a partial thickness of the second sidewall material layer is still retained on the outer side of the first sidewall 23 (away from the JFET region 25 ), which is equivalent to the thickness of the first sidewall 23 becoming thicker, that is, the width of the channel region 24 is slightly widened. The actual width of the channel region 24 is the sum of the thickness of the first sidewall 23 and the thickness of the second sidewall retained on the outer side of the first sidewall 12 .

[0062] Please refer to Figure 2g , a second ion implantation of a second conductivity type is performed using the first sidewall 23 and the second sidewall 26 to form a source region 27 in the silicon carbide epitaxial layer 13. The conductivity type of the second ion implantation is the same as the conductivity type of the first ion implantation (JFET region 25), but the ion concentration of the second ion implantation is greater than the ion concentration of the first ion implantation, and the implantation depth of the second ion implantation is less than the thickness of the silicon carbide epitaxial layer 13, that is, the implantation depth of the second ion implantation is less than the implantation depth of the first ion implantation. Therefore, compared with using multiple masks to define the above-mentioned channel region 24, JFET region 25 and source region 27 respectively, in the present embodiment, only one mask (a mask corresponding to the first patterned mask 21) can be used to define the channel region 24, JFET region 25 and source region 27 in sequence in the silicon carbide epitaxial layer 13 by using the first side wall 23 and the second side wall 26. Not only can the above-mentioned double self-alignment process be used to achieve accurate definition of the above-mentioned regions (channel region 24, JFET region 25 and source region 27) and high consistency between various products, but also the mask (photomask) investment and the number of photolithography times can be reduced, thereby effectively reducing the wafer production cost.

[0063] Please refer to Figure 2h, remove the first side wall 23, the second side wall 26 and the ion implantation protection layer 22 to expose the surface of the silicon carbide epitaxial layer 13, and sequentially form a body diode region 28 and a terminal structure (not shown in the figure) in the source region 27 away from the channel region 24 (JFET region 25), and use the source region 27 between the channel region 24 and the body diode region 28 as the source 29, and the terminal structure is located in the peripheral area of ​​the device structure in the silicon carbide epitaxial layer 13. Specifically, after removing the first side wall 23 and the second side wall 26, a second patterned mask is formed, and the opening of the second patterned mask exposes the area of ​​the source region 27 away from the JFET region 25, that is, exposes the area for forming the body diode; using the second patterned mask, a third ion implantation of the first conductivity type is performed to form a body diode region 28 in the source region 27, and the body diode region 28 is connected to the silicon carbide epitaxial layer 13. The conductivity type of the ions implanted in the body diode region is the same as the conductivity type of the silicon carbide epitaxial layer 13, and is opposite to the conductivity type of the source region 27. The body diode region 28 can be a high-concentration (heavily doped) first conductivity type, which can make the P-well region (body region) and the source region 27 have the same potential.

[0064] Please refer to Figure 2i A gate structure 30 is formed on the surface of the silicon carbide epitaxial layer 13 . The gate structure 30 may include a gate dielectric layer 31 covering the surface of the JFET region 25 , the channel region 24 and a portion of the source 29 (source region 27 ), and a gate conductive layer 32 disposed on the gate dielectric layer 31 .

[0065] Please refer to Figure 2j In fact, the manufacturing process of the silicon carbide power device may also include the steps of forming an interlayer dielectric layer 33 to cover the silicon carbide epitaxial layer 13 and the gate structure 30, forming a front metal layer 34 on the silicon carbide epitaxial layer 13 and the interlayer dielectric layer 33, and removing the substrate 10 to form a back metal layer 35 on the back side of the silicon carbide epitaxial layer 13, which will not be elaborated here.

[0066] Embodiment 2

[0067] Embodiment 2 provides a method for preparing a silicon carbide power device.

[0068] Figure 1 This is a flow chart of the method for preparing a silicon carbide power device provided in Example 2.

[0069] like Figure 1 As shown, the method for preparing a silicon carbide power device provided in this embodiment includes:

[0070] S01: providing a substrate having a silicon carbide epitaxial layer in-situ doped to a first conductivity type during epitaxy;

[0071] S02: forming a first patterned mask on the silicon carbide epitaxial layer, and forming a first sidewall spacer on the sidewall of the opening of the first patterned mask, and using the silicon carbide epitaxial layer under the first sidewall spacer as a channel region;

[0072] S03: Perform a first ion implantation of a second conductivity type using the first patterned mask and the first sidewalls to form a JFET region in the silicon carbide epitaxial layer between the first sidewalls and use other regions of the silicon carbide epitaxial layer as a body region, and then remove the first patterned mask.

[0073] The preparation method of the silicon carbide power device provided in this embodiment is basically the same as the preparation method of Example 1 in principle. The main difference lies in that, compared with Example 1 in which the source region is formed after the channel region and the JFET region are formed, this embodiment forms the channel region and the JFET region after the source region is formed.

[0074] Specifically, step S01 of this embodiment is basically the same as that of the first embodiment, and a silicon carbide epitaxial layer in-situ doped with a first conductivity type during epitaxy is provided on the surface of the substrate, so as to utilize the first conductivity type silicon carbide epitaxial layer to form the body region and the channel region of the power device.

[0075] In this embodiment, between step S01 and step S02, that is, before forming the first patterned mask, a third patterned mask is formed to expose a portion of the surface of the silicon carbide epitaxial layer, and the opening of the third patterned mask exposes the region corresponding to the source region of the power device, and then, a second ion implantation of the second conductivity type is performed to form a source region in the silicon carbide epitaxial layer; then, the third patterned mask is removed. The specific method of performing the second ion implantation of the second conductivity type to form the source region can be referred to in detail in the second ion implantation performed in the first embodiment.

[0076] Step S02 and step S03 of this embodiment may be substantially the same as those in the first embodiment, which may include forming a first patterned mask, forming a first sidewall spacer on the sidewall of the first patterned mask to form a channel region, and performing a first ion implantation to form a JFET region. After forming the JFET region, the steps of continuing to form the body diode region and the terminal structure may refer to the first embodiment, and will not be described in detail here.

[0077] Embodiment 3

[0078] Embodiment 3 provides a method for preparing a silicon carbide power device.

[0079] Figure 1 This is a flow chart of the method for preparing a silicon carbide power device provided in Example 3.

[0080] like Figure 1As shown, the method for preparing a silicon carbide power device provided in this embodiment includes:

[0081] S01: providing a substrate having a silicon carbide epitaxial layer in-situ doped to a first conductivity type during epitaxy;

[0082] S02: forming a first patterned mask on the silicon carbide epitaxial layer, and forming a first sidewall spacer on the sidewall of the opening of the first patterned mask, and using the silicon carbide epitaxial layer under the first sidewall spacer as a channel region;

[0083] S03: Perform a first ion implantation of a second conductivity type using the first patterned mask and the first sidewalls to form a JFET region in the silicon carbide epitaxial layer between the first sidewalls and use other regions of the silicon carbide epitaxial layer as a body region, and then remove the first patterned mask.

[0084] The preparation method of the silicon carbide power device provided in this embodiment is basically the same as the preparation method of Example 1 in principle, and the main difference lies in that, compared with Example 1 or Example 2 in which the terminal structure is formed after the JFET region is formed, this embodiment forms the terminal structure or a part of the terminal structure while forming the JFET region.

[0085] Specifically, step S01 of this embodiment is basically the same as that of the first embodiment, and a silicon carbide epitaxial layer in-situ doped with a first conductivity type during epitaxy is provided on the surface of the substrate, so as to utilize the first conductivity type silicon carbide epitaxial layer to form the body region and the channel region of the power device.

[0086] In step S02 of this embodiment, when forming the first patterned mask, the first patterned mask includes a plurality of first openings to expose the JFET region and the channel region, and also includes a plurality of second openings disposed in the peripheral region of the silicon carbide epitaxial layer to expose the terminal region of the power device, wherein the second opening may be slightly larger than the size of the terminal region, so as to reserve space for the first sidewall formed on the sidewall of the second opening. Next, using the first patterned mask, a first sidewall is formed on the sidewalls of the first opening and the second opening, the first sidewall of the sidewall of the first opening is used to define the channel region, the region between the first sidewalls in the first opening is used to define the JFET region, and the region between the first sidewalls in the second opening is used to define the terminal region.

[0087] In step S03 of this embodiment, a first ion implantation of the second conductivity type is performed using the first patterned mask and the first sidewall to form a JFET region in the silicon carbide epitaxial layer between the first sidewalls of the first opening, a terminal structure (or part of the terminal structure) is formed in the silicon carbide epitaxial layer between the first sidewalls of the second opening, and other regions of the silicon carbide epitaxial layer are used as body regions, and then the first patterned mask is removed. In addition, similar to the first embodiment, a second sidewall is formed between the first sidewalls (including the first opening and the second opening), the second sidewall covers the JFET region and the terminal structure, and a second ion implantation of the second conductivity type is performed using the first sidewall and the second sidewall to form a source region in the silicon carbide epitaxial layer, and then, the first sidewall and the second sidewall are removed to form a second patterned mask, the opening of the second patterned mask exposes the region of the source region away from the JFET region, and a third ion implantation of the first conductivity type is performed using the second patterned mask to form a body diode region in the source region, and the source region between the body diode region and the channel region is used as the source electrode.

[0088] Embodiment 4

[0089] Embodiment 4 provides a silicon carbide power device.

[0090] Figure 2j This is a schematic diagram of the structure of a semiconductor device provided in Embodiment 4.

[0091] The silicon carbide power device provided in this embodiment may be a planar gate structure, which may be prepared, for example, by any of the preparation methods in Embodiments 1 to 3. Figure 2j As shown, the silicon carbide power device provided in this embodiment includes a substrate (such as Figure 2i As shown, the subsequent part is replaced by the back metal layer 35), silicon carbide epitaxial layer 13, body region, JFET region 25 and channel region 24. The silicon carbide epitaxial layer 13 is arranged on the surface of the substrate 10, has a first conductivity type and is formed by in-situ doping during epitaxy. The body region, JFET region 25 and channel region 24 are arranged in the silicon carbide epitaxial layer 13, the JFET region 25 has a second conductivity type, the channel region 24 is arranged in the body region and connected to the JFET region 25, and the body region and the channel region 24 are composed of part of the silicon carbide epitaxial layer 13.

[0092] Please continue to refer to Figure 2j, between the substrate and the first conductive type silicon carbide epitaxial layer 13, several layers of other types of silicon carbide epitaxial layers are also formed by epitaxial growth and in-situ doping, as or for forming other functional film layers of power devices. In this embodiment, for example, it can be used to form an N-type power device, and three layers of silicon carbide epitaxial layers are sequentially arranged on the substrate, namely, the first to third silicon carbide epitaxial layers 11 to 13 are sequentially away from the substrate, the conductivity type of the first silicon carbide epitaxial layer 11 can be N-type for use as a buffer layer, the conductivity type of the second silicon carbide epitaxial layer 12 can be N-type for use as a drift layer, and the conductivity type of the third silicon carbide epitaxial layer 13 can be P-type for forming a body region. If there is no special explanation, the silicon carbide epitaxial layer mentioned below is the third silicon carbide epitaxial layer 13. Of course, this embodiment does not limit the number of layers and specific settings of other silicon carbide epitaxial layers under the most surface silicon carbide epitaxial layer, for example, a super junction structure can also be provided in the second silicon carbide epitaxial layer 12.

[0093] Specifically, the silicon carbide power device of this embodiment is an N-type power device as an example, and the body region (i.e., P-well) of the silicon carbide power device is composed of a part of the above-mentioned silicon carbide epitaxial layer 13 (third silicon carbide epitaxial layer 13), that is, it is directly defined from the silicon carbide epitaxial layer 13 in a graphical manner, rather than being formed by graphical ion implantation. Therefore, the channel region 24 provided in the body region is also directly defined from the silicon carbide epitaxial layer 13, so that the channel region 24 has a lower surface roughness and better size (length, width and thickness) and uniformity in doping concentration. It is not difficult to understand that the channel region 24 with lower surface roughness can improve the reliability of the gate dielectric layer 31 located on the channel region 24 to improve the performance and reliability of the power device, and the channel region 24 with better size and uniformity in doping concentration can reduce the performance difference between different power devices. In a preferred example, the surface roughness of the silicon carbide epitaxial layer 13 formed by epitaxial growth and in-situ doping is less than or equal to 10 nanometers, that is, the surface roughness of the channel region 24 is less than or equal to 10 nanometers, which is much smaller than the surface roughness of the epitaxial layer after ion implantation. In particular, for silicon carbide materials, the diffusion of implanted ions in silicon carbide materials is weak, and multiple high-energy ion implantations are usually used to ensure the doping concentration during ion implantation, which causes greater damage to the surface of the silicon carbide material, so that the surface roughness of the silicon carbide epitaxial layer 13 after ion implantation is usually greater than 30 nanometers.

[0094] Please continue to refer to Figure 2j, a source 29 and a body diode region 28 are also provided in the body region. The body diode region 28 is heavily doped and has the same conductivity type as the body region. The conductivity type of the source 29 is opposite to that of the body region. The source 29 is provided between the body diode region 28 and the channel region 24, and the junction depth (implantation depth) is less than the thickness of the silicon carbide epitaxial layer 13. The JFET region 25 is provided between the body regions, that is, between the two channel regions 24, and its junction depth is greater than or equal to the thickness of the silicon carbide epitaxial layer 13. In addition, a gate structure 30, an interlayer dielectric layer 33 and a front metal layer 34 are provided on the silicon carbide epitaxial layer 13. The gate structure 30 includes a gate dielectric layer 31 and a gate conductive layer 32. The gate dielectric layer 31 covers the surface of the JFET region 25, the channel region 24 and part of the source 29, and the gate conductive layer 32 is provided on the gate dielectric layer 31. The interlayer dielectric layer 33 covers part of the surface of the silicon carbide epitaxial layer 13 and the outer wall of the gate structure 30, and the front metal layer 34 electrically leads out various structures (source 29, body diode region, gate structure 30 and terminal structure). Of course, the substrate 10 on the back side of the silicon carbide epitaxial layer 13 is replaced by the back metal layer 35 as the drain.

[0095] In summary, the method for preparing a silicon carbide power device provided by the present invention includes providing a substrate having a silicon carbide epitaxial layer doped in situ to a first conductivity type during epitaxy; forming a first patterned mask on the silicon carbide epitaxial layer, forming a first sidewall on the sidewall of the opening of the first patterned mask, and using the silicon carbide epitaxial layer under the first sidewall as a channel region; using the first patterned mask and the first sidewall, performing a first ion implantation of a second conductivity type to form a JFET region in the silicon carbide epitaxial layer between the first sidewalls, and using other regions of the silicon carbide epitaxial layer as a body region, and then removing the first patterned mask. Compared with the silicon carbide layer formed by epitaxy followed by ion implantation, the present invention uses a silicon carbide epitaxial layer formed by in-situ doping during epitaxy, so that it has a lower surface roughness, and the first sidewall of the first patterned mask sidewall is used to self-align and define a channel region in the above silicon carbide epitaxial layer, so that the channel region has better size (length, width and thickness) and uniformity in doping concentration. Therefore, the channel region as a part of the silicon carbide epitaxial layer (directly composed of a part of the silicon carbide epitaxial layer) also has the above advantages. The channel region with lower surface roughness can improve the reliability of the gate dielectric layer located on the channel region to improve the performance and reliability of the power device. The channel region with better size and uniformity of doping concentration can reduce the performance difference between different power devices. In addition, the silicon carbide epitaxial layer with lower surface roughness in the present invention is also conducive to the exposure equipment to identify the lithography mark set on the silicon carbide epitaxial layer, so as to improve the alignment accuracy and reduce the risk of alarm caused by abnormal alignment of the exposure equipment.

[0096] The above description is only a description of the preferred embodiments of the present invention, and is not intended to limit the scope of the present invention. Any changes or modifications made by a person skilled in the art in the field of the present invention based on the above disclosure shall fall within the scope of protection of the claims.

Claims

1. A method for preparing a silicon carbide power device, characterized in that: include: Providing a substrate having a silicon carbide epitaxial layer in-situ doped to a first conductivity type during epitaxy; Forming a first patterned mask on the silicon carbide epitaxial layer, and forming a first sidewall spacer on the sidewall of the opening of the first patterned mask, and using the silicon carbide epitaxial layer under the first sidewall spacer as a channel region; Using the first patterned mask and the first sidewall spacer, performing a first ion implantation of a second conductivity type to form a JFET region in the silicon carbide epitaxial layer between the first sidewall spacers, and using other regions of the silicon carbide epitaxial layer as a body region; The first patterned mask is removed to form a second side wall between the first side walls, wherein the second side wall covers the JFET region and exposes the silicon carbide epitaxial layer outside the first side wall; a second ion implantation of the second conductivity type is performed using the first side wall and the second side wall to form a source region in the silicon carbide epitaxial layer, wherein the implantation depth of the source region is less than the thickness of the silicon carbide epitaxial layer.

2. The method for preparing a silicon carbide power device according to claim 1, characterized in that: The silicon carbide power device includes an NMOS device, the first conductivity type is P type, and the second conductivity type is N type.

3. The method for preparing a silicon carbide power device according to claim 1, characterized in that: An ion implantation protection layer is further provided between the silicon carbide epitaxial layer and the first patterned mask, and an opening of the first patterned mask exposes a surface of the corresponding ion implantation protection layer.

4. The method for preparing a silicon carbide power device according to claim 1, characterized in that: removing the first side wall and the second side wall; forming a second patterned mask, wherein an opening of the second patterned mask exposes a region of the source region away from the JFET region; performing a third ion implantation of the first conductivity type using the second patterned mask to form a body diode region in the source region; A termination structure is formed in a peripheral region of the silicon carbide epitaxial layer.

5. The method for preparing a silicon carbide power device according to any one of claims 1 to 4, characterized in that: The method also includes forming a gate structure on surfaces of the JFET region, the channel region, and a portion of the source region.

6. The method for preparing a silicon carbide power device according to claim 1, characterized in that: The opening of the first patterned mask not only exposes the area for forming the JFET area, but also exposes the area for forming the terminal structure, and when performing the first ion implantation of the second conductivity type, the JFET area and the terminal structure are simultaneously formed in the silicon carbide epitaxial layer.

Citation Information

Patent Citations

  • Silicon carbide metal oxide semiconductor field effect transistor

    CN104409501A

  • Manufacturing method of planar SiC MOSFET device

    CN116259542A

  • Preparation method of silicon carbide field effect transistor and silicon carbide field effect transistor

    CN116895531A

  • Silicon carbide MOSFET device and self-alignment manufacturing method thereof

    CN117711946A

  • Method for manufacturing silicon carbide chip with low registration deviation

    CN117855047A