A hard carbon composite material and its preparation method and application

By covering the hard carbon material with metal conductive agents, sodium ion solid electrolytes, sodium supplement agents and amorphous carbon, we build a porous structure hard carbon composite material, which solves the problem of insufficient conductivity of hard carbon materials and significantly improves its speed Charge, magnification and high temperature storage performance.

CN118553897BActive Publication Date: 2024-11-05GUOKE TANMEI NEW MATERIALS (HUZHOU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411018480.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-05
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

The porous structure and messy layer structure of hard carbon materials lead to poor electronic conductivity, reducing fast charging performance and first-time efficiency. The combination of solid electrolytes and hard carbon has the problem of insufficient electronic conductivity of the material.

Method used

Coated metal conducting agent, sodium ion solid electrolyte, sodium supplementing agent and amorphous carbon together on the core surface of the secondary particles of asphalt-based hard carbon material to build a porous structure hard carbon composite material to improve its electron and ion conductivity. Coordinately improve fast charging, magnification and high-temperature storage performance.

Benefits of technology

The fast charging performance, first-time efficiency, rate performance and high-temperature storage performance of hard carbon composite materials have been significantly improved, and the conductivity and compaction density of the material are enhanced through synergistic effects, reducing material expansion and side reactions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118553897B_ABST
    Figure CN118553897B_ABST
Patent Text Reader

Abstract

The present invention provides a hard carbon composite material and its preparation method and application, which belong to the field of battery material technology. The hard carbon composite material includes a secondary particle core and a shell layer coated on the surface of the secondary particle core; the secondary particle core includes an asphalt-based hard carbon material, and the shell layer includes a metal conductive agent, a sodium ion solid electrolyte, a sodium supplement and amorphous carbon. The present invention jointly coats the metal conductive agent, the sodium ion solid electrolyte, the sodium supplement and the amorphous carbon on the surface of the secondary particle core constructed by the asphalt-based hard carbon material, effectively exerting the synergistic effect between the four, not only improving the fast charging performance and the first efficiency of the hard carbon composite material, but also improving the rate performance and high temperature storage performance of the hard carbon composite material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of battery materials, and in particular relates to a hard carbon composite material and a preparation method and application thereof. Background Art

[0002] As the main negative electrode material of sodium-ion batteries, hard carbon is a negative electrode material with great development potential. Its sodium storage mechanism is mainly through material adsorption and intercalation of sodium ions between material layers. However, due to the porous structure and disordered layer structure of hard carbon, the electronic conductivity of hard carbon materials is poor, which reduces their fast charging performance and initial efficiency. The main reason for the poor fast charging performance of hard carbon materials is the low electronic conductivity of the material and the high impedance caused by the sodium intercalation between its pore layers.

[0003] Compared with amorphous carbon, solid electrolytes have the advantages of stable structure and good ionic conductivity, but their electronic conductivity is poor. Therefore, solid electrolytes need to be mixed with materials with high electronic conductivity and coated on the surface of hard carbon to improve the electronic and ionic conductivity of the material, improve the insertion and extraction rate of sodium ions during charging and discharging, reduce side reactions on the surface of the material, and improve the electrochemical performance.

[0004] In summary, how to effectively use solid electrolytes to modify hard carbon materials, thereby significantly improving the fast charging performance and initial efficiency of hard carbon materials, is a technical problem that needs to be solved urgently. Summary of the invention

[0005] In view of the deficiencies of the prior art, the purpose of the present invention is to provide a hard carbon composite material and its preparation method and application. The present invention co-coats a metal conductive agent, a sodium ion solid electrolyte, a sodium supplement and amorphous carbon on the surface of the secondary particle core constructed by an asphalt-based hard carbon material, effectively exerting the synergistic effect between the four, not only improving the fast charging performance and the first efficiency of the hard carbon composite material, but also improving the rate performance and high temperature storage performance of the hard carbon composite material.

[0006] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0007] In a first aspect, the present invention provides a hard carbon composite material, the hard carbon composite material comprising a secondary particle core, and a shell layer coated on the surface of the secondary particle core;

[0008] The secondary particle inner core comprises a pitch-based hard carbon material, and the shell layer comprises a metal conductive agent, a sodium ion solid electrolyte, a sodium supplement and amorphous carbon.

[0009] The present invention jointly coats a metal conductive agent, a sodium ion solid electrolyte, a sodium supplementer and amorphous carbon on the surface of the secondary particle inner core constructed of an asphalt-based hard carbon material. The sodium ion solid electrolyte itself has a high sodium ion diffusion rate and a stable structure. The metal conductive agent has high electronic conductivity and specific capacity. The sodium supplementer can release sufficient sodium ions during the first charge and discharge process to reduce material defects. The amorphous carbon has excellent conductivity. The four work synergistically to improve not only the fast charging performance and the first efficiency of the hard carbon composite material, but also the rate performance and high-temperature storage performance of the hard carbon composite material, and have good development potential.

[0010] Preferably, the particle size D50 of the inner core of the secondary particles is 3-10 μm, for example, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 9 μm, 9 μm or 10 μm.

[0011] Preferably, the hard carbon composite material has a porous structure.

[0012] In the present invention, the porous structure helps to improve the power performance of the material and reduce the expansion of the material.

[0013] Preferably, based on the mass of the hard carbon composite material, the mass content of the shell layer is 5-10%, for example, 5%, 6%, 7%, 8%, 9% or 10%.

[0014] Preferably, the mass ratio of the metal conductive agent, the sodium ion solid electrolyte, the sodium supplement and the amorphous carbon is (5-10):(10-30):(5-10):(50-80), wherein the selection range of the metal conductive agent "5-10" can be, for example, 5, 6, 7, 8, 9 or 10, etc., the selection range of the sodium ion solid electrolyte "10-30" can be, for example, 10, 15, 20, 25 or 30, etc., the selection range of the sodium supplement "5-10" can be, for example, 5, 6, 7, 8, 9 or 10, etc., and the selection range of the amorphous carbon "50-80" can be, for example, 50, 60, 70 or 80, etc.

[0015] In the present invention, if the amount of the metal conductive agent is too small, the power performance of the material is limited and the synergistic effect is weakened; if the amount of the metal conductive agent is too large, the expansion is large, the initial efficiency is low, and the synergistic effect is weakened. If the amount of the sodium supplement is too small, the initial efficiency of the material is limited and the number of sodium ions during the charging and discharging process is limited, resulting in limited improvement in its rate performance and weakened synergistic effect; if the amount of the sodium supplement is too large, the alkalinity is too high, the processing performance is reduced, and the synergistic effect is weakened.

[0016] Preferably, the metal conductive agent includes any one of metal tin powder, metal antimony powder or metal germanium powder, or a combination of at least two of them.

[0017] Preferably, the particle size D50 of the metal conductive agent is 10-50µm, for example, 10µm, 20µm, 30µm, 40µm or 50µm.

[0018] Preferably, the chemical formula of the sodium ion solid electrolyte is Na 1+x Zr2Si x P 3-x O 12 , where 1≤x≤3, for example, it can be 1, 1.5, 2, 2.5 or 3, etc.

[0019] Preferably, the sodium supplement comprises any one of Na6CoO4, Na5FeO4 or Na2NiO2 or a combination of at least two thereof.

[0020] In a second aspect, the present invention provides a method for preparing the hard carbon composite material as described in the first aspect, the preparation method comprising the following steps:

[0021] (a) mixing a metal conductive agent, a sodium ion solid electrolyte, a sodium supplementing agent, a binder and an organic solvent to obtain a coating solution;

[0022] (b) mixing a resin precursor and a cross-linking agent, curing and cross-linking the mixture to obtain an intermediate, and then mixing the intermediate with asphalt and carbonizing the mixture to obtain an asphalt-based hard carbon material in the form of secondary particles;

[0023] (c) mixing the pitch-based hard carbon material and the coating liquid, and performing a sintering treatment to obtain the hard carbon composite material.

[0024] Preferably, the binder in step (a) comprises sodium carboxymethyl cellulose.

[0025] Preferably, the organic solvent in step (a) comprises any one of ethylene carbonate, carboxylic acid ester, fluorocarbonate, methyl ether or ethyl ether, or a combination of at least two thereof.

[0026] Preferably, the resin precursor in step (b) comprises any one of turpentine resin, oily polyurethane resin, maleic acid rosin resin or thermoplastic phenolic resin, or a combination of at least two thereof.

[0027] Preferably, the cross-linking agent in step (b) includes any one of hexanediol diacrylate, triallyl isocyanurate, trimethylolpropane triacrylate or pentaerythritol triacrylate, or a combination of at least two thereof.

[0028] Preferably, the mass ratio of the resin precursor to the cross-linking agent in step (b) is 100:(10-30), for example, it can be 100:10, 100:15, 100:20, 100:25 or 100:30.

[0029] Preferably, the curing and cross-linking temperature in step (b) is 400-600°C, for example, 400°C, 450°C, 500°C, 550°C or 600°C, and the time is 1-6h, for example, 1h, 2h, 3h, 4h, 5h or 6h.

[0030] In the present invention, if the curing and cross-linking temperature is too low, the moisture and volatile matter in the material cannot be discharged, resulting in a high impurity content in the material; if the curing and cross-linking temperature is too high, the pores in the material are too small, which is not conducive to sodium storage in the material and reduces the specific capacity.

[0031] Preferably, the asphalt in step (b) comprises any one of petroleum asphalt, coal asphalt or mesophase asphalt, or a combination of at least two thereof.

[0032] Preferably, the mass ratio of the intermediate to asphalt in step (b) is 100:(5-20), for example, it can be 100:5, 100:10, 100:15 or 100:20.

[0033] In the present invention, if the mass ratio of the intermediate to the asphalt is too small, the granulation size of the material is small and the expansion reduction is limited; if the mass ratio of the intermediate to the asphalt is too large, it will cause processing performance deviation and reduce the specific capacity of the material.

[0034] Preferably, the carbonization treatment in step (b) is carried out by multi-stage carbonization, which includes primary carbonization and secondary carbonization.

[0035] Preferably, the primary carbonization temperature is 200-300°C, for example, 200°C, 220°C, 240°C, 260°C, 280°C or 300°C, and the insulation time is 1-6h, for example, 1h, 2h, 3h, 4h, 5h or 6h.

[0036] In the present invention, primary carbonization is performed at 200-300°C, and the intermediate and asphalt can be pre-melted at low temperature, so that the asphalt is melted and evenly coated on the surface of the resin material, thereby improving the consistency of the material and facilitating the improvement of the compaction density.

[0037] Preferably, the temperature of the secondary carbonization is 1200-1500°C, for example, 1200°C, 1300°C, 1400°C or 1500°C, etc., and the insulation time is 1-6h, for example, 1h, 2h, 3h, 4h, 5h or 6h, etc.

[0038] In the present invention, the asphalt can be carbonized to form soft carbon through secondary carbonization at 1200-1500°C, thereby improving the compaction density and isotropy of the hard carbon composite material and improving the fast charging performance.

[0039] Preferably, in step (c), the mass ratio of the pitch-based hard carbon material to the coating liquid is 100:(50-200), for example, it can be 100:50, 100:100, 100:150 or 100:200.

[0040] Preferably, the atmosphere of the sintering treatment in step (c) is an inert atmosphere.

[0041] Preferably, the gas in the inert atmosphere includes nitrogen.

[0042] Preferably, the sintering treatment in step (c) is performed by multi-stage sintering, and the multi-stage sintering includes primary sintering and secondary sintering.

[0043] Preferably, the primary sintering temperature is 200-300°C, for example, 200°C, 220°C, 240°C, 260°C, 280°C or 300°C, and the holding time is 1-6h, for example, 1h, 2h, 3h, 4h, 5h or 6h.

[0044] In the present invention, the purpose of primary sintering at 200-300° C. is to convert the asphalt from solid to liquid and evenly coat the surface of the intermediate, thereby improving the consistency of the material and the compaction density.

[0045] Preferably, the secondary sintering temperature is 1000-1500°C, for example, it can be 1000°C, 1100°C, 1200°C, 1300°C, 1400°C or 1500°C, and the holding time is 1-6h, for example, it can be 1h, 2h, 3h, 4h, 5h or 6h.

[0046] Preferably, the preparation method comprises the following steps:

[0047] (1) adding a binder to an organic solvent to dissolve it, then adding a sodium ion solid electrolyte, a metal conductive agent and a sodium supplement agent, and performing ultrasonic mixing to obtain a coating solution;

[0048] Wherein, the mass ratio of the metal conductive agent, the sodium ion solid electrolyte, the sodium supplement agent, the binder and the organic solvent is (5-10):(10-30):(5-10):(50-80):1000;

[0049] (2) A resin precursor and a cross-linking agent are mixed in a mass ratio of 100:(10-30), and cured and cross-linked at 400-600°C for 1-6 hours to obtain an intermediate, and then the intermediate and asphalt are added to a ball mill in a mass ratio of 100:(5-20) for ball milling, and then the obtained ball milled material is subjected to primary carbonization at 200-300°C for 1-6 hours. After the end, the temperature is raised to 1200-1500°C for secondary carbonization for 1-6 hours to obtain a pitch-based hard carbon material with a secondary particle morphology;

[0050] (3) adding the pitch-based hard carbon material to the coating liquid and mixing them evenly, then transferring them to a rotary kiln, sequentially performing primary sintering and secondary sintering in an inert atmosphere, and cooling them to room temperature to obtain the hard carbon composite material;

[0051] Among them, the mass ratio of the asphalt-based hard carbon material and the coating liquid is 100:(50-200), the temperature of the primary sintering is 200-300°C, the insulation time is 1-6h, the temperature of the secondary sintering is 1000-1500°C, and the insulation time is 1-6h.

[0052] In a third aspect, the present invention provides a negative electrode plate, wherein the negative electrode plate comprises the hard carbon composite material as described in the first aspect.

[0053] In a fourth aspect, the present invention provides a sodium ion battery, comprising the negative electrode sheet as described in the third aspect.

[0054] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0055] Compared with the prior art, the present invention has the following beneficial effects:

[0056] (1) The present invention uses secondary particles constructed of asphalt-based hard carbon materials as the core, which improves the compaction density and isotropy of the hard carbon composite material, reduces material expansion, and improves the fast charging performance of the hard carbon composite material.

[0057] (2) The present invention uses a metal conductive agent, a sodium ion solid electrolyte, a sodium supplement and amorphous carbon to synergistically construct the outer shell of the secondary particle core. By giving full play to the synergistic effect among the four, the fast charging performance, initial efficiency, rate performance and high-temperature storage performance of the hard carbon composite material are effectively improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0058] Figure 1 This is a SEM image of the hard carbon composite material prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0059] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0060] It should be noted that the room temperature below refers to 25°C.

[0061] Example 1

[0062] This embodiment provides a hard carbon composite material, the hard carbon composite material comprising a secondary particle core and a shell layer coated on the surface of the secondary particle core;

[0063] The secondary particle inner core comprises a pitch-based hard carbon material, and the shell layer comprises a metal conductive agent, a sodium ion solid electrolyte, a sodium supplement and amorphous carbon;

[0064] The particle size D50 of the secondary particle core is 5 μm; the hard carbon composite material is a porous structure;

[0065] Based on the mass of the hard carbon composite material, the mass content of the shell layer is 8%;

[0066] The mass ratio of the metal conductive agent, the sodium ion solid electrolyte, the sodium supplement and the amorphous carbon is 8:20:8:75. The metal conductive agent is a metal nickel powder with a particle size D50 of 30 μm. The sodium ion solid electrolyte is Na2Zr2SiP2O 12 , the sodium supplement is Na6CoO4.

[0067] This embodiment also provides a method for preparing the hard carbon composite material, the preparation method comprising the following steps:

[0068] (1) Add 75g of sodium carboxymethyl cellulose to 1000g of ethylene carbonate to dissolve, then add 20g of Na2Zr2SiP2O 12 , 8g of metal nickel powder and 8g of sodium supplement Na6CoO4, and ultrasonically mix to obtain a coating solution;

[0069] (2) 100 g of turpentine resin and 20 g of hexanediol diacrylate are mixed and cured and cross-linked at 500° C. for 3 h to obtain an intermediate, and then 100 g of the intermediate and 10 g of petroleum asphalt are added to a ball mill for ball milling, and then the obtained ball milled material is subjected to primary carbonization at 250° C. for 3 h, and then the temperature is raised to 1300° C. for secondary carbonization for 3 h to obtain a pitch-based hard carbon material with a secondary particle morphology;

[0070] (3) adding 100 g of the pitch-based hard carbon material to 100 g of the coating liquid and transferring the mixture to a mixer for uniform mixing, then transferring the mixture to a rotary kiln, introducing nitrogen, and sequentially performing primary sintering and secondary sintering in a nitrogen atmosphere, and then cooling the mixture to room temperature to obtain the hard carbon composite material;

[0071] The primary sintering temperature is 250°C and the holding time is 3 hours, and the secondary sintering temperature is 1250°C and the holding time is 3 hours.

[0072] Figure 1 The SEM image of the hard carbon composite material prepared in this embodiment is shown. It can be seen from the image that the hard carbon composite material has a granular structure, a uniform size distribution, a porous structure on the surface, and a particle size between 3-8 μm.

[0073] Example 2

[0074] This embodiment provides a hard carbon composite material, the hard carbon composite material comprising a secondary particle core and a shell layer coated on the surface of the secondary particle core;

[0075] The secondary particle inner core comprises a pitch-based hard carbon material, and the shell layer comprises a metal conductive agent, a sodium ion solid electrolyte, a sodium supplement and amorphous carbon;

[0076] The particle size D50 of the secondary particle core is 3 μm; the hard carbon composite material is a porous structure;

[0077] Based on the mass of the hard carbon composite material, the mass content of the shell layer is 5%;

[0078] The mass ratio of the metal conductive agent, the sodium ion solid electrolyte, the sodium supplement and the amorphous carbon is 5:10:5:50. The metal conductive agent is a metal germanium powder with a particle size D50 of 10 μm. The sodium ion solid electrolyte is Na3Zr2Si2PO 12 , the sodium supplement is Na5FeO4.

[0079] This embodiment also provides a method for preparing the hard carbon composite material, the preparation method comprising the following steps:

[0080] (1) Add 50g of sodium carboxymethyl cellulose to 1000g of carboxylic acid ester to dissolve, then add 10g of Na3Zr2Si2PO 12 , 5g of metallic germanium powder and 5g of sodium supplement Na5FeO4, and ultrasonically mixed to obtain a coating solution;

[0081] (2) 100 g of an oily polyurethane resin and 10 g of triallyl isocyanurate are mixed and cured and cross-linked at 400°C for 6 hours to obtain an intermediate, and then 100 g of the intermediate and 5 g of coal tar pitch are added to a ball mill for ball milling, and then the obtained ball milled material is subjected to primary carbonization at 200°C for 6 hours, and then the temperature is raised to 1200°C for secondary carbonization for 6 hours to obtain a pitch-based hard carbon material with a secondary particle morphology;

[0082] (3) adding 100 g of the pitch-based hard carbon material to 50 g of the coating liquid and transferring the mixture to a mixer for uniform mixing, then transferring the mixture to a rotary kiln, introducing nitrogen, and sequentially performing primary sintering and secondary sintering in a nitrogen atmosphere, and then cooling the mixture to room temperature to obtain the hard carbon composite material;

[0083] Wherein, the temperature of the primary sintering is 200° C., and the holding time is 6 hours; the temperature of the secondary sintering is 1000° C., and the holding time is 6 hours.

[0084] Example 3

[0085] This embodiment provides a hard carbon composite material, the hard carbon composite material comprising a secondary particle core and a shell layer coated on the surface of the secondary particle core;

[0086] The secondary particle inner core comprises a pitch-based hard carbon material, and the shell layer comprises a metal conductive agent, a sodium ion solid electrolyte, a sodium supplement and amorphous carbon;

[0087] The particle size D50 of the secondary particle core is 10 μm; the hard carbon composite material is a porous structure;

[0088] Based on the mass of the hard carbon composite material, the mass content of the shell layer is 10%;

[0089] The mass ratio of the metal conductive agent, the sodium ion solid electrolyte, the sodium supplement and the amorphous carbon is 10:30:10:80. The metal conductive agent is a metal antimony powder with a particle size D50 of 50 μm. The sodium ion solid electrolyte is Na2Zr2SiP2O 12 , the sodium supplement is Na2NiO2.

[0090] This embodiment also provides a method for preparing the hard carbon composite material, the preparation method comprising the following steps:

[0091] (1) Add 80 g of sodium carboxymethyl cellulose to 1000 g of fluorocarbonate to dissolve, then add 30 g of Na2Zr2SiP2O 12 , 10g of metal antimony powder and 10g of sodium supplement Na2NiO2, and ultrasonically mix to obtain a coating solution;

[0092] (2) 100 g of maleic acid rosin resin and 30 g of pentaerythritol triacrylate are mixed and cured and cross-linked at 600°C for 1 hour to obtain an intermediate, and then 100 g of the intermediate and 20 g of mesophase asphalt are added to a ball mill for ball milling, and then the obtained ball milled material is subjected to primary carbonization at 300°C for 1 hour, and then the temperature is raised to 1500°C for secondary carbonization for 1 hour to obtain a pitch-based hard carbon material with a secondary particle morphology;

[0093] (3) adding 100 g of the pitch-based hard carbon material to 200 g of the coating liquid and transferring the mixture to a mixer for uniform mixing, then transferring the mixture to a rotary kiln, introducing nitrogen, and sequentially performing primary sintering and secondary sintering in a nitrogen atmosphere, and then cooling the mixture to room temperature to obtain the hard carbon composite material;

[0094] The primary sintering temperature is 300° C. and the holding time is 1 hour, and the secondary sintering temperature is 1500° C. and the holding time is 1 hour.

[0095] Comparative Example 1

[0096] The difference between this comparative example and Example 1 is that in step (1), no Na2Zr2SiP2O is added. 12 .

[0097] The rest of the preparation methods and parameters were the same as those in Example 1.

[0098] Comparative Example 2

[0099] The difference between this comparative example and Example 1 is that metal nickel powder is not added in step (1).

[0100] The rest of the preparation methods and parameters were the same as those in Example 1.

[0101] Comparative Example 3

[0102] The difference between this comparative example and Example 1 is that the sodium supplement Na6CoO4 is not added in step (1).

[0103] The rest of the preparation methods and parameters were the same as those in Example 1.

[0104] Performance Testing

[0105] 1. The hard carbon composite materials prepared in the above examples and comparative examples were tested for tap density, specific surface area, interlayer spacing and powder resistivity.

[0106] The testing methods include: testing the tap density of the hard carbon composite material by GB / T-43114-2023 "Hard Carbon"; testing the specific surface area of ​​the hard carbon composite material by a specific surface area tester; testing the interlayer spacing of the hard carbon composite material by XRD; and testing the powder resistivity by a four-probe tester.

[0107] 2. Electrochemical performance test of button battery

[0108] The hard carbon composite materials prepared in the above embodiments and comparative examples were assembled into button batteries, and the assembly method was as follows: 6 g of a binder, 3 g of a conductive agent and 220 mL of a solvent were added to 90 g of the hard carbon composite material, the mixture was stirred to make a slurry, and then coated on a copper foil, and dried and rolled to obtain a negative electrode sheet; the binder used was LA132 binder, the conductive agent was SP, and the solvent was double distilled water; the electrolyte was NaPF6 / (EC+DEC) (volume ratio 1:1, concentration 1.1 mol / L), the metal sodium sheet was the counter electrode, and the diaphragm was a polyethylene PE film, and the simulated battery assembly was carried out in an argon-filled glove box.

[0109] The electrochemical performance of the button battery was tested on a Wuhan Blue Power CT2001A battery tester, with a charge and discharge voltage range of 0.00V to 2.0V and a charge and discharge rate of 0.1C; the rate performance (2C / 0.1C) and cycle performance (0.2C / 0.2C, 100 times) were also tested.

[0110] The above test results are shown in Table 1.

[0111] Table 1

[0112]

[0113] It can be seen from Table 1 that compared with comparative examples 1-3, the first discharge capacity, first efficiency, rate performance and cycle performance of the hard carbon composite materials prepared in Examples 1-3 are significantly improved. The reason is that the hard carbon composite materials provided by the present invention utilize the metal conductive agent coated on the surface of the secondary particles, the sodium ion solid electrolyte, the sodium supplement agent and the amorphous carbon to cooperate with each other, which not only reduces the loss of sodium ions in the material during the charging and discharging process, but also utilizes the metal conductive agent to form a metal alloy during the first charging and discharging process, thereby improving the specific capacity of the material; at the same time, the sodium supplement agent releases sodium ions during the first charging and discharging process, thereby effectively improving the first efficiency of the material.

[0114] 3. Electrochemical performance test of soft pack battery

[0115] The hard carbon composite materials prepared in the above examples and comparative examples are used as negative electrodes, and the negative electrode sheets are prepared by slurry mixing and coating. 1 / 3 Mn 1 / 3 Ni 1 / 3A 2Ah soft-pack battery was prepared using O2) as the positive electrode, NaPF6 (the solvent is EC+DEC, the volume ratio is 1:1, the electrolyte concentration is 1.3 mol / L) as the electrolyte, and Celgard2400 membrane as the separator.

[0116] The 2Ah soft-pack battery was tested for high temperature storage performance, cycle performance and rate performance.

[0117] High temperature storage performance test: At 60°C, the capacity of a 2Ah soft-pack battery in a fully charged state is tested to be X1, and then placed at 60°C for 30 days. The battery capacity is then tested again to be X2, and the charge retention rate is calculated to be X2 / X1*100%. The battery is then fully charged to a fully charged state (100% SOC), the battery capacity is tested to be X3, and the capacity recovery rate is calculated to be X3 / X1*100%.

[0118] Cycle performance test: temperature 25℃, 1.5-3.95V, 1C / 1C, 500 weeks.

[0119] Rate performance test: Charge the battery at a rate of 2C+0.1C with constant current + constant voltage up to 3.95C, and then calculate the constant current ratio of the battery = 2C constant current capacity / (2C constant current capacity + 0.1C constant voltage capacity).

[0120] The above test results are shown in Table 2.

[0121] Table 2

[0122]

[0123] It can be seen from Table 2 that the high-temperature storage performance, rate performance and cycle performance of the hard carbon composite materials provided in Examples 1-3 are better than those of the comparative examples. The reason is that the hard carbon composite materials prepared by the present invention have high powder conductivity, which can improve the constant current ratio of the material; at the same time, the shell coated on the surface of the material can effectively reduce the irreversible capacity of the material, increase the transmission rate of sodium ions, and improve the high-temperature storage performance and its constant current ratio.

[0124] The applicant declares that the present invention illustrates the process method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A hard carbon composite material, characterized in that: The hard carbon composite material comprises a secondary particle core and a shell layer coated on the surface of the secondary particle core; The secondary particle inner core comprises a pitch-based hard carbon material, and the shell layer comprises a metal conductive agent, a sodium ion solid electrolyte, a sodium supplement and amorphous carbon; The mass ratio of the metal conductive agent, the sodium ion solid electrolyte, the sodium supplement and the amorphous carbon is (5-10):(10-30):(5-10):(50-80); The metal conductive agent includes any one of metal tin powder, metal antimony powder or metal germanium powder, or a combination of at least two of them; The method for preparing the hard carbon composite material comprises the following steps: (a) mixing a metal conductive agent, a sodium ion solid electrolyte, a sodium supplementing agent, a binder and an organic solvent to obtain a coating solution; (b) mixing a resin precursor and a cross-linking agent, curing and cross-linking the mixture to obtain an intermediate, and then mixing the intermediate with asphalt and carbonizing the mixture to obtain an asphalt-based hard carbon material in the form of secondary particles; (c) mixing the pitch-based hard carbon material and the coating liquid, and performing a sintering treatment to obtain the hard carbon composite material.

2. The hard carbon composite material according to claim 1, characterized in that The particle size D50 of the secondary particle core is 3-10 μm; The hard carbon composite material has a porous structure.

3. The hard carbon composite material according to claim 1, characterized in that Based on the mass of the hard carbon composite material, the mass content of the shell layer is 5-10%; The particle size D50 of the metal conductive agent is 10-50 μm; The chemical formula of the sodium ion solid electrolyte is Na 1+x Zr2Si x P 3-x O 12 , Among them, 1≤x≤3; The sodium supplement includes any one of Na6CoO4, Na5FeO4 or Na2NiO2 or a combination of at least two thereof.

4. A method for preparing a hard carbon composite material according to any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: (a) mixing a metal conductive agent, a sodium ion solid electrolyte, a sodium supplementing agent, a binder and an organic solvent to obtain a coating solution; (b) mixing a resin precursor and a cross-linking agent, curing and cross-linking the mixture to obtain an intermediate, and then mixing the intermediate with asphalt and carbonizing the mixture to obtain an asphalt-based hard carbon material in the form of secondary particles; (c) mixing the pitch-based hard carbon material and the coating liquid, and performing a sintering treatment to obtain the hard carbon composite material.

5. The preparation method according to claim 4, characterized in that: The binder in step (a) comprises sodium carboxymethyl cellulose; The organic solvent in step (a) comprises any one of ethylene carbonate, carboxylic acid ester, fluorocarbonate, methyl ether or ethyl ether, or a combination of at least two thereof; The resin precursor in step (b) comprises any one of turpentine resin, oily polyurethane resin, maleic acid rosin resin or thermoplastic phenolic resin, or a combination of at least two thereof; The crosslinking agent in step (b) includes any one of hexanediol diacrylate, triallyl isocyanurate, trimethylolpropane triacrylate or pentaerythritol triacrylate, or a combination of at least two thereof; The mass ratio of the resin precursor to the crosslinking agent in step (b) is 100:(10-30); The curing and cross-linking in step (b) is carried out at a temperature of 400-600° C. and for a time of 1-6 hours.

6. The preparation method according to claim 4, characterized in that: The asphalt in step (b) includes any one of petroleum asphalt, coal asphalt or mesophase asphalt, or a combination of at least two thereof; The mass ratio of the intermediate to asphalt in step (b) is 100:(5-20); The carbonization treatment in step (b) is carried out in a multi-stage carbonization manner, wherein the multi-stage carbonization comprises a primary carbonization and a secondary carbonization; The temperature of the primary carbonization is 200-300°C, and the insulation time is 1-6h; The temperature of the secondary carbonization is 1200-1500° C., and the insulation time is 1-6 hours.

7. The preparation method according to claim 4, characterized in that: In step (c), the mass ratio of the pitch-based hard carbon material to the coating liquid is 100:(50-200); The atmosphere of the sintering treatment in step (c) is an inert atmosphere; The sintering process in step (c) is a multi-stage sintering process, wherein the multi-stage sintering process includes a primary sintering process and a secondary sintering process; The primary sintering temperature is 200-300°C, and the holding time is 1-6h; The temperature of the secondary sintering is 1000-1500° C., and the holding time is 1-6 hours.

8. The preparation method according to claim 4, characterized in that: The preparation method comprises the following steps: (1) adding a binder to an organic solvent to dissolve it, then adding a sodium ion solid electrolyte, a metal conductive agent and a sodium supplement agent, and performing ultrasonic mixing to obtain a coating solution; Wherein, the mass ratio of the metal conductive agent, the sodium ion solid electrolyte, the sodium supplement agent, the binder and the organic solvent is (5-10):(10-30):(5-10):(50-80):1000; (2) A resin precursor and a cross-linking agent are mixed in a mass ratio of 100:(10-30), and cured and cross-linked at 400-600°C for 1-6 hours to obtain an intermediate, and then the intermediate and asphalt are added to a ball mill in a mass ratio of 100:(5-20) for ball milling, and then the obtained ball milled material is subjected to primary carbonization at 200-300°C for 1-6 hours. After the end, the temperature is raised to 1200-1500°C for secondary carbonization for 1-6 hours to obtain a pitch-based hard carbon material with a secondary particle morphology; (3) adding the pitch-based hard carbon material to the coating liquid and mixing them evenly, then transferring them to a rotary kiln, sequentially performing primary sintering and secondary sintering in an inert atmosphere, and cooling them to room temperature to obtain the hard carbon composite material; Among them, the mass ratio of the asphalt-based hard carbon material and the coating liquid is 100:(50-200), the temperature of the primary sintering is 200-300°C, the insulation time is 1-6h, the temperature of the secondary sintering is 1000-1500°C, and the insulation time is 1-6h.

9. A negative electrode plate, characterized in that: The negative electrode plate comprises the hard carbon composite material as described in any one of claims 1 to 3.

10. A sodium ion battery, characterized in that: The sodium ion battery comprises the negative electrode sheet as claimed in claim 9.