Lotus root hard carbon, lotus root hard carbon / silicon composite material and preparation method and application thereof
By preparing lotus root hard carbon/silicon composite materials, the problems of volume expansion and cycle performance of lithium-ion battery anode materials were solved, achieving excellent characteristics of high capacity, high rate and low expansion, thus improving the overall performance of the battery.
Patent Information
- Application Number
- CN202410962812.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-18
AI Technical Summary
Among existing lithium-ion battery anode materials, silicon materials suffer from significant volume expansion and particle pulverization during charging and discharging, leading to reduced cycle performance. Furthermore, traditional preparation methods struggle to achieve uniform dispersion and efficient lithium-ion intercalation/deintercalation, impacting battery kinetic performance and cost.
Using lotus root as raw material, soluble substances are removed and polyphenols are oxidized through acid soaking and high-temperature carbonization. Combined with structural stabilizers, a porous hard carbon material is formed, which is then composited with nano-silicon to form a lotus root hard carbon/silicon composite material, providing buffer space and conductive network.
It improves the battery's energy density, cycle stability, and rate performance, reduces costs, and optimizes electrochemical performance through the synergistic effect of lotus root hard carbon and nano-silicon.
Smart Images

Figure BDA0004950790590000091
Abstract
Description
Technical Field
[0001] The invention relates to the field of negative electrode materials for lithium ion batteries, and in particular to a lotus root hard carbon, a lotus root hard carbon / silicon composite material, and a preparation method and application thereof. Background Art
[0002] In recent years, as portable electronic products have higher and higher requirements for battery volume, battery capacity and energy density need to be further improved. Graphite materials with a theoretical specific capacity of only 372mAh / g can no longer meet market demand, while silicon materials with a theoretical specific capacity of up to 4200mAh / g have become the mainstream development trend of small electronic products.
[0003] However, unlike the intercalation reaction with graphite, the silicon material that removes / inserts lithium in the form of alloying has a huge volume expansion (~300%) during the charge and discharge process. The particles are very easy to pulverize and lose electrical contact with the current collector, resulting in continuous deactivation of the particles during the cycle and a sharp decrease in cycle performance. In order to slow down the expansion of the negative electrode, people often use graphite, silicon, and organic carbon to form secondary particles to suppress this problem.
[0004] For example, patent CN112310363A prepares graphite / silicon composite materials by dispersing, granulating, molding, cold / static pressing, heat treating, crushing, and carbon coating graphite, silicon, and organic carbon precursors in sequence.
[0005] However, this preparation method has many disadvantages. Since the particle sizes of nano-silicon and graphite differ by two orders of magnitude, it is difficult to disperse the two evenly, resulting in different expansion amplitudes in different regions, which has a very limited effect on suppressing electrode expansion. The graphite material undergoes lithium ion deintercalation / embedding through intercalation reaction, and the ion deintercalation is slow, which inhibits the dynamic performance of the composite material. In addition, the preparation method is complex and has high processing costs. Summary of the invention
[0006] The present invention aims to overcome the defects of lithium-ion battery negative electrode materials in the prior art, such as low theoretical specific capacity and huge volume expansion during charging and discharging, and provides a lotus root hard carbon, a lotus root hard carbon / silicon composite material and a preparation method and application thereof to overcome the above-mentioned shortcomings.
[0007] To achieve the above-mentioned purpose, the present invention is implemented by the following technical solutions: In a first aspect, the present invention first provides a method for preparing lotus root hard carbon, comprising the following steps: (S.1) cutting the lotus root and pre-treating it to oxidize the polyphenols in the lotus root; (S.2) placing the pre-treated lotus root in a solution containing an acid and a structure stabilizer, so that soluble substances in the lotus root are dissolved; (S.3) drying and high-temperature carbonizing the lotus root treated in step (S.2) to obtain crude lotus root hard carbon; (S.4) removing impurities from the crude lotus root hard carbon to obtain the lotus root hard carbon.
[0008] The hard carbon in this application uses lotus root as raw material. Compared with other biomass, lotus root has more microscopic pores and fiber structure. This structure may help to form a specific pore structure and morphology during the carbonization process, thereby giving the hard carbon good physical properties, such as porosity, specific surface area, etc.
[0009] However, fresh lotus roots contain more soluble substances (such as sugars and organic acids, etc.). The presence of these soluble substances may produce impurities in the subsequent carbonization process, thereby affecting the purity and quality of the hard carbon. At the same time, these soluble substances will also interfere with the carbonization reaction during the carbonization process. During the carbonization process, they will damage the structure of the hard carbon due to decomposition or phase change, thereby reducing the structural stability and service life of the hard carbon, and ultimately affecting the uniformity and efficiency of carbonization. Therefore, the present application performs a pretreatment step before carbonizing the lotus root to remove the soluble substances in the lotus root, which helps to obtain a purer hard carbon product, form a more ideal hard carbon structure and performance, and make the carbonization process more controllable and stable.
[0010] However, in the process of removing soluble substances from lotus roots, the applicant found that both acid dissolution and alkaline solution can achieve the removal of soluble substances. However, in the process of choosing to use alkaline solution, hemicellulose and other substances in the lotus roots are also easily dissolved and removed, resulting in the final lotus root having poor structural stability, which is easy to be damaged during transfer and touch, and even melted to form a muddy product, thereby failing to maintain its own porous properties.
[0011] Therefore, in the present application, the inventor adopts the acid soaking method to selectively dissolve the soluble substances therein, while the insoluble substances such as cellulose and hemicellulose therein remain in place, which is conducive to the maintenance of its porous structure. In order to further maintain these porous structures, the inventor of the present application also added a certain amount of structural stabilizers to the solution. These structural stabilizers are mainly water-soluble polymers, which can provide certain support for the lotus root skeleton after the organic substances are dissolved, thereby greatly improving the structural stability of the lotus root and preventing the collapse of the porous structure.
[0012] In addition, the applicant also found that fresh lotus roots also contain a large amount of polyphenols, which have high reducibility and can react with oxygen to form black quinones. The applicant found that when the polyphenols in the lotus roots are converted into quinones, they have an important influence on the subsequent carbonization step. Among them, during the carbonization process of lotus roots, high temperature will decompose and transform the organic matter in the lotus roots to form a hard carbon structure. Quinones have certain chemical activity and may participate in a series of reactions at high temperatures, affecting the formation and performance of hard carbon. Specifically, first of all, the presence of quinones can enable them to undergo cross-linking and polymerization reactions with other organic matter, thereby helping to increase the structural stability and mechanical strength of hard carbon materials. Secondly, the presence of quinones may affect the pore structure of hard carbon materials. They may participate in the process of forming pores, or react on the pore walls, thereby affecting the size, distribution and connectivity of the pores. Finally, the functional groups in quinones may provide active sites on the surface of hard carbon materials, which is very beneficial for some applications such as energy storage and adsorption. Therefore, the present application achieves the purpose of regulating the structure and properties of hard carbon materials to a certain extent by oxidizing polyphenols into quinones before carbonization.
[0013] In summary, the present invention makes targeted selections and improvements on the types of raw materials for hard carbon materials, the methods for processing raw materials, and the transformation of specific substances in the raw materials, thereby being able to effectively remove components that may interfere with the carbonization process and affect the quality of the final product, so that the prepared hard carbon material may have higher purity and better structural stability.
[0014] Preferably, the pretreatment in step (S.1) comprises the step of soaking the lotus root in an alkaline solution with a pH value of 8.5-10; The pre-treatment time in the step (S.1) is greater than or equal to 6 hours.
[0015] In step (S.1), the lotus root is immersed in an alkaline solution with a pH of 8.5-10. The reason is that the alkaline solution within this pH range can not only react with the soluble substances in the lotus root to a certain extent, dissolve and remove them, thereby reducing impurities in the subsequent carbonization process. At the same time, it can also maintain the porous microstructure of the lotus root, create favorable conditions for the subsequent carbonization process, and help form a more ideal hard carbon structure. In addition, the environment of the alkaline solution helps to promote the oxidation reaction of polyphenols in the lotus root, thereby helping to achieve the desired oxidation effect.
[0016] Preferably, the pH value of the acid solution in step (S.2) is 2-3.
[0017] Preferably, the structural stabilizer is a combination of one or more of polyvinyl alcohol, polyethylene glycol, acrylamide, carboxymethyl cellulose, sodium polyacrylate and sodium alginate.
[0018] Preferably, the concentration of the structural stabilizer is 0.5-10 g / 100 ml.
[0019] Preferably, the high temperature carbonization temperature in the step (S.2) is in the range of 500°C to 900°C.
[0020] In the present application, the high-temperature carbonization temperature range is 500°C-900°C. The reason is that within this temperature range, the organic matter in the lotus root can be fully decomposed and transformed to form a carbon structure with a certain degree of crystallinity and stability. In addition. The appropriate temperature helps to regulate the pore size and distribution of the hard carbon. Lower temperatures may result in underdeveloped pores, while too high temperatures may cause excessive shrinkage or merging of pores. The range of 500°C-900°C is conducive to the formation of a suitable pore structure to meet the requirements of pore properties for different applications. At the same time, this temperature range can not only fully carbonize the material, but also avoid excessive embrittlement or structural collapse of the material caused by excessive temperature, thereby maintaining a certain mechanical strength, which helps to form hard carbon with good conductivity, so that it exhibits better charge and discharge performance in applications such as batteries.
[0021] In a second aspect, the present invention further provides a lotus root hard carbon, which is prepared by the method described above.
[0022] In a third aspect, the present invention further provides a lotus root hard carbon / silicon composite material, which is obtained by compounding the lotus root hard carbon and nano-silicon as described above.
[0023] Silicon has an extremely high theoretical specific capacity, which can significantly improve the lithium storage capacity of the composite material, thereby improving the energy density of the battery. However, during the charge and discharge process, silicon will undergo large volume expansion and contraction. The lotus root hard carbon / silicon composite material provided by the present invention utilizes the porous structure of the lotus root carbonized material to provide a buffer space for silicon, reduce the stress caused by volume change, and thus improve the cyclic stability of the material. At the same time, the three-dimensional structure of the hard carbon in the composite material can provide support and restriction for the silicon particles, prevent the silicon particles from agglomerating, thereby maintaining the integrity of the electrode structure.
[0024] In addition, the porous carbon material itself has high conductivity and can be used as an electronic and ion conductor network of the electrode. After being combined with silicon, it can improve the poor conductivity of silicon, improve the electron transmission efficiency, and thus improve the rate performance of the battery. In addition, the gram capacity of the lotus root hard carbon material itself (790mAh / g@700℃ high temperature carbonization) is higher than that of graphite, which improves the capacity of the battery. The hard carbon / silicon composite material finally obtained by the present invention has the excellent characteristics of high capacity, high rate, low expansion, and high cycle.
[0025] Compared with the use of silicon materials alone, the present application can reduce costs to a certain extent and achieve better performance by using a certain proportion of lotus root hard carbon in combination. In addition, lotus root hard carbon and nano silicon are complementary in performance, and the combination of the two can play a synergistic role, so that the composite material shows better comprehensive performance in terms of electrochemical performance than a single material.
[0026] Preferably, the mass ratio of the lotus root hard carbon to nano-silicon is 4:1-1:1.
[0027] In a fourth aspect, the present invention also provides a method for preparing the lotus root hard carbon / silicon composite material as described above, comprising mixing lotus root hard carbon and nano-silicon, adding ethanol and zirconium balls, ball milling to make the composite material evenly mixed, and drying to obtain the lotus root hard carbon / silicon composite material.
[0028] Preferably, the mass ratio of the zirconium balls to the lotus root hard carbon and nano-silicon mixed material is 1:5-15.
[0029] In a fifth aspect, the present invention also provides the use of the lotus root hard carbon or lotus root hard carbon / silicon composite material as described above in a lithium ion battery.
[0030] In summary, this application has the following beneficial effects: In order to solve the problems of large expansion rate of silicon negative electrode, poor rate performance, and easy battery diving after short-term cycling, the present invention provides a new negative electrode material preparation method, which has better improvement effect than traditional graphite / silicon composite. The hard carbon / silicon composite material obtained by the present invention has excellent characteristics of high capacity, high rate, low expansion and high cycle. DETAILED DESCRIPTION
[0031] The present invention is further described below in conjunction with specific embodiments. Those of ordinary skill in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all embodiments. Therefore, based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work should fall within the scope of protection of the present invention.
[0032] Example 1 Preparation of lotus root hard carbon material: The lotus root slices were placed in a sodium carbonate solution with a pH of 9 and soaked for 24 hours, wherein the mass ratio of lotus root to sodium carbonate solution was 2:1. After soaking, the lotus root slices changed from white to black. Then the lotus root strips were taken out and soaked in a hydrochloric acid solution with a pH of 2.5, wherein the mass ratio of lotus root to hydrochloric acid solution was 2:1, wherein the hydrochloric acid also contained 5g / 100ml of polyvinyl alcohol. After soaking for 24 hours, the lotus root strips were taken out and dried at 110°C for 12 hours. Then, in a quartz tube, high temperature carbonization was performed at 700°C for 2 hours under a N2 atmosphere. After carbonization, the strips were washed with a 1mol / L HCl solution to remove residual potassium salts and impurities, then washed with deionized water and ethanol until neutral, and finally dried at 80°C.
[0033] Preparation of composite materials: Mix lotus root hard carbon material and nano-silicon in a mass ratio of 1:1, add ethanol and zirconium balls, and the mass ratio of zirconium balls to lotus root hard carbon and nano-silicon mixed material is 1:10. Ball mill for 4 hours to mix the composite material evenly; dry at 80°C to obtain a lotus root hard carbon / silicon composite material.
[0034] Example 2 Preparation of lotus root hard carbon material: The lotus root slices were placed in a sodium carbonate solution with a pH of 9 and soaked for 24 hours, wherein the mass ratio of lotus root to sodium carbonate solution was 2:1. After soaking, the lotus root slices changed from white to black. Then the lotus root strips were taken out and soaked in a hydrochloric acid solution with a pH of 2.5, wherein the mass ratio of lotus root to hydrochloric acid solution was 2:1, wherein the hydrochloric acid also contained 5g / 100ml of polyvinyl alcohol. After soaking for 24 hours, the lotus root strips were taken out and dried at 110°C for 12 hours. Then, in a quartz tube, high temperature carbonization was performed at 500°C for 4 hours under a N2 atmosphere. After carbonization, the strips were washed with a 1mol / L HCl solution to remove residual potassium salts and impurities, then washed with deionized water and ethanol until neutral, and finally dried at 80°C.
[0035] Preparation of composite materials: Add ethanol and zirconium balls in a mass ratio of 1:1 to lotus root hard carbon material and nano-silicon; the mass ratio of zirconium balls to lotus root hard carbon and nano-silicon mixed material is 1:5; ball mill for 4 hours to make the composite material evenly mixed; dry at 80°C to obtain a lotus root hard carbon / silicon composite material.
[0036] Example 3 Preparation of lotus root hard carbon material: The lotus root slices were placed in a sodium carbonate solution with a pH of 9 and soaked for 24 hours, wherein the mass ratio of lotus root to sodium carbonate solution was 2:1. After soaking, the lotus root slices changed from white to black. Then the lotus root strips were taken out and soaked in a hydrochloric acid solution with a pH of 2.5, wherein the mass ratio of lotus root to hydrochloric acid solution was 2:1, wherein the hydrochloric acid also contained 5g / 100ml of polyvinyl alcohol. After soaking for 24 hours, the lotus root strips were taken out and dried at 110°C for 12 hours. Then, in a quartz tube, high-temperature carbonization was performed at 600°C for 3 hours under a N2 atmosphere. After carbonization, the strips were washed with a 1mol / L HCl solution to remove residual potassium salts and impurities, then washed with deionized water and ethanol until neutral, and finally dried at 80°C.
[0037] Preparation of composite materials: Mix lotus root hard carbon material and nano-silicon in a mass ratio of 1:1, add ethanol and zirconium balls, and the mass ratio of zirconium balls to lotus root hard carbon and nano-silicon mixed material is 1:10. Ball mill for 4 hours to mix the composite material evenly; dry at 80°C to obtain a lotus root hard carbon / silicon composite material.
[0038] Example 4 Preparation of lotus root hard carbon material: The lotus root slices were placed in a sodium carbonate solution with a pH of 9 and soaked for 24 hours, wherein the mass ratio of lotus root to sodium carbonate solution was 2:1. After soaking, the lotus root slices changed from white to black. Then the lotus root strips were taken out and soaked in a hydrochloric acid solution with a pH of 2.5, wherein the mass ratio of lotus root to hydrochloric acid solution was 2:1, wherein the hydrochloric acid also contained 5g / 100ml of polyvinyl alcohol. After soaking for 24 hours, the lotus root strips were taken out and dried at 110°C for 12 hours. Then, in a quartz tube, high-temperature carbonization was performed at 800°C for 2 hours under a N2 atmosphere. After carbonization, the strips were washed with a 1mol / L HCl solution to remove residual potassium salts and impurities, then washed with deionized water and ethanol until neutral, and finally dried at 80°C.
[0039] Preparation of composite materials: Mix lotus root hard carbon material and nano-silicon in a mass ratio of 1:1, add ethanol and zirconium balls, and the mass ratio of zirconium balls to lotus root hard carbon and nano-silicon mixed material is 1:10. Ball mill for 4 hours to mix the composite material evenly; dry at 80°C to obtain a lotus root hard carbon / silicon composite material.
[0040] Example 5 Preparation of lotus root hard carbon material: The lotus root slices were placed in a sodium carbonate solution with a pH of 9 and soaked for 24 hours, wherein the mass ratio of lotus root to sodium carbonate solution was 2:1. After soaking, the lotus root slices changed from white to black. Then the lotus root strips were taken out and soaked in a hydrochloric acid solution with a pH of 2.5, wherein the mass ratio of lotus root to hydrochloric acid solution was 2:1, wherein the hydrochloric acid also contained 5g / 100ml of polyvinyl alcohol. After soaking for 24 hours, the lotus root strips were taken out and dried at 110°C for 12 hours. Then, in a quartz tube, high-temperature carbonization was performed at 900°C for 2 hours under a N2 atmosphere. After carbonization, the strips were washed with a 1mol / L HCl solution to remove residual potassium salts and impurities, then washed with deionized water and ethanol until neutral, and finally dried at 80°C.
[0041] Preparation of composite materials: Mix lotus root hard carbon material and nano-silicon in a mass ratio of 1:1, add ethanol and zirconium balls, and the mass ratio of zirconium balls to lotus root hard carbon and nano-silicon mixed material is 1:10. Ball mill for 4 hours to mix the composite material evenly; dry at 80°C to obtain a lotus root hard carbon / silicon composite material.
[0042] Example 6 Preparation of lotus root hard carbon material: The lotus root slices were placed in a KOH solution with a pH of 8.5 and soaked for 24 hours, wherein the mass ratio of lotus root to KOH solution was 2:1. After soaking, the lotus root slices changed from white to black. Then the lotus root strips were taken out and soaked in a hydrochloric acid solution with a pH of 2, wherein the mass ratio of lotus root to hydrochloric acid solution was 2:1, wherein the hydrochloric acid also contained 0.5g / 100ml of carboxymethyl cellulose. After soaking for 24 hours, the lotus root strips were taken out and dried at 110°C for 12 hours. Then, in a quartz tube, high-temperature carbonization was performed at 700°C for 2 hours under a N2 atmosphere. After carbonization, the strips were washed with a 1mol / L HCl solution to remove residual potassium salts and impurities, then washed with deionized water and ethanol until neutral, and finally dried at 80°C.
[0043] Preparation of composite materials: Add ethanol and zirconium balls to lotus root hard carbon material and nano-silicon in a mass ratio of 4:1; the mass ratio of zirconium balls to lotus root hard carbon and nano-silicon mixed material is 1:10; ball mill for 4 hours to make the composite material evenly mixed; dry at 80°C to obtain a lotus root hard carbon / silicon composite material.
[0044] Example 7 Preparation of lotus root hard carbon material: The lotus root slices were placed in a 3mol / L KOH solution and soaked for 24 hours, wherein the mass ratio of lotus root to KOH solution was 2:1. After soaking, the lotus root slices changed from white to black. Then the lotus root strips were taken out and soaked in a hydrochloric acid solution with a pH value of 3, wherein the mass ratio of lotus root to hydrochloric acid solution was 2:1, wherein the hydrochloric acid also contained 10g / 100ml of polyethylene glycol. After soaking for 24 hours, the lotus root strips were taken out and dried at 110°C for 12 hours. Then, in a quartz tube, high temperature carbonization was performed at 700°C for 2 hours under a N2 atmosphere. After carbonization, the strips were washed with a 1mol / L HCl solution to remove residual potassium salts and impurities, then washed with deionized water and ethanol until neutral, and finally dried at 80°C.
[0045] Preparation of composite materials: Add ethanol and zirconium balls to lotus root hard carbon material and nano-silicon in a mass ratio of 1.5:1; the mass ratio of zirconium balls to lotus root hard carbon and nano-silicon mixed material is 1:10; ball mill for 4 hours to make the composite material evenly mixed; dry at 80°C to obtain a lotus root hard carbon / silicon composite material.
[0046] Comparative Example 1 Preparation of lotus root hard carbon material: The lotus root slices were placed in a sodium carbonate solution with a pH of 9 and soaked for 24 hours, wherein the mass ratio of lotus root to sodium carbonate solution was 2:1. After soaking, the lotus root slices changed from white to black. Then the lotus root strips were taken out and soaked in a hydrochloric acid solution with a pH of 2.5, wherein the mass ratio of lotus root to hydrochloric acid solution was 2:1, wherein the hydrochloric acid also contained 5g / 100ml of polyvinyl alcohol. After soaking for 24 hours, the lotus root strips were taken out and dried at 110°C for 12 hours. Then, in a quartz tube, high-temperature carbonization was performed at 400°C for 4 hours under a N2 atmosphere. After carbonization, the strips were washed with a 1mol / L HCl solution to remove residual potassium salts and impurities, then washed with deionized water and ethanol until neutral, and finally dried at 80°C.
[0047] Preparation of composite materials: Mix lotus root hard carbon material and nano-silicon in a mass ratio of 1:1, add ethanol and zirconium balls, and the mass ratio of zirconium balls to lotus root hard carbon and nano-silicon mixed material is 1:10. Ball mill for 4 hours to mix the composite material evenly; dry at 80°C to obtain a lotus root hard carbon / silicon composite material.
[0048] Comparative Example 2 Preparation of lotus root hard carbon material: The lotus root slices were placed in a sodium carbonate solution with a pH of 9 and soaked for 24 hours, wherein the mass ratio of lotus root to sodium carbonate solution was 2:1. After soaking, the lotus root slices changed from white to black. Then the lotus root strips were taken out and soaked in a hydrochloric acid solution with a pH of 2.5, wherein the mass ratio of lotus root to hydrochloric acid solution was 2:1, wherein the hydrochloric acid also contained 5g / 100ml of polyvinyl alcohol. After soaking for 24 hours, the lotus root strips were taken out and dried at 110°C for 12 hours. Then, in a quartz tube, high-temperature carbonization was performed at 1000°C for 2 hours under a N2 atmosphere. After carbonization, the strips were washed with a 1mol / L HCl solution to remove residual potassium salts and impurities, then washed with deionized water and ethanol until neutral, and finally dried at 80°C.
[0049] Preparation of composite materials: Mix lotus root hard carbon material and nano-silicon in a mass ratio of 1:1, add ethanol and zirconium balls, and the mass ratio of zirconium balls to lotus root hard carbon and nano-silicon mixed material is 1:10. Ball mill for 4 hours to mix the composite material evenly; dry at 80°C to obtain a lotus root hard carbon / silicon composite material.
[0050] Comparative Example 3 Preparation of lotus root hard carbon material: The lotus root slices were placed in a sodium carbonate solution with a pH of 9 and soaked for 24 hours, wherein the mass ratio of lotus root to sodium carbonate solution was 2:1. After soaking, the lotus root slices changed from white to black. Then the lotus root strips were taken out and soaked in a hydrochloric acid solution with a pH of 2.5, wherein the mass ratio of lotus root to hydrochloric acid solution was 2:1, wherein the hydrochloric acid also contained 5g / 100ml of polyvinyl alcohol. After soaking for 24 hours, the lotus root strips were taken out and dried at 110°C for 12 hours. Then, in a quartz tube, high temperature carbonization was performed at 700°C for 4 hours under a N2 atmosphere. After carbonization, the strips were washed with a 1mol / L HCl solution to remove residual potassium salts and impurities, then washed with deionized water and ethanol until neutral, and finally dried at 80°C.
[0051] Preparation of composite materials: Add ethanol and zirconium balls to lotus root hard carbon material and nano-silicon in a mass ratio of 1:1.5; the mass ratio of zirconium balls to lotus root hard carbon and nano-silicon mixed material is 1:10; ball mill for 4 hours to make the composite material evenly mixed; dry at 80°C to obtain a lotus root hard carbon / silicon composite material.
[0052] Comparative Example 4 Preparation of lotus root hard carbon material: The lotus root slices were placed in a sodium carbonate solution with a pH of 9 and soaked for 24 hours, wherein the mass ratio of lotus root to sodium carbonate solution was 2:1. After soaking, the lotus root slices changed from white to black. Then the lotus root strips were taken out and soaked in a hydrochloric acid solution with a pH of 2.5, wherein the mass ratio of lotus root to hydrochloric acid solution was 2:1, wherein the hydrochloric acid also contained 5g / 100ml of polyvinyl alcohol. After soaking for 24 hours, the lotus root strips were taken out and dried at 110°C for 12 hours. Then, in a quartz tube, high temperature carbonization was performed at 700°C for 4 hours under a N2 atmosphere. After carbonization, the strips were washed with a 1mol / L HCl solution to remove residual potassium salts and impurities, then washed with deionized water and ethanol until neutral, and finally dried at 80°C.
[0053] Preparation of composite materials: Add ethanol and zirconium balls to lotus root hard carbon material and nano-silicon in a mass ratio of 1:4; the mass ratio of zirconium balls to lotus root hard carbon and nano-silicon mixed material is 1:10; ball mill for 4 hours to make the composite material evenly mixed; dry at 80°C to obtain a lotus root hard carbon / silicon composite material.
[0054] Comparative Example 5 Preparation of lotus root hard carbon material: Soak the lotus root slices in a 3mol / L KOH solution for 24 hours, where the mass ratio of lotus root to KOH solution is 2:1. After soaking, the lotus root slices change from white to black sludge. The black lotus root sludge is taken out and dried at 110℃ for 12 hours. Then, carbonize at 700℃ for 4 hours in a quartz tube under N2 atmosphere. After carbonization, wash with 1mol / L HCl solution to remove residual potassium salts and impurities, then wash with deionized water and ethanol until neutral, and finally dry at 80℃.
[0055] Preparation of composite materials: Mix lotus root hard carbon material and nano-silicon in a mass ratio of 1:1, add ethanol and zirconium balls, and the mass ratio of zirconium balls to lotus root hard carbon and nano-silicon mixed material is 1:10. Ball mill for 4 hours to mix the composite material evenly; dry at 80°C to obtain a lotus root hard carbon / silicon composite material.
[0056] Comparative Example 6 Preparation of lotus root hard carbon material: The lotus root slices were placed in a sodium carbonate solution with a pH of 9 and soaked for 24 hours, where the mass ratio of lotus root to sodium carbonate solution was 2:1. After soaking, the lotus root slices changed from white to black. Then the lotus root strips were taken out and soaked in a hydrochloric acid solution with a pH of 2.5, where the mass ratio of lotus root to hydrochloric acid solution was 2:1. After soaking for 24 hours, the lotus root strips were taken out and dried at 110°C for 12 hours. Then, in a quartz tube, high-temperature carbonization was performed at 700°C for 2 hours under a N2 atmosphere. After carbonization, it was washed with a 1mol / L HCl solution to remove residual potassium salts and impurities, then washed with deionized water and ethanol until neutral, and finally dried at 80°C.
[0057] Preparation of composite materials: Mix lotus root hard carbon material and nano-silicon in a mass ratio of 1:1, add ethanol and zirconium balls, and the mass ratio of zirconium balls to lotus root hard carbon and nano-silicon mixed material is 1:10. Ball mill for 4 hours to mix the composite material evenly; dry at 80°C to obtain a lotus root hard carbon / silicon composite material.
[0058] Comparative Example 7 Comparative Example 7 is a pure silicon negative electrode.
[0059] The negative electrode materials prepared in Examples 1 to 7 and Comparative Examples 1 to 7 were used to prepare electrodes.
[0060] Preparation of electrode: Finally, the obtained lotus root hard carbon / silicon composite material is applied to the negative electrode and a button half-cell is assembled. Lotus root hard carbon / silicon composite material: SP: CMC: SBR = 96:1:1:2 is added to the agate mortar according to the mass ratio, and then an appropriate amount of deionized water solvent is dripped and fully ground. Finally, the mixture is evenly coated on the surface of the copper foil (i.e., the negative electrode current collector) and vacuum dried at 60°C for 12h. The dried pole piece is rolled and cut into discs with a diameter of 12mm. The lithium sheet is used as the counter electrode to determine the battery's gram capacity, rate performance, cycle performance and pole piece expansion. The gram capacity performance research mainly tests the gram capacity after activation for three weeks at 25℃0.2C, the rate performance research mainly tests the discharge capacity retention rate under 25℃2C constant current discharge, the cycle performance research mainly tests the capacity retention rate after 300 cycles at 25℃0.2C, and the expansion of the electrode after the cycle is mainly to disassemble the battery after 300 cycles, and measure the ratio of the thickness difference between the electrode after activation and the cycle for 300 weeks to the thickness before the cycle through SEM to calculate the volume expansion rate.
[0061] The test results are shown in Table 1 below: Table 1 Comparing Example 1 with Comparative Example 7, it can be seen that the introduction of lotus root hard carbon material can significantly improve the rate performance, cycle performance and active expansion of the battery, which is mainly due to the influence of the conductive electrons, ion network and buffer cavity provided by the lotus root hard carbon material. Compared with Examples 2-5 and Comparative Examples 1 / 2, it can be seen that the carbonization temperature affects the electrical properties of the material, mainly because the carbonization temperature changes the structure of the material, and the electrical performance is best when the carbonization temperature is 700°C; Compared with Examples 6 / 7 and Comparative Examples 3 / 4, it can be seen that the mass ratio of lotus root hard carbon material and nano-silicon material will affect the performance of the battery. As the proportion of nano-silicon material increases, the capacity of the battery increases, the rate performance and cycle performance of the battery decrease, and the expansion of the pole piece increases. When the proportion of nano-silicon in the composite material is greater than 60%, the battery cycle performance drops sharply, or even plummets; when the proportion of nano-silicon in the composite material is greater than 50%, the differences in the battery cycle, rate, and volume expansion are small. Combined with the characteristics that the greater the proportion of nano-silicon in the composite material, the higher the capacity, it is finally determined that when the mass ratio of lotus root hard carbon material to nano-silicon is 1:1, the battery performance is optimal. Compared with Example 5, after immersion in a high concentration of potassium hydroxide solution, Example 1 shows that the porous structure in the lotus root is destroyed, resulting in a significant decrease in the performance of the lotus root hard carbon prepared therefrom. In Comparative Example 6, since no structural stabilizer was added, part of the porous structure could not be maintained, resulting in a certain decrease in its performance.
[0062] The specific embodiments described herein are merely examples of the spirit of the present invention. A person skilled in the art of the present invention may make various modifications or additions to the specific embodiments described or replace them in a similar manner, but this will not deviate from the spirit of the present invention or exceed the scope defined by the appended claims.
Claims
1. A method for preparing lotus root hard carbon, characterized in that: The following steps are involved: (S.1) cutting the lotus root and pre-treating it to oxidize the polyphenols in the lotus root; (S.2) placing the pre-treated lotus root in a solution containing an acid and a structure stabilizer, so that soluble substances in the lotus root are dissolved; (S.3) drying and high-temperature carbonizing the lotus root treated in step (S.2) to obtain crude lotus root hard carbon; (S.4) removing impurities from the crude lotus root hard carbon to obtain the lotus root hard carbon.
2. The method for preparing lotus root hard carbon according to claim 1, characterized in that: The pretreatment in step (S.1) comprises the step of soaking the lotus root in an alkaline solution with a pH of 8.5-10; The pre-treatment time in the step (S.1) is greater than or equal to 6 hours.
3. The method for preparing lotus root hard carbon according to claim 2, characterized in that: The pH value of the acid solution in the step (S.2) is 2-3; The structural stabilizer is a combination of one or more of polyvinyl alcohol, polyethylene glycol, acrylamide, carboxymethyl cellulose, sodium polyacrylate, and sodium alginate; The concentration of the structural stabilizer is 0.5-10 g / 100 ml.
4. The method for preparing lotus root hard carbon according to claim 1, characterized in that: The high temperature carbonization temperature in the step (S.2) ranges from 500°C to 900°C.
5. A lotus root hard carbon, characterized in that: The invention is prepared by the method according to any one of claims 1 to 4.
6. A lotus root hard carbon / silicon composite material, characterized in that: The invention is obtained by compounding the lotus root hard carbon and nano silicon as claimed in claim 5.
7. The lotus root hard carbon / silicon composite material according to claim 6, characterized in that: The mass ratio of the lotus root hard carbon to the nano-silicon is 4:1-1:
1.
8. A method for preparing the lotus root hard carbon / silicon composite material as claimed in claim 5 or 6, characterized in that: Lotus root hard carbon and nano silicon are mixed, ethanol and zirconium balls are added, ball milling is performed to make the composite material evenly mixed, and drying is performed to obtain the lotus root hard carbon / silicon composite material.
9. The method according to claim 8, characterized in that The mass ratio of the zirconium ball to the lotus root hard carbon and nano-silicon mixed material is 1:5-15.
10. Use of the lotus root hard carbon as claimed in claim 5 or the lotus root hard carbon / silicon composite material as claimed in claim 6 or 7 in lithium ion batteries.
Citation Information
Patent Citations
A preparation method of biomass hard carbon material for negative electrode of sodium ion battery
CN109004199A
Lithium ion battery negative plate and preparation method and application thereof
CN113871574A
Preparation method and application of hard carbon negative electrode material
CN114702022A
Durian shell-based hard carbon negative electrode material and preparation method thereof
CN115650202A
Method for preparing hard carbon through cooperation of chemical gel and alkaline metal oxide template method and application of hard carbon
CN115974045A
Cited By
Lotus waste hierarchical carbon material, preparation method and application thereof
CN122789377A