Interdigital transducers and their fabrication methods, surface acoustic wave filters

By using a combination method of two layers of photoresist and preset chemical solvent in the preparation of SAW resonator, the problem of incomplete peeling in the peeling process is solved, and the electrical performance and reliability of the filter are improved.

CN118554909BActive Publication Date: 2024-11-08LANSUS TECH INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411014689.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-08
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

During the preparation of the SAW resonator, incomplete peeling is prone to occur in the peeling process, which affects the electrical performance and reliability of the filter.

Method used

The two-layer photoresist coating method is used to form a T-shaped structure by spin-coating the developer to ensure that a gap is formed between the metal film and the underlying photoresist, avoiding the photoresist adhesion, and peeling is performed using a preset chemical solvent.

Benefits of technology

It effectively avoids incomplete peeling and improves the electrical performance and reliability of interfinger transducers and surface acoustic filters.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118554909B_ABST
    Figure CN118554909B_ABST
Patent Text Reader

Abstract

The present invention is applicable to the field of wireless communication technology, and in particular, relates to an interdigital transducer and a preparation method thereof, and an acoustic surface filter. The method comprises the following steps: performing two photoresist and two hardening treatments on a wafer, performing exposure treatment, spin coating a developer, performing a coating treatment, and stripping a photoresist to obtain an interdigital transducer. Compared with the prior art, the present invention applies two layers of photoresist to a wafer. Due to the difference in the physical properties of the two layers of photoresist, in the subsequent spin coating process of the developer, the top layer of photoresist has more residual structure than the bottom layer of photoresist, forming a photoresist similar to a T-shaped structure, so that when the wafer is coated, a gap is formed between the metal film and the bottom layer of photoresist, effectively avoiding the photoresist adhering to the periphery of the metal film, causing the phenomenon of incomplete stripping, and effectively improving the electrical performance and reliability of the interdigital transducer and its acoustic surface filter.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention is applicable to the field of wireless communication technology, and in particular relates to an interdigital transducer and a preparation method thereof, and a surface acoustic wave filter. Background Art

[0002] As fifth-generation wireless communication technology solutions mature, smartphones need to add filters to support the increasing number of frequency bands. The dense frequency bands make the interference problem between uplinks in the system more prominent. In order to ensure high-quality data communication between spectrums, a typical high-end smartphone needs to be equipped with at least 50 RF front-end filters. With the continuous upgrading of communication technology (5G mobile phones) and the deployment of new technologies such as carrier aggregation (CA) and multiple-input multiple-output (MIMO), the number of communication frequency bands continues to increase, and this number will continue to grow violently.

[0003] Surface acoustic wave (SAW) resonator is a transducer passive bandpass filter made by using the piezoelectric effect and the physical properties of surface acoustic wave propagation. SAW resonator is increasingly valued in communication circuit design due to its small size, strong radiation resistance, high speed, low power consumption and high reliability. The resonant frequency of SAW resonator can be precisely tuned in a wide range through photolithography technology, and it has a small form factor, low connection loss and low cost, which is very suitable for monolithic integration of different frequency filters.

[0004] There are two mainstream SAW processing technologies: stripping and etching. The main difference between the two is the order of coating and coating. In the stripping process, after coating, the photoresist will be patterned, and then coated and stripped to finally obtain the interdigital transducer. Compared with the etching process, it is widely used by international leading manufacturers because of its better resolution.

[0005] However, the stripping process currently has certain technical defects, mainly manifested in the incomplete stripping phenomenon. The main reason is that during the coating process, the temperature of the evaporated aluminum film material is relatively high. After falling on the wafer surface, the photoresist will be further heated, so that its adhesion is further enhanced compared with the post-development baking, especially in the contact area between the interdigital transducer and the photoresist. Excessive adhesion can easily cause incomplete stripping, which will greatly affect the electrical performance and reliability of the filter.

[0006] Therefore, there is an urgent need for a new interdigital transducer and a preparation method thereof, and an acoustic surface filter to solve the above problems. Summary of the invention

[0007] The present invention provides an IDT and a preparation method thereof, and an acoustic surface filter, aiming to completely strip off the photoresist attached to the IDT during preparation, so as to improve the reliability and electrical performance of the IDT.

[0008] In a first aspect, the present invention provides a method for preparing an interdigital transducer, the method comprising the following steps:

[0009] S1, cleaning the surface of the wafer to obtain a first wafer;

[0010] S2, spin-coating a layer of first photoresist on the surface of the first wafer to obtain a second wafer coated with the first photoresist;

[0011] S3, performing a first hardening treatment on the second wafer to obtain a third wafer; wherein the baking time of the first hardening treatment on the second wafer is 20-45 seconds and the baking temperature is 70-100° C.;

[0012] S4, spin-coating a second layer of photoresist on the surface of the first layer of photoresist on the third wafer and performing a second hardening treatment to obtain a fourth wafer coated with two layers of photoresist;

[0013] S5, performing exposure processing on the fourth wafer to obtain a fifth wafer;

[0014] S6, spin-coating a developer on the surface of the fifth wafer to remove an unexposed area on the fifth wafer to obtain a sixth wafer; wherein the remaining structure of the second layer of photoresist of the sixth wafer is greater than the remaining structure of the first layer of photoresist of the sixth wafer;

[0015] S7, performing a coating process on the sixth wafer to obtain a seventh wafer;

[0016] S8. Stripping the photoresist on the seventh wafer by using a preset chemical solvent to obtain an IDT.

[0017] Preferably, step S4 includes the following sub-steps:

[0018] S41a, spin-coating a second photoresist on the surface of the first photoresist layer of the third wafer, wherein the sensitivity of the second photoresist is lower than that of the first photoresist;

[0019] S42a, performing a second hardening treatment on the third wafer after spin coating the second photoresist to obtain the fourth wafer, wherein the baking time of the second hardening treatment on the third wafer is 20-45 seconds and the baking temperature is 70-100°C.

[0020] Preferably, the sensitivity of the first photoresist is 1.3-2.0 times the sensitivity of the second photoresist.

[0021] Preferably, the sensitivity of the first photoresist is in the range of 10-1000 mJ / cm 2 .

[0022] Preferably, step S4 includes the following sub-steps:

[0023] S41b, spin coating the first photoresist on the surface of the first photoresist layer of the third wafer to form a second photoresist layer;

[0024] S42b, performing a second hardening treatment on the third wafer after spin coating the first photoresist through a heating platform to obtain the fourth wafer; wherein, the baking time of the second hardening treatment is 20-45 seconds, and the baking temperature of the second hardening treatment is higher than the baking temperature of the first hardening treatment.

[0025] Preferably, the baking temperature during the second film hardening treatment is 5-30° C. higher than the baking temperature during the first film hardening treatment.

[0026] Preferably, the preset chemical solvent includes N-methylpyrrolidone and tetramethylammonium hydroxide;

[0027] Based on the total mass of the preset chemical solvent, the mass of the N-methylpyrrolidone accounts for 5%-30% of the total mass of the preset chemical solvent, the mass of the tetramethylammonium hydroxide accounts for 2.5% of the total mass of the preset chemical solvent, and the remainder is water.

[0028] Preferably, in step S1, the surface of the wafer is cleaned by ultrasound; in step S2, a layer of first photoresist is spin-coated on the surface of the first wafer by a high-speed coating machine; in step S3, the second wafer is subjected to a first hardening treatment by a heating platform; in step S5, the fourth wafer is exposed by a deep ultraviolet light source through a mask; in step S7, the sixth wafer is coated by electron beam evaporation.

[0029] In a second aspect, the present invention further provides an IDT, which is manufactured by the IDT manufacturing method as described in the above embodiment.

[0030] In a third aspect, a surface acoustic wave filter is provided, wherein the surface acoustic wave filter comprises the interdigital transducer as described in the above embodiment.

[0031] Compared with the prior art, the present invention applies two layers of photoresist to the wafer. Due to the difference in the properties of the two layers of photoresist, in the subsequent spin coating of the developer, the top layer of photoresist will have more residual structure than the bottom layer of photoresist, forming a photoresist similar to a T-shaped structure, so that when the wafer is coated, a gap will be formed between the metal film and the bottom layer of photoresist, effectively avoiding the photoresist adhering to the periphery of the metal film and causing incomplete peeling, thereby effectively improving the electrical performance and reliability of the interdigital transducer and its surface acoustic wave filter. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] The present invention will be described in detail below in conjunction with the accompanying drawings. The above and other aspects of the present invention will become clearer and easier to understand through the detailed description made in conjunction with the following drawings. In the accompanying drawings:

[0033] Figure 1 is a flow chart of a method for preparing an interdigital transducer provided by an embodiment of the present invention;

[0034] Figure 2 Schematic diagram of the interface between the metal film and the photoresist in the method for preparing the interdigital transducer provided by an embodiment of the present invention;

[0035] Figure 3 It is a cross-sectional schematic diagram of the preparation process flow of a specific embodiment 1 of the preparation method of the interdigital transducer provided in an embodiment of the present invention;

[0036] Figure 4 It is a schematic cross-sectional diagram of the preparation process flow of specific embodiment 2 of the method for preparing an interdigital transducer provided in an embodiment of the present invention.

[0037] In the figure, 1, a first wafer, 2, a second wafer, 3, a third wafer, 4, a fourth wafer, 5, a fifth wafer, 6, a sixth wafer, 7, a seventh wafer, 8, an interdigital transducer, 11, a first photoresist, 12, a second photoresist, 13, a mask, and 14, a metal film. DETAILED DESCRIPTION

[0038] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0039] Implementation Method 1

[0040] Please refer to Figure 1-Figure 4 The present invention provides a method for preparing an interdigital transducer, the method comprising the following steps:

[0041] S1. Clean the surface of a wafer to obtain a first wafer 1.

[0042] In the embodiment of the present invention, the surface of the wafer is cleaned by ultrasonic waves.

[0043] S2. Spin-coat a layer of first photoresist 11 on the surface of the first wafer 1 to obtain a second wafer 2 coated with the first photoresist layer.

[0044] In the embodiment of the present invention, the sensitivity range of the first photoresist 11 is 10-1000 mJ / cm 2 , the first photoresist 11 is evenly spin-coated on the first wafer 1 by a high-speed photoresist coating machine.

[0045] S3, performing a first hardening treatment on the second wafer 2 to obtain a third wafer 3; wherein, the baking time of the first hardening treatment on the second wafer 2 is 20-45 seconds, and the baking temperature is 70-100°C.

[0046] In an embodiment of the present invention, the second wafer 2 is subjected to a first hardening treatment through a heating platform. The first hardening treatment removes part of the residual water vapor in the first photoresist 11 to form the first photoresist 11 after the first hardening treatment, thereby improving the adhesion and stability between the first photoresist 11 and the surface of the second wafer 2.

[0047] S4, spin-coating a second layer of photoresist on the surface of the first layer of photoresist on the third wafer 3 and performing a second hardening treatment to obtain a fourth wafer 4 coated with two layers of photoresist.

[0048] In an embodiment of the present invention, the second layer of photoresist has different physical properties from the first layer of photoresist, and since the two layers of photoresist have different physical properties after the second hardening treatment (such as sensitivity, hardness, viscosity, etc.), when the developer is spin-coated in the subsequent step S6, the remaining structure of the second layer of photoresist after the developer is spin-coated will be greater than the remaining structure of the first layer of photoresist.

[0049] S5 , performing exposure processing on the fourth wafer 4 to obtain a fifth wafer 5 .

[0050] In the embodiment of the present invention, a deep ultraviolet light source is used to expose the fourth wafer 4 through the mask 13 , and the exposure time of the deep ultraviolet light source (DUV) through the mask 13 on the fourth wafer 4 can be set according to actual conditions.

[0051] S6. Spin-coat a developer on the fifth wafer 5 to remove unexposed areas on the fifth wafer 5 to obtain a sixth wafer 6; wherein the remaining structure of the second layer of photoresist on the sixth wafer 6 is greater than the remaining structure of the first layer of photoresist on the sixth wafer 6.

[0052] In an embodiment of the present invention, due to the difference in physical properties between the second layer of photoresist and the first layer of photoresist, there is a difference in the development effect of the developer, so that the remaining structure of the second layer of photoresist of the sixth wafer 6 is greater than the remaining structure of the first layer of photoresist of the sixth wafer 6.

[0053] S7 , performing coating treatment on the sixth wafer 6 to obtain a seventh wafer 7 .

[0054] In an embodiment of the present invention, the sixth wafer 6 is coated by electron beam evaporation. Since the second layer of photoresist has more residual structure than the first layer of photoresist, when the metal film 14 is coated, a circle of gap will be formed between the first layer of photoresist, which effectively prevents the photoresist from adhering to the periphery of the metal film 14 and causing incomplete peeling.

[0055] S8 . Stripping the photoresist on the seventh wafer 7 by using a preset chemical solvent to obtain an IDT 8 .

[0056] In an embodiment of the present invention, the preset chemical solvent includes N-methylpyrrolidone (NMP) and tetramethylammonium hydroxide (TMAH); based on the total mass of the preset chemical solvent, the mass of the N-methylpyrrolidone accounts for 5%-30% of the total mass of the preset chemical solvent, and the mass of the tetramethylammonium hydroxide accounts for 2.5% of the total mass of the preset chemical solvent.

[0057] Compared with the prior art, the present invention applies two layers of photoresist to the wafer. Due to the difference in the properties of the two layers of photoresist, in the subsequent spin coating of the developer, the top layer of photoresist will have more residual structure than the bottom layer of photoresist, forming a photoresist similar to a T-shaped structure, so that when the wafer is coated, a gap will be formed between the metal film and the bottom layer of photoresist, effectively avoiding the photoresist adhering to the periphery of the metal film and causing incomplete peeling, thereby effectively improving the electrical performance and reliability of the interdigital transducer and its surface acoustic wave filter.

[0058] In order to better reflect the technical effects achieved by the embodiments of the present invention, two specific embodiments are described in detail below: Specific embodiment 1

[0060] Please refer to Figure 3 , Figure 3 It is a cross-sectional schematic diagram of the preparation process flow of a specific embodiment 1 of the preparation method of the interdigital transducer 8 provided in an embodiment of the present invention.

[0061] S1. Clean the surface of a wafer to obtain a first wafer 1.

[0062] In the embodiment of the present invention, the surface of the wafer is cleaned by ultrasonic waves.

[0063] S2. Spin-coat a layer of first photoresist 11 on the surface of the first wafer 1 to obtain a second wafer 2 coated with the first photoresist layer.

[0064] In the embodiment of the present invention, the sensitivity range of the first photoresist 11 is 10-1000 mJ / cm 2 , the first photoresist 11 is evenly spin-coated on the first wafer 1 by a high-speed photoresist coating machine.

[0065] S3, performing a first hardening treatment on the second wafer 2 to obtain a third wafer 3; wherein, the baking time of the first hardening treatment on the second wafer is 20-45 seconds, and the baking temperature is 70-100°C.

[0066] In an embodiment of the present invention, the second wafer 2 is subjected to a first hardening treatment through a heating platform. The first hardening treatment removes part of the residual water vapor in the first photoresist 11 to form the first hardened first photoresist 11, thereby improving the adhesion and stability between the first photoresist 11 and the surface of the second wafer 2.

[0067] S4, spin-coating a second layer of photoresist on the surface of the first layer of photoresist on the third wafer 3 and performing a second hardening treatment to obtain a fourth wafer 4 coated with two layers of photoresist.

[0068] In the embodiment of the present invention, step S4 includes the following sub-steps:

[0069] S41a, spin-coating a second photoresist 12 on the surface of the first photoresist layer of the third wafer 3, wherein the sensitivity of the second photoresist 12 is lower than that of the first photoresist 11;

[0070] Specifically, the sensitivity range of the second photoresist 12 is 10-1000 mJ / cm 2 , and the sensitivity of the first photoresist 11 is 1.3-2.0 times that of the second photoresist 12. When the sensitivity of the photoresists during the two spin coatings is slightly different, the exposure time and exposure dose in step S5 can be appropriately adjusted.

[0071] S42a, performing a second hardening treatment on the third wafer 3 after spin coating the second photoresist 12 to obtain the fourth wafer 4, wherein the baking time of the second hardening treatment on the third wafer 3 is 20-45 seconds and the baking temperature is 70-100°C.

[0072] Specifically, due to the difference in sensitivity between the two layers of photoresist after the second hardening treatment, when the developer is spin-coated in the subsequent step S6, the remaining structure of the second layer of photoresist after the developer is spin-coated will be greater than the remaining structure of the first layer of photoresist, and a T-shaped photoresist will be formed as a whole.

[0073] S5 , performing exposure processing on the fourth wafer 4 to obtain a fifth wafer 5 .

[0074] In the embodiment of the present invention, a deep ultraviolet light source is used to expose the fourth wafer 4 through the mask 13 , and the exposure time of the deep ultraviolet light source (DUV) through the mask 13 on the fourth wafer 4 can be set according to actual conditions.

[0075] S6. Spin-coat a developer on the fifth wafer 5 to remove unexposed areas on the fifth wafer 5 to obtain a sixth wafer 6; wherein the remaining structure of the second layer of photoresist on the sixth wafer 6 is greater than the remaining structure of the first layer of photoresist on the sixth wafer 6.

[0076] In the embodiment of the present invention, due to the difference in sensitivity between the second layer of photoresist and the first layer of photoresist, there is a difference in the development effect of the developer, so that the remaining structure of the second layer of photoresist of the sixth wafer 6 is greater than the remaining structure of the first layer of photoresist of the sixth wafer 6.

[0077] S7 , performing coating treatment on the sixth wafer 6 to obtain a seventh wafer 7 .

[0078] In an embodiment of the present invention, the sixth wafer 6 is coated by electron beam evaporation. Since the second layer of photoresist has more residual structure than the first layer of photoresist, when the metal film 14 is coated, a circle of gap will be formed between the first layer of photoresist, which effectively prevents the photoresist from adhering to the periphery of the metal film 14 and causing incomplete peeling.

[0079] S8 . Stripping the photoresist on the seventh wafer 7 by using a preset chemical solvent to obtain an IDT 8 .

[0080] In an embodiment of the present invention, the preset chemical solvent includes N-methylpyrrolidone (NMP) and tetramethylammonium hydroxide (TMAH); based on the total mass of the preset chemical solvent, the mass of the N-methylpyrrolidone accounts for 5%-30% of the total mass of the preset chemical solvent, and the mass of the tetramethylammonium hydroxide accounts for 2.5% of the total mass of the preset chemical solvent. Specific embodiment 2

[0082] Please refer to Figure 4 , Figure 4It is a cross-sectional schematic diagram of the preparation process flow of specific embodiment 2 of the preparation method of the interdigital transducer 8 provided in an embodiment of the present invention.

[0083] S1. Clean the surface of a wafer to obtain a first wafer 1.

[0084] In the embodiment of the present invention, the surface of the wafer is cleaned by ultrasonic waves.

[0085] S2. Spin-coat a layer of first photoresist 11 on the surface of the first wafer 1 to obtain a second wafer 2 coated with the first photoresist layer.

[0086] In the embodiment of the present invention, the sensitivity range of the first photoresist 11 is 10-1000 mJ / cm 2 , the first photoresist 11 is evenly spin-coated on the first wafer 1 by a high-speed photoresist coating machine.

[0087] S3, performing a first hardening treatment on the second wafer 2 to obtain a third wafer 3; wherein, the baking time of the first hardening treatment on the second wafer is 20-45 seconds, and the baking temperature is 70-100°C.

[0088] In an embodiment of the present invention, the second wafer 2 is subjected to a first hardening treatment through a heating platform. The first hardening treatment removes part of the residual water vapor in the first photoresist 11, thereby improving the adhesion and stability between the first photoresist 11 and the surface of the second wafer 2.

[0089] S4, spin-coating a second layer of photoresist on the surface of the first layer of photoresist on the third wafer 3 and performing a second hardening treatment to obtain a fourth wafer 4 coated with two layers of photoresist.

[0090] In the embodiment of the present invention, step S4 includes the following sub-steps:

[0091] S41b, spin-coating the first photoresist 11 on the surface of the first photoresist layer of the third wafer 3 to form a second photoresist layer;

[0092] S42b, the third wafer 3 after spin coating the first photoresist 11 is subjected to a second hardening treatment through the heating platform to obtain the fourth wafer 4; wherein, the baking time of the second hardening treatment is 20-45 seconds, and the baking temperature of the second hardening treatment is higher than the baking temperature of the first hardening treatment, and is higher than 5-35°C.

[0093] Specifically, due to the difference in hardness and viscosity between the two layers of photoresist after the second hardening treatment, when the developer is spin-coated in the subsequent step S6, the remaining structure of the second layer of photoresist after the developer is spin-coated will be greater than the remaining structure of the first layer of photoresist, forming a T-shaped photoresist as a whole.

[0094] S5 , performing exposure processing on the fourth wafer 4 to obtain a fifth wafer 5 .

[0095] In the embodiment of the present invention, a deep ultraviolet light source is used to expose the fourth wafer 4 through the mask 13 , and the exposure time of the deep ultraviolet light source (DUV) through the mask 13 on the fourth wafer 4 can be set according to actual conditions.

[0096] S6. Spin-coat a developer on the fifth wafer 5 to remove unexposed areas on the fifth wafer 5 to obtain a sixth wafer 6; wherein the remaining structure of the second layer of photoresist on the sixth wafer 6 is greater than the remaining structure of the first layer of photoresist on the sixth wafer 6.

[0097] In an embodiment of the present invention, due to the difference in physical properties between the second layer of photoresist and the first layer of photoresist, there is a difference in the development effect of the developer, so that the remaining structure of the second layer of photoresist of the sixth wafer 6 is greater than the remaining structure of the first layer of photoresist of the sixth wafer 6.

[0098] S7 , performing coating treatment on the sixth wafer 6 to obtain a seventh wafer 7 .

[0099] In an embodiment of the present invention, the sixth wafer 6 is coated by electron beam evaporation. Since the second layer of photoresist has more residual structure than the first layer of photoresist, when the metal film 14 is coated, a circle of gap will be formed between the first layer of photoresist, which effectively prevents the photoresist from adhering to the periphery of the metal film 14 and causing incomplete peeling.

[0100] S8 . Stripping the photoresist on the seventh wafer 7 by using a preset chemical solvent to obtain an IDT 8 .

[0101] In an embodiment of the present invention, the preset chemical solvent includes N-methylpyrrolidone (NMP) and tetramethylammonium hydroxide (TMAH); based on the total mass of the preset chemical solvent, the mass of the N-methylpyrrolidone accounts for 5%-30% of the total mass of the preset chemical solvent, and the mass of the tetramethylammonium hydroxide accounts for 2.5% of the total mass of the preset chemical solvent.

[0102] Implementation Method 2

[0103] The present invention also provides an IDT, which is manufactured by the IDT manufacturing method described above. Since the IDT in this embodiment is manufactured by the IDT manufacturing method in the first embodiment, the IDT in this embodiment can also achieve the technical effect achieved by the IDT manufacturing method in the first embodiment, and no further description is given here.

[0104] Implementation Method 3

[0105] The present invention also provides a surface acoustic wave filter, wherein the surface acoustic wave filter includes the interdigital transducer described in Embodiment 2. Since the surface acoustic wave filter in this embodiment includes the interdigital transducer in Embodiment 2, the surface acoustic wave filter in this embodiment can also achieve the technical effect achieved by the interdigital transducer in Embodiment 2, which will not be described in detail here.

[0106] It should be noted that, in this article, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, an element defined by the sentence "comprises a ..." does not exclude the existence of other identical elements in the process, method, article or device including the element.

[0107] The embodiments of the present invention are described above in conjunction with the accompanying drawings. What is disclosed is only the preferred embodiment of the present invention. However, the present invention is not limited to the above-mentioned specific implementation manner. The above-mentioned specific implementation manner is only illustrative rather than restrictive. Under the enlightenment of the present invention, ordinary technicians in this field can also make many forms and equivalent changes without departing from the scope of protection of the purpose of the present invention and the claims, all of which are within the protection of the present invention.

Claims

1. A method for preparing an interdigital transducer, characterized in that: The preparation method comprises the following steps: S1, cleaning the surface of the wafer to obtain a first wafer; S2, spin-coating a layer of first photoresist on the surface of the first wafer to obtain a second wafer coated with the first photoresist; S3, performing a first hardening treatment on the second wafer to obtain a third wafer; wherein the baking time of the first hardening treatment on the second wafer is 20-45 seconds and the baking temperature is 70-100° C.; S4, spin-coating a second layer of photoresist on the surface of the first layer of photoresist on the third wafer and performing a second hardening treatment to obtain a fourth wafer coated with two layers of photoresist; S5, performing exposure processing on the fourth wafer to obtain a fifth wafer; S6, spin-coating a developer on the surface of the fifth wafer to remove an unexposed area on the fifth wafer to obtain a sixth wafer; wherein the remaining structure of the second layer of photoresist of the sixth wafer is greater than the remaining structure of the first layer of photoresist of the sixth wafer; S7, performing a coating process on the sixth wafer to obtain a seventh wafer; S8. Stripping the photoresist on the seventh wafer by using a preset chemical solvent to obtain an IDT.

2. The method for preparing an interdigital transducer according to claim 1, characterized in that: Step S4 includes the following sub-steps: S41a, spin-coating a second photoresist on the surface of the first photoresist layer of the third wafer, wherein the sensitivity of the second photoresist is lower than that of the first photoresist; S42a, performing a second hardening treatment on the third wafer after spin coating the second photoresist to obtain the fourth wafer, wherein the baking time of the second hardening treatment on the third wafer is 20-45 seconds and the baking temperature is 70-100°C.

3. The method for preparing an interdigital transducer according to claim 2, characterized in that: The sensitivity of the first photoresist is 1.3-2.0 times the sensitivity of the second photoresist.

4. The method for preparing an interdigital transducer according to claim 3, characterized in that: The sensitivity of the first photoresist ranges from 10 to 1000 mJ / cm 2 .

5. The method for preparing an IDT according to claim 1, characterized in that: Step S4 includes the following sub-steps: S41b, spin coating the first photoresist on the surface of the first photoresist layer of the third wafer to form a second photoresist layer; S42b, performing a second hardening treatment on the third wafer after spin coating the first photoresist through a heating platform to obtain the fourth wafer; wherein, the baking time of the second hardening treatment is 20-45 seconds, and the baking temperature of the second hardening treatment is higher than the baking temperature of the first hardening treatment.

6. The method for preparing an interdigital transducer according to claim 5, characterized in that: The baking temperature during the second film hardening treatment is 5-30°C higher than the baking temperature during the first film hardening treatment.

7. The method for preparing an IDT according to claim 1, characterized in that: The preset chemical solvent includes N-methylpyrrolidone and tetramethylammonium hydroxide; Based on the total mass of the preset chemical solvent, the mass of the N-methylpyrrolidone accounts for 5%-30% of the total mass of the preset chemical solvent, the mass of the tetramethylammonium hydroxide accounts for 2.5% of the total mass of the preset chemical solvent, and the remainder is water.

8. The method for preparing an interdigital transducer according to claim 1, characterized in that: In step S1, the surface of the wafer is cleaned by ultrasound; in step S2, a layer of the first photoresist is spin-coated on the surface of the first wafer by a high-speed coating machine; in step S3, the second wafer is subjected to a first hardening treatment by a heating platform; in step S5, the fourth wafer is exposed by a deep ultraviolet light source through a mask; in step S7, the sixth wafer is coated by electron beam evaporation.

9. An interdigital transducer, characterized in that: The IDT is manufactured by the IDT manufacturing method according to claims 1-8.

10. A surface acoustic wave filter, characterized in that: The surface acoustic wave filter comprises the interdigital transducer according to claim 9.