A rGO-loaded manganese oxide catalyst for removing formaldehyde at room temperature and preparation method thereof
The rGO-supported manganese oxide catalyst is formed by one-step hydrogen reduction method, which solves the problem of insufficient catalytic oxidation performance and stability of manganese-based oxides at room temperature, and achieves efficient formaldehyde elimination and good circulation performance, which is suitable for room temperature applications.
Patent Information
- Application Number
- CN202411001060.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-25
AI Technical Summary
The existing manganese-based oxide catalysts lack the catalytic oxidation performance and stability of formaldehyde at room temperature, mainly due to the low catalytic activity and poor circulation performance caused by the small amount of oxygen vacancy and the prone to agglomeration of nanomaterials.
The one-step hydrogen reduction method is used to reduce graphene oxide to rGO during the roasting process, and the Mn precursor is dehydrated and reduced to manganese oxide in various valence states to form an rGO-supported manganese oxide catalyst, increasing oxygen vacancy and catalytic activity, and avoiding Aggregation of manganese oxides improves circulation performance.
It achieves efficient formaldehyde elimination, stronger catalytic activity, significantly improved circulation performance, and maintains good performance under high humidity conditions, making it suitable for room temperature applications.
Smart Images

Figure CN118558317B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of formaldehyde removal catalysts, and specifically relates to an rGO-loaded manganese oxide catalyst for removing formaldehyde at room temperature and a preparation method thereof. Background Art
[0002] Formaldehyde (HCHO) is the most common and serious indoor air pollutant. It affects the upper respiratory tract and lungs, causes liver function, immune function and nervous system abnormalities, and even induces cancer in severe cases. It is extremely harmful to human health. Therefore, the elimination of indoor formaldehyde gas has received more and more attention.
[0003] Studies have shown that room temperature catalytic oxidation technology is one of the most efficient technologies for purifying formaldehyde, and catalytic materials are the core factors that determine the performance of formaldehyde catalytic oxidation elimination. Therefore, it is very important to find a catalytic material with excellent performance.
[0004] Compared with other non-precious metals, manganese-based oxides have multiple valence states and different crystal phases, excellent catalytic performance and strong oxidation ability, and are a catalytic material with great application prospects. At present, the application research of manganese-based oxides in formaldehyde purification has made good progress. For example, patent document CN117398992A discloses a method for preparing a manganese dioxide catalyst for catalytic decomposition of formaldehyde, which mainly comprises Mn 2+ The product is prepared by oxidizing an inorganic salt, then adding an alkali solution to adjust the pH, separating the solid and the liquid, and drying. The obtained manganese dioxide catalyst has a very good formaldehyde catalytic decomposition effect at a high temperature of 85°C, which can reach up to more than 99%. However, its formaldehyde catalytic decomposition effect is poor under relatively low temperature conditions. In addition, the formaldehyde catalytic decomposition performance of the manganese dioxide catalyst still has room for improvement under the conditions of high formaldehyde space velocity and low concentration.
[0005] Many researchers have tried different approaches. For example, patent document CN117816151A discloses a manganese dioxide catalyst for decomposing formaldehyde. The crystal structure of the catalyst is delta-MnO2 type, and the specific surface area of the catalyst is greater than or equal to 50 m 2 / g; manganese salt and potassium salt are used as raw materials, the molar ratio of K to Mn is 0.05-0.25, and hydrothermal treatment is carried out at 80-200°C for 1-24h. However, the document does not mention the cyclic reaction, does not verify the persistence of activity, and has limitations in practical application.
[0006] Patent document CN107754785A discloses a graphene-manganese oxide composite catalyst for low-temperature catalytic oxidation of formaldehyde, including graphene nanosheets and manganese oxide nanosheets loaded on the graphene nanosheets; including the following steps: 1) dispersing graphene oxide in deionized water, and then ultrasonically dispersing for 10-60 minutes to obtain a graphene oxide dispersion; transferring the graphene oxide dispersion into a reactor, sealing and reacting at 80-200°C for 6-18 hours, centrifuging, washing and freeze-drying after the reaction to obtain graphene nanosheets; 2) mixing the graphene nanosheets and potassium permanganate aqueous solution, and then stirring and reacting at room temperature for 10-24 hours, washing, filtering and freeze-drying after the reaction to obtain a graphene-manganese oxide composite catalyst. However, the document does not mention the phenomenon that the manganese oxide catalyst is deactivated at high humidity, and no humidity verification is performed.
[0007] Patent document CN117427630A discloses a δ-MnO2-GO catalyst and its preparation method and application in formaldehyde degradation at room temperature, including the following steps: S1. Prepare 1.6-10g / L graphene oxide aqueous solution, add manganese sulfate to the graphene oxide solution, so that the concentration of manganese sulfate is 50-300g / L, and obtain a mixed solution; S2. Add a potassium permanganate aqueous solution with a concentration of 30-60g / L to the mixed solution of S1, stir for 30min, age at room temperature for more than 12h, and dry. The document uses low-amount GO doping to significantly limit the growth of manganese dioxide nanosheets and create abundant mass transfer channels. The δ-MnO2-GO catalyst presents a unique two-dimensional crown structure, and the δ-MnO2 nanorods with a two-dimensional coral-like hierarchical pore structure are uniformly dispersed on the planar structure of GO. Graphene oxide has many surface active groups and is more likely to absorb moisture, which has a great influence on the catalytic activity of manganese oxide, but the document does not mention the influence of humidity and its influence on catalytic activity.
[0008] Patent document CN118237010A discloses a composite catalyst for efficient formaldehyde elimination, wherein the raw materials for preparation include phase A and phase B, wherein phase A includes activated carbon powder, wherein the specific surface area of the activated carbon powder is greater than 1000 m2 / g, and the mesh size is greater than 300 meshes; phase B includes a manganese source compound and an alkaline solution; the manganese source compound includes one of manganese sulfate, manganese acetate, manganese chloride or manganese oxalate, and the alkaline solution includes one of potassium hydroxide solution, sodium hydroxide solution, potassium carbonate solution, potassium bicarbonate solution, sodium carbonate solution or sodium bicarbonate solution; the document is prepared by hydrophilic modification of activated carbon powder, and then reacting with a manganese source compound and an alkaline solution. However, the synergistic effect of activated carbon powder and manganese oxide is not reflected in the document, and only the structure of activated carbon is used to avoid the agglomeration of manganese oxide, which is not very helpful for the catalytic activity and regeneration of manganese oxide, so the cyclicity of room temperature catalytic oxidation of formaldehyde still needs to be improved.
[0009] The above literature still has the problem of poor performance and stability of manganese-based oxides in catalytic oxidation of formaldehyde at room temperature. The main reason is that manganese-based oxides have fewer oxygen vacancies, which affects the catalytic activity. In addition, nanomaterials are easy to agglomerate, resulting in reduced performance and stability. Summary of the invention
[0010] The purpose of the present invention is to provide an rGO-loaded manganese oxide catalyst for removing formaldehyde at room temperature and a preparation method thereof, so as to solve the problems of low catalytic activity and poor cycle performance caused by insufficient oxygen vacancies and easy agglomeration in the prior art.
[0011] The purpose of the present invention is achieved through the following technical solutions:
[0012] The present invention discloses an rGO-supported manganese oxide catalyst for removing formaldehyde at room temperature, wherein a Mn precursor is supported on graphene oxide, and then reduced by hydrogen once and calcined at 200-500° C. to form an rGO-supported manganese oxide catalyst; the mass fraction of manganese oxide in the catalyst is 10%-70%, preferably 20%-60%; the graphene oxide is reduced by hydrogen to become reduced graphene oxide (usually abbreviated as rGO, where r means reduced);
[0013] The graphene oxide is a common commercially available multilayer graphene oxide with 2 to 5 layers and a specific surface area of ≥100 m 2 / g, the larger the specific surface area, the better the effect, and the better the hydrophilicity, the better the effect; for example, the DN-20DY brand product produced by Zhejiang Zhiti Nano Micro New Materials Co., Ltd.
[0014] The Mn precursor is formed by a precipitation reaction between a manganese source compound and an alkaline solution, wherein the manganese source compound is at least one of manganese sulfate, manganese acetate, manganese nitrate, manganese chloride or manganese oxalate; and the alkaline solution is at least one of a potassium hydroxide solution, a sodium hydroxide solution, a potassium carbonate solution, a potassium bicarbonate solution, a sodium carbonate solution or a sodium bicarbonate solution with a mass concentration of 1% to 15%.
[0015] The method for preparing a rGO-supported manganese oxide catalyst for removing formaldehyde at room temperature according to the present invention comprises the following steps:
[0016] S1, dispersing the graphene oxide in water, stirring to make it uniform, and obtaining a graphene oxide solution;
[0017] S2, adding a manganese source compound to the graphene oxide solution, and stirring to obtain a mixed solution;
[0018] S3, adding an alkaline solution dropwise to the mixed solution, adjusting the pH value of the solution to 9-12, and stirring to perform a precipitation reaction;
[0019] S4, filtering, washing, and drying the reaction product to obtain graphene oxide loaded with a Mn precursor;
[0020] S5. Grind the graphene oxide loaded with the Mn precursor, place it in an atmosphere furnace and calcine it at 200-500° C., and introduce hydrogen as a protective gas and a reaction raw material to reduce the graphene oxide once; thus, the rGO-loaded manganese oxide catalyst for removing formaldehyde at room temperature can be obtained.
[0021] Preferably, the mass concentration of the manganese source compound in the mixed solution is 0.5% to 2%, and the precipitation reaction time is 1 to 5 hours.
[0022] Preferably, the precipitation reaction time in step S3 is 1 to 5 hours.
[0023] Preferably, the drying temperature of step S4 is 20-100° C., and the drying time is 1-6 hours.
[0024] Preferably, the calcination time in step S5 is 1 to 6 hours, and the flow rate of hydrogen is controlled at 15 to 45 ml / min.
[0025] The above-mentioned solution concentration, pH value, precipitation time, calcination temperature and calcination time will all affect the crystal form (β-MnO2, γ-MnO2, α-Mn2O3, γ-Mn2O3, α-Mn3O4 and Mn5O8) of the prepared manganese-based oxides and the valence state (+Ⅱ, +Ⅲ, +Ⅳ) of the manganese atoms, thereby changing the formaldehyde elimination performance parameters of the final product.
[0026] Compared with the prior art, the present invention has the following advantages:
[0027] The present invention adopts a one-step reduction method of hydrogen to reduce graphene oxide to rGO and dehydrate and reduce the Mn precursor to a mixture of manganese oxides of various valence states (MnO 2-x ), more oxygen vacancies, and stronger catalytic activity; one-step reduction makes the composite of manganese oxide and rGO more solid, avoiding the agglomeration of manganese oxide during the catalytic reaction and increasing the cycle performance; rGO is more stable than GO, has good conductivity, is conducive to electron transmission, and is helpful for the catalytic reaction and regeneration of manganese oxide, thereby increasing the cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The formaldehyde decomposition rate curves under different reaction cycles of Example 1 and Comparative Examples 1-3 are shown.
[0029] Figure 2 The formaldehyde decomposition rate curves of Example 2 and Comparative Examples 2, 4-5 at high air velocity and low concentration.
[0030] Figure 3The formaldehyde decomposition rate curves of Example 3 and Comparative Example 1 at high air velocity and low concentration are shown. DETAILED DESCRIPTION
[0031] Those skilled in the art should realize that the present embodiment is only used to illustrate the present invention, but not to limit the present invention.
[0032] The raw materials used in the present invention are all commercially available products: graphene oxide: Zhejiang Zhitai Nanowei New Materials Co., Ltd., DN-20DY brand, thickness 1-3nm, number of layers 2-5; MnCl2: Aladdin, M591138, anhydrous, 98%; Na2CO3: Aladdin, S432761, anhydrous, powder, 99.5%; MnO2: Aladdin, M101135, AR, 85%; Mn(NO3)2 4H2O: Aladdin, M191978, tetrahydrate, 98%; NaOH: Aladdin, S111498, AR, 96%.
[0033] Example 1: Formaldehyde elimination test
[0034] A method for preparing an rGO-supported manganese oxide catalyst for removing formaldehyde at room temperature comprises the following steps:
[0035] S1. Disperse 0.6 g of graphene oxide in 150 mL of water and stir for 1 h to make it uniform to obtain a graphene oxide solution;
[0036] S2, adding 1.26 g (0.01 mol) of MnCl2 into the graphene oxide solution, stirring to obtain a uniform mixed solution of MnCl2 and graphene oxide;
[0037] S3, adding Na2CO3 solution dropwise to the mixed solution, adjusting the pH value of the solution to 9.5, stirring for precipitation reaction until no more precipitate is generated;
[0038] S4, filtering and washing the reaction product, and drying it by air blast at 200° C. to obtain graphene oxide loaded with a Mn precursor (Mn(OH)4);
[0039] S5. Grind and break up the graphene oxide loaded with the Mn precursor, place it in an atmosphere furnace, and calcine it at 350°C for 4 hours under hydrogen protection (flow rate 15 mL / min) to reduce the graphene oxide once; a 60 wt% (mass fraction of manganese oxide in the catalyst, the same below) rGO-loaded manganese oxide catalyst for removing formaldehyde at room temperature can be obtained, and the yield is 63.1%.
[0040] 0.10 g of the rGO-supported manganese oxide catalyst for removing formaldehyde at room temperature prepared in Example 1 was weighed and placed in a quartz tube fixed bed reactor with an inner diameter of 8 mm; the reaction atmosphere was 0.55 mg / m3 Formaldehyde gas and 100% high-purity air, the reaction gas flow rate is 100mL / min; at a temperature of 30°C and a humidity of 50%, the reaction was continued for 5 times (each reaction was 20min, which is the tail gas absorption time, the same below); the formaldehyde residue in the tail gas was determined by phenol reagent spectrophotometry, and the decomposition rate curve of the catalyst removing formaldehyde in the air was obtained. The results are shown in Figure 1 and Table 1.
[0041] The results show that the rGO-loaded manganese oxide catalyst for room temperature formaldehyde removal prepared in Example 1, with 60 wt % of the catalyst, still achieved a formaldehyde elimination rate of more than 99%, and had good formaldehyde elimination performance.
[0042] Table 1 Comparison of formaldehyde decomposition rates of Example 1 and Comparative Examples 1-3, unit: %
[0043] cycle Example 1 Comparative Example 1 Comparative Example 2 Comparative Example 3 1 99.8 44.2 99.1 37.3 2 99.7 41.4 98.4 34.6 3 99.5 37.7 99.0 34.4 4 99.7 35.6 99.1 33.5 5 99.4 34.1 98.5 32.8
[0044] Comparative Example 1
[0045] 0.10 g of commercially available MnO2 sample was weighed and placed in a quartz tube fixed bed reactor with an inner diameter of 8 mm; the reaction was continued for five times under the same conditions as in Example 1. The formaldehyde residue in the tail gas was determined by phenol reagent spectrophotometry to obtain a curve of the catalyst removing formaldehyde from the air. The results are shown in Figure 1 and Table 1.
[0046] Comparative Example 2
[0047] 0.10 g of the catalyst of Example 3 of CN118237010A was weighed and placed in a quartz tube fixed bed reactor with an inner diameter of 8 mm; the reaction was continued for five times under the same conditions as in Example 1. The formaldehyde residue in the tail gas was determined by phenol reagent spectrophotometry to obtain a curve of the catalyst removing formaldehyde from the air. The results are shown in Figure 1 and Table 1.
[0048] Comparative Example 3
[0049] Comparative Example 3 is a comparative example of Example 1. The difference is that in step S2, 1.26 g of MnCl2 is added to the graphene oxide solution to obtain a uniform mixed solution of MnCl2 and graphene oxide; in step S5, the reactants are placed in an atmosphere furnace and calcined at 600°C for 4 hours under the protection of H2 gas. The reaction is continued for five times under the same conditions as in Example 1. The results show that the formaldehyde elimination efficiency of the composite catalyst is maintained at about 30%, which is much lower than that of the sample calcined at 200°C to 500°C, indicating that hydrogen reduction at different temperatures has an important influence on the catalytic performance of the composite catalyst.
[0050] Example 2: High air velocity, low concentration formaldehyde elimination test
[0051] A method for preparing an rGO-supported manganese oxide catalyst for removing formaldehyde at room temperature comprises the following steps:
[0052] S1. Disperse 2 g of graphene oxide in 150 mL of water and stir for 1 h to make it uniform to obtain a graphene oxide solution;
[0053] S2, adding 1.26 g (0.01 mol) of MnCl2 into the graphene oxide solution, stirring to obtain a uniform mixed solution of MnCl2 and graphene oxide;
[0054] S3, adding Na2CO3 solution dropwise to the mixed solution, adjusting the pH value of the solution to 9.5, stirring for precipitation reaction until no more precipitate is generated;
[0055] S4, filtering and washing the reaction product, and drying it by air blast at 200° C. to obtain graphene oxide loaded with a Mn precursor (Mn(OH)4);
[0056] S5. Grind and break up the graphene oxide loaded with the Mn precursor, place it in an atmosphere furnace, and calcine it at 350°C for 4 hours at a hydrogen flow rate of 30 mL / min to reduce the graphene oxide once; a 30 wt% rGO-loaded manganese oxide catalyst for room temperature formaldehyde removal can be obtained, and the yield is 70.7%.
[0057] 0.10 g of the rGO-supported manganese oxide catalyst for removing formaldehyde at room temperature prepared in Example 2 was weighed and placed in a quartz tube fixed bed reactor with an inner diameter of 8 mm; the reaction atmosphere was 0.28 mg / m 3 Formaldehyde gas and 100% high-purity air, the reaction gas flow rate is 500mL / min; the humidity inside the reactor is changed by bubbling method, and the decomposition efficiency is tested at a temperature of 30°C and a humidity of 70%RH, and the reaction is repeated 5 times; the formaldehyde residue in the tail gas is determined by phenol reagent spectrophotometry, and the decomposition rate curve of the catalyst eliminating formaldehyde in the air is obtained. The results are shown in Figure 2 and Table 2.
[0058] The results show that under high humidity conditions of 70% RH, the rGO-loaded manganese oxide catalyst for room temperature formaldehyde removal prepared in Example 2 still achieved a formaldehyde elimination rate of more than 95%.
[0059] Comparative Example 4
[0060] Comparative Example 4 is a comparative example of Example 2, except that the precipitated product was calcined at 350°C for 4h in the atmosphere to obtain a 30wt% MnO2 / GO composite catalyst. 0.10g of the MnO2 / GO composite catalyst was placed in a quartz tube fixed bed reactor with an inner diameter of 8mm, and the reaction was repeated five times under the same conditions as in Example 2. The formaldehyde residue in the tail gas was determined by phenol reagent spectrophotometry to obtain a catalyst decomposition rate curve for formaldehyde removal in the air. The results are shown in Table 2. Figure 2 and Table 2.
[0061] Table 2 Comparison of formaldehyde decomposition rates of Example 2 and Comparative Examples 2, 4-5, unit: %
[0062] cycle Example 2 Comparative Example 4 Comparative Example 5 Comparative Example 2 1 99.8 64.2 92.1 65.5 2 98.7 56.4 90.9 62.4 3 97.4 47.3 89.8 61.3 4 98.1 45.5 90.2 60.5 5 96.3 43.4 90.1 60.4
[0063] Comparative Example 5
[0064] Comparative Example 5 is the catalyst (60wt% MnOx / AC) of Example 2 of CN118237010A; 0.10g of the catalyst was weighed and placed in a quartz tube fixed bed reactor with an inner diameter of 8mm, and the reaction was continued for five times under the same conditions as Example 2. The formaldehyde residue in the tail gas was measured by phenol reagent spectrophotometry to obtain the decomposition rate curve of the catalyst for removing formaldehyde from the air. The results are shown in Figure 2 and Table 2.
[0065] Comparative Example 2 is the catalyst 60wt% MnOx / GO of Example 3 of CN118237010A); 0.10g of the catalyst of Comparative Example 2 was also weighed and placed in a quartz tube fixed bed reactor with an inner diameter of 8mm, and the reaction was continued for five times under the same conditions as Example 2. The formaldehyde residue in the tail gas was measured by phenol reagent spectrophotometry to obtain the catalyst decomposition rate curve of formaldehyde in the air. The results are shown in Figure 2 and Table 2.
[0066] As can be seen from Table 2, the manganese element after one-time reduction with hydrogen is no longer a simple +4 valence, but a mixture of manganese oxides with multiple valences, which has a synergistic effect with rGO, so that the rGO-loaded manganese oxide catalyst of the present invention has a better formaldehyde removal activity.
[0067] Example 3: Test on the effect of changing reduction conditions on formaldehyde elimination performance
[0068] A method for preparing an rGO-supported manganese oxide catalyst for removing formaldehyde at room temperature comprises the following steps:
[0069] S1. Disperse 0.6 g of graphene oxide (GO) in 150 mL of water and stir for 1 h to make it uniform to obtain a graphene oxide solution;
[0070] S2, adding 1.26 g (0.007 mol) of Mn(NO3)2 to the graphene oxide solution, stirring to obtain a uniform mixed solution of Mn(NO3)2 and graphene oxide;
[0071] S3, adding NaOH solution dropwise to the mixed solution, adjusting the pH value of the solution to 9.5, stirring for precipitation reaction until no more precipitate is generated;
[0072] S4, filtering and washing the reaction product, and drying it by air blast at 200° C. to obtain graphene oxide loaded with a Mn precursor (Mn(OH)4);
[0073] S5. Grind and break up the graphene oxide loaded with Mn precursor, and finally calcine the reactant under hydrogen protection (hydrogen flow rate is 30 mL / min) for 4 h to reduce the graphene oxide once; the calcination temperatures are 250°C, 350°C, and 450°C, respectively, to obtain three 60wt% rGO-loaded manganese oxide catalysts for room temperature formaldehyde removal, with yields of 66.3%, 63.1%, and 62.4%, respectively.
[0074] 0.10 g of the three room temperature formaldehyde removal rGO-supported manganese oxide catalysts prepared in Example 3 were respectively placed in a quartz tube fixed bed reactor with an inner diameter of 8 mm; the reaction atmosphere was 0.28 mg / m 3 Formaldehyde gas and 100% high-purity air, the reaction gas flow rate is 500 mL / min; under the high humidity conditions of temperature 30℃ and humidity 70%RH, the reaction is carried out continuously for 5 times; the formaldehyde residue in the tail gas is determined by phenol reagent spectrophotometry, and the decomposition rate curve of the catalyst eliminating formaldehyde in the air is obtained. The results are shown in Figure 3 and Table 3.
[0075] 0.10 g of the commercially available MnO2 sample of Comparative Example 1 was weighed and placed in a quartz tube fixed bed reactor with an inner diameter of 8 mm; the reaction was continued for five times under the same conditions as in Example 3. The formaldehyde residue in the tail gas was determined by phenol reagent spectrophotometry to obtain a curve of the catalyst removing formaldehyde from the air. The results are shown in Figure 3 and Table 3.
[0076] Table 3 Comparison of formaldehyde decomposition rates between Example 3 and Comparative Example 1, unit: %
[0077] cycle Example 3 (250°C) Example 3 (350°C) Example 3 (450°C) Comparative Example 1 1 97.8 99.1 75.4 24.9 2 98.0 99.5 74.9 23.2 3 97.5 99.6 75.1 19.2 4 96.2 99.3 74.8 21.1 5 97.1 99.4 75.0 17.8
[0078] From the results in Table 3, we can see that the formaldehyde removal efficiency of the rGO-supported manganese oxide catalyst calcined at 350°C for room temperature formaldehyde removal is still maintained at more than 99% at high space velocity and low concentration. However, the catalytic performance of commercially available MnO2 at high space velocity and low concentration further decreases.
[0079] The present invention adopts a coprecipitation reaction and subsequent calcination in an atmosphere furnace, the raw materials are cheap, the preparation method is simple, and it is suitable for large-scale, industrial applications. The present invention reduces once during calcination so that it has more oxygen vacancies, increases catalytic activity, and thus improves its catalytic activity, and is compounded with graphene oxide to reduce the agglomeration of manganese-based oxides, which enables it to have good low-temperature redox ability and significantly improves catalytic durability. It can be seen from Examples 1-3 that the catalyst of the present invention has good catalytic properties and moisture resistance, and multiple cycle tests also show that the catalyst has high activity and good stability.
Claims
1. A rGO-supported manganese oxide catalyst for removing formaldehyde at room temperature, characterized in that: A Mn precursor is loaded on graphene oxide, and then calcined and reduced once in a hydrogen atmosphere at 200-500° C. to form an rGO-loaded manganese oxide catalyst; the mass fraction of manganese oxide in the catalyst is 10%-70%; the graphene oxide becomes reduced graphene oxide rGO after being reduced by hydrogen; the Mn precursor is formed by a precipitation reaction between a manganese source compound and an alkaline solution; the manganese source compound is at least one of manganese sulfate, manganese acetate, manganese nitrate, manganese chloride or manganese oxalate; the alkaline solution is at least one of a potassium hydroxide solution, a sodium hydroxide solution, a potassium carbonate solution, a potassium bicarbonate solution, a sodium carbonate solution or a sodium bicarbonate solution with a mass concentration of 1%-15%.
2. The rGO-supported manganese oxide catalyst for removing formaldehyde at room temperature according to claim 1, characterized in that: The mass fraction of the manganese oxide in the catalyst is 20% to 60%.
3. The rGO-supported manganese oxide catalyst for removing formaldehyde at room temperature according to claim 1, characterized in that: The graphene oxide is multi-layer graphene oxide with 2 to 5 layers and a specific surface area of ≥100m 2 / g.
4. A method for preparing the rGO-supported manganese oxide catalyst for removing formaldehyde at room temperature according to any one of claims 1 to 3, characterized in that: The steps include: S1, dispersing the graphene oxide in water, stirring to make it uniform, to obtain a graphene oxide solution; S2, adding a manganese source compound to the graphene oxide solution, and stirring to obtain a mixed solution; S3, adding an alkaline solution dropwise to the mixed solution, adjusting the pH value of the solution to 9-12, and stirring to perform a precipitation reaction; S4, filtering, washing, and drying the reaction product to obtain graphene oxide loaded with a Mn precursor; S5. Grind the graphene oxide loaded with the Mn precursor, place it in an atmosphere furnace and calcine it at 200-500° C., and introduce hydrogen as a protective gas and a reaction raw material to reduce the graphene oxide once; thus, the rGO-loaded manganese oxide catalyst for removing formaldehyde at room temperature can be obtained.
5. The preparation method according to claim 4, characterized in that: The mass concentration of the manganese source compound in the mixed solution is 0.5% to 2%, and the precipitation reaction time is 1 to 5 hours.
6. The preparation method according to claim 4, characterized in that: The drying temperature of step S4 is 20-100° C., and the drying time is 1-6 hours.