A catalyst and its preparation method and application
By using metal active components and modified molecular sieve catalysts, the problem of low efficiency in the co-catalytic cracking of biomass pyrolysis oil and atmospheric pressure residual oil is solved, the hydrogen transfer deoxygenation capacity and the utilization rate of biological carbon atoms are improved, and the coke is reduced Generation, achieving efficient bio-oil modification.
Patent Information
- Application Number
- CN202411035482.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-07-31
AI Technical Summary
The polymerization and coke generation in the co-catalytic cracking of biomass pyrolysis oil and atmospheric pressure residue oil leads to the problem of low efficiency, low utilization rate of biological carbon atoms and large amount of coke generation.
A catalyst is used, including metal active components (CeO2, ZrO2, Nb2O3, La2O3) and H-type Y molecular sieve. The modified molecular sieve is used to regulate the hydrogen transfer and hydrogen supply capacity and inhibit the formation of coke. It is used for biomass pyrolysis oil and petroleum fractions. of co-catalytic cracking.
It effectively improves the hydrogen transfer deoxygenation ability of bio-oil, reduces the coke yield, and improves the utilization rate of bio-carbon atoms. The deoxygenation rate reaches about 90 wt%, and the coke yield is as low as 3.91 wt%.
Smart Images

Figure CN118558357B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of petroleum processing, and in particular relates to a catalyst and a preparation method and application thereof. Background Art
[0002] As the only renewable carbon-containing resource, biomass can be converted into high-value chemicals and fuels through catalytic cracking, which can not only recycle agricultural and forestry wastes, but also reduce dependence on non-renewable energy. The production of bio-oil fuel by pyrolysis of biomass is an important method to maximize the utilization of biomass, but due to the high oxygen content, low calorific value, and poor chemical and thermal stability of bio-oil obtained by pyrolysis, it cannot be used directly as fuel.
[0003] Therefore, before using it as fuel, the bio-oil is first upgraded. Based on the problems of large coke production, high oxygen content and low carbon atom utilization rate in traditional biomass pyrolysis oil catalytic cracking, H / C eff Higher solvents can be used as hydrogen donors for catalytic cracking of bio-oil to further improve its quality. Even though the reaction conditions of co-catalytic cracking are milder than those of hydrogenation technology, the method is simple and economical. However, current research is limited to the use of an equilibrator (E-CAT) to blend bio-oil with petroleum fractions for co-catalytic cracking. In addition, bio-oil is easily polymerized during the reaction, resulting in low utilization of bio-carbon atoms and large amounts of coke. The technical problem of low co-catalytic cracking efficiency of biomass pyrolysis oil and atmospheric residue has not been overcome.
[0004] Therefore, how to prepare a catalyst that can regulate the hydrogen transfer and hydrogen supply capacity of hydrocarbon molecules, enhance the CO bond activation ability and inhibit coke formation is a problem that needs to be solved urgently. Summary of the invention
[0005] One of the purposes of the present invention is to provide a catalyst for co-catalytic cracking of biomass pyrolysis oil and petroleum fractions and a preparation method thereof, so as to effectively solve the problem of low efficiency caused by polymerization and coking in the existing co-catalytic cracking of biomass pyrolysis oil and atmospheric residue; another purpose is to provide the use of the above catalyst in the process of co-refining of bio-oil model compounds and / or their model compounds guaiacol, etc. with petroleum hydrocarbon components and / or VGO to inhibit the polymerization of bio-oil and improve the hydrogen transfer deoxygenation ability.
[0006] The technical solution adopted is as follows.
[0007] A catalyst comprising a metal active component, a molecular sieve and / or H 3 PO 4 , the metal active component is CeO 2 、ZrO 2 , Nb 2 O 3 ,La2 O 3 One or more of the above, wherein the molecular sieve is an H-type Y molecular sieve with a silicon-aluminum mass ratio of 1.4 to 10:1 and a sodium oxide mass fraction of 0.8 to 1%; using metal active components and / or H 3 PO 4 The modified molecular sieve is used as a catalyst for the co-catalytic cracking of biomass pyrolysis oil and petroleum fractions.
[0008] A method for preparing a catalyst comprises the following steps:
[0009] (1) Add molecular sieve into deionized water and stir to obtain a uniform slurry;
[0010] (2) adding a metal salt to the uniform slurry prepared in step (1), stirring the slurry to obtain a catalyst precursor, wherein the metal salt is one or more of a soluble cerium salt, a soluble lanthanum salt, a soluble zirconium salt, and a soluble niobium salt;
[0011] (3) calcining the catalyst precursor obtained in step (2) to obtain a first modified molecular sieve;
[0012] Alternatively, the catalyst precursor obtained in step (2) is calcined and H 3 PO 4 The solution is subjected to standing, impregnation, aging, drying and calcination to obtain a second modified molecular sieve;
[0013] (4) The first modified molecular sieve or the second modified molecular sieve is subjected to hydrothermal treatment to obtain a first catalyst or a second catalyst.
[0014] Preferably, the soluble cerium salt is Ce(NO 3 ) 4 6H 2 O, soluble lanthanum salts are La(NO 3 ) 3 6H 2 O, soluble zirconium salt is Zr(NO 3 ) 4 ·5H 2 O, soluble niobium salt is C 2 H 2 NbO 4 .
[0015] Preferably, the metal oxide accounts for 5-50% of the mass of the prepared first catalyst or the second catalyst; and the phosphorus element accounts for 0.5-5% of the mass of the prepared second catalyst.
[0016] Preferably, in step (2), the stirring aging time is 6 to 12 hours, the drying temperature is 90 to 150° C., and the drying time is 2 to 12 hours.
[0017] Preferably, in step (3), the calcination temperature is 500-700° C., and the calcination time is 4-12 hours.
[0018] Preferably, in step (3), H 3 PO 4 The concentration of the solution is 0.3~1 mol / L, the dropping rate is 1 drop per second, and the immersion time is 6~12 h.
[0019] Preferably, in step (4), the hydrothermal treatment is a steam treatment at 600-800° C. for 4-17 h.
[0020] The catalyst provided or prepared by the present invention is used to inhibit bio-oil polymerization and improve hydrogen transfer deoxygenation ability during the co-refining process of biomass pyrolysis oil and / or its model compound with petroleum fractions and / or VGO.
[0021] Preferably, the reaction temperature is 450-550°C;
[0022] The mass space velocity of the reaction raw materials is 5~60 h -1 ;
[0023] The reaction raw materials are 5-20 wt% guaiacol and tetralin.
[0024] Reaction mechanism: The molecular sieve hydrogen transfer and hydrogen supply position are regulated while suppressing the polymerization and coking of bio-oil. First, the molecular sieve supplies part of the hydrogen to -OH, so that the oxygen in the bio-oil is converted to H 2 O, and the other part supplies hydrogen to olefins formed by self-cracking, thereby generating alkanes. The hydrogen transfer capacity of the molecular sieve is regulated by metal modification to produce appropriate hydrogen supply, and hydrogen is supplied to oxygen in bio-oil as much as possible; secondly, the acid properties of the molecular sieve are controlled, and the acid amount and B / L acid ratio of the molecular sieve are regulated by less metal and acid modification to weaken the ability to generate coke and bio-oil polymerization, thereby also improving the utilization rate of bio-carbon atoms. Based on this, the present invention introduces rare earth metal components on the one hand to improve the hydrothermal stability of the active components of the molecular sieve to ensure that the reaction can continue; on the other hand, the metal components are introduced into the zeolite molecular sieve, which can regulate the hydrogen transfer capacity to supply hydrogen to oxygen contained in the bio-oil, and at the same time inhibit the polymerization reaction of the bio-oil.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] The catalyst provided by the present invention provides a part of hydrogen to -OH by molecular sieve, so that the oxygen in the bio-oil is converted into H 2O, and the other part is used to supply hydrogen to olefins formed by self cracking, and then to generate alkanes. The hydrogen transfer ability of the molecular sieve is regulated by metal modification to produce appropriate hydrogen supply, so as to supply hydrogen to the oxygen in the bio-oil as much as possible. On the other hand, the acid properties of the molecular sieve are controlled. The acid amount and B / L acid ratio of the molecular sieve are regulated by some metal modifications to weaken the ability to generate coke and polymerize bio-oil, which can also improve the utilization rate of biological carbon atoms.
[0027] The preparation method of the invention is simple and the conditions are easy to implement. The prepared catalyst is applied to the co-catalytic cracking process of guaiacol and tetralin, the deoxygenation rate reaches about 90 wt%, and the coke yield is as low as 3.91 wt%. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a comparison chart of the deoxygenation rate and coke yield of the catalyst prepared in Test Example 1 of the present invention in the co-catalytic cracking process of guaiacol and tetralin. DETAILED DESCRIPTION
[0029] The accompanying drawings are only used for illustrative purposes. The present invention will be described in detail below in conjunction with the embodiments and the accompanying drawings.
[0030] Unless otherwise specified, the raw materials, chemical reagents, etc. used in the present invention can be obtained through regular commercial channels, and the standards of the chemical reagents are the usual standards used in laboratories.
[0031] The HY molecular sieve used was produced by Tianjin Nanhua Catalyst Factory, in which SiO 2 / Al 2 O 3 =5.4, calcined at 550℃ for 6 hours before use to remove impurities.
[0032] The metal salts are all nitrates.
[0033] Phosphoric acid is a product of Xilong.
[0034] Embodiment 1, a method for preparing a catalyst, comprising the following steps:
[0035] Take 4 g of HY molecular sieve and add it into 20 ml of deionized water, stir evenly to make a slurry. Then, take 2.52 g of Ce(NO 3 ) 4 •6H 2 O was added to the slurry, stirred for 12 h, and then dried at 90° C. for 12 h. Subsequently, it was calcined at 550° C. for 6 h to obtain a modified molecular sieve.
[0036] The modified molecular sieve was treated with steam at 700°C for 4 h to obtain catalyst CAT-1. The metal oxide component composite content of the obtained catalyst was about 20 wt%.
[0037] Test Example 1: Different CeO 2 Testing of the composite amount of components.
[0038] According to the preparation method of Example 1, different composite amounts of CeO 2 -HY catalyst, CeO 2 The composite amounts of the components are 0 wt%, 5 wt%, 10 wt%, 15 wt%, 25 wt%, 30 wt%, 40 wt%, and 50 wt%, respectively; 0 wt% means only molecular sieve HY. 2 The catalyst with the composite amount of components and the catalyst prepared in Example 1 were respectively applied in the co-catalytic cracking process of guaiacol and tetralin. The comparison diagram of the deoxidation rate and the coke yield obtained is shown in Figure 1 As shown. Figure 1 It can be seen that when the compounding amount is 30 wt%, the coke yield is reduced to 4.75 wt%, and the deoxidation rate reaches a maximum of 91 wt%. This shows that the introduction of Ce can reduce B acid and introduce more L acid, which inhibits the polymerization reaction of oxygen-containing compounds. However, on the one hand, the excessive compounding amount of metal oxides leads to a decrease in the relative crystallinity of the molecular sieve, and on the other hand, the coke yield does not meet the production requirements, and the acid properties of the molecular sieve need to be further regulated to reduce the coke yield.
[0039] Example 2: The method of Example 1 was followed, except that 2.66 g La(NO 3 ) 3 •6H 2 O replaces 2.52 g Ce(NO 3 ) 4 •6H 2 O, to obtain catalyst CAT-2. The composite amount of the metal oxide component of the obtained catalyst is about 20 wt%.
[0040] Example 3: The method of Example 1 was followed except that 1.87 g Zr (NO 3 ) 4 •5H 2 O replaces 2.52 g Ce(NO 3 ) 4 •6H 2 O, to obtain catalyst CAT-3. The composite amount of the metal oxide component of the obtained catalyst is about 20 wt%.
[0041] Example 4: The method of Example 1 is followed, except that 4.05 g C 2 H 2 NbO 4Instead of 2.52 g Ce(NO 3 ) 4 •6H 2 O, to obtain catalyst CAT-4. The composite amount of the metal oxide component of the obtained catalyst is about 20wt%.
[0042] Example 5: 3.8 g of HY molecular sieve was added into 20 ml of deionized water and stirred to obtain a slurry. Then, 0.50 g of Ce(NO 3 ) 4 •6H 2 O was added to the slurry, stirred for 12 h, and then dried at 90° C. for 12 h. Subsequently, it was calcined at 550° C. for 6 h to obtain a modified molecular sieve.
[0043] Take 0.06 g H 3 PO 4 (85%) was prepared into a 0.15 mol / L concentration solution, which was dripped onto 3 g of modified molecular sieve at room temperature. After impregnation, it was aged for 12 hours, dried at 90°C for 12 hours, and then calcined at 550°C for 6 hours to obtain a secondary modified molecular sieve.
[0044] The secondary modified molecular sieve was treated with steam at 700°C for 4 h to obtain catalyst CAT-5. The metal oxide CeO 2 The composite amount is about 5 wt%, and the P loading is 0.5 wt%.
[0045] Example 6: The method of Example 5 was followed, except that 0.11 g H 3 PO 4 (85%) replaced 0.06 g H 3 PO 4 (85%), and the catalyst CAT-6 was obtained. The metal oxide CeO 2 The composite amount is about 5 wt%, and the loading amount of the second component P is 1 wt%.
[0046] Example 7: The method of Example 5 was followed, except that 0.22 g H 3 PO 4 (85%) replaced 0.06 g H 3 PO 4 (85%), and the catalyst CAT-7 was obtained. The metal oxide CeO 2 The composite amount is about 5 wt%, and the loading amount of the second component P is 2 wt%.
[0047] Example 8: The method of Example 5 was followed, except that 0.33 g H3 PO 4 (85%) replaced 0.06 g H 3 PO 4 (85%), and the catalyst CAT-8 was obtained. The metal oxide CeO 2 The composite amount is about 5 wt%, and the loading amount of the second component P is 3 wt%.
[0048] Example 9: The method of Example 5 was followed, except that 0.45 g H 3 PO 4 (85%) replaced 0.06 g H 3 PO 4 (85%), and the catalyst CAT-9 was obtained. The metal oxide CeO 2 The composite amount is about 5 wt%, and the loading amount of the second component P is 4 wt%.
[0049] Comparative Example 1: 4 g of HY molecular sieve was calcined at 550°C for 6 h, and then treated with steam at 700°C for 4 h to obtain catalyst CAT-D1.
[0050] Comparative Example 2: 3.8 g of HY molecular sieve was added into 20 ml of deionized water and stirred to obtain a slurry. 3 ) 4 •6H 2 O was added to the slurry, stirred for 12 h, and then dried at 90° C. for 12 h. Subsequently, it was calcined at 550° C. for 6 h to obtain a modified molecular sieve.
[0051] The modified molecular sieve was treated with steam at 700 °C for 4 h to obtain catalyst CAT-D2, metal oxide CeO 2 The composite amount is about 5 wt%, and the P loading is 0 wt%.
[0052] In this experiment, the catalysts prepared in Examples 1-9 were applied to the co-catalytic cracking process of guaiacol and tetralin, comprising the following steps: using a fixed bed microreactor, 2 g of the catalyst was loaded into a reaction tube, the reactor was then sealed, the temperature was raised to a reaction temperature of 480°C, and N 2 The air in the reaction tube and the impurities adsorbed on the catalyst were replaced; after 2 hours, a mixed reaction solution of guaiacol and tetralin was introduced into the reaction tube for reaction at a mass space velocity of 30 h -1 , the catalyst-oil ratio is 1:1, the reaction pressure is 0.1 MPa, and finally the gas phase and liquid phase products are collected respectively. The mass percentage of the product yield includes the coke yield, the total material balance, the O balance, and the deoxidation rate. The product yields of each embodiment and comparative example are calculated as follows:
[0053] CAT-1, coke yield 4.86 wt%, total material balance 94 wt%, O balance 95 wt%, deoxidation rate 88.1 wt%;
[0054] CAT-2, coke yield 5.72 wt%, total material balance 94 wt%, O balance 96 wt%, deoxidation rate 80.3 wt%;
[0055] CAT-3, coke yield 3.78 wt%, total material balance 96 wt%, O balance 89 wt%, deoxidation rate 69.0 wt%;
[0056] CAT-4, coke yield 2.45 wt%, total material balance 97 wt%, O balance 90 wt%, deoxidation rate 66.5 wt%;
[0057] CAT-5, coke yield 7.75 wt%, total material balance 91 wt%, O balance 98 wt%, deoxidation rate 70.6 wt%;
[0058] CAT-6, coke yield 5.83 wt%, total material balance 93 wt%, O balance 97 wt%, deoxidation rate 78.3 wt%;
[0059] CAT-7, coke yield 3.91 wt%, total material balance 95 wt%, O balance 99 wt%, deoxidation rate 90.2 wt%;
[0060] CAT-8, coke yield 1.82 wt%, total material balance 92 wt%, O balance 96 wt%, deoxidation rate 67.8 wt%;
[0061] CAT-9, coke yield 0.68 wt%, total material balance 96 wt%, O balance 92 wt%, deoxidation rate 57.2 wt%;
[0062] CAT-D1, coke yield 7.14 wt%, total material balance 94 wt%, O balance 77 wt%, deoxidation rate 53.1 wt%;
[0063] CAT-D2, coke yield 7.56 wt%, total material balance 93 wt%, O balance 96 wt%, deoxidation rate 75.2wt%.
[0064] It can be seen that among Examples 1-4, the catalyst CAT-1 of Example 1 has the best catalytic effect, the highest deoxidation rate and the lowest coke yield. The catalytic effect of the unmodified catalyst CAT-D1 of Comparative Example 1 is worse than that of the catalysts CAT-1 to CAT-4 of Examples 1-4, and the deoxidation effect of the catalysts of Examples 1-4 is CAT-1>CAT-2>CAT-3>CAT-4. In Examples 1-4, only the type of metal oxide is changed, which shows that in the preparation of the catalyst, the metal oxide component is preferably CeO 2 . Adding metal oxide Nb 2 O 3 Although the deoxygenation rate is not high, the coke yield is the lowest. The deoxygenation rate can be further increased through the hydrogenation process.
[0065] In Examples 5-9, the catalyst of Example 7 has the best effect, the highest deoxygenation rate and a lower coke yield than that of Comparative Example 2. In Examples 5-9, only the loading amount of P is changed, which indicates that in the catalyst preparation, the loading amount of P is preferably 2 wt%.
[0066] Compared with the examples, the catalyst CAT-D1 of comparative example 1 is only an unmodified molecular sieve, and no metal components are added during the preparation process. The catalyst CAT-D2 of comparative example 2 is only a metal oxide CeO 2 Compounded with molecular sieve, without adding the second component P. Adding too much metal oxide will cover the molecular sieve, which will reduce the activity of the molecular sieve in the long run. After adding P element, when the P loading is 2 wt%, the deoxidation rate is the highest and the coke yield is low. This shows that while reducing the metal oxide content, a certain amount of acid in the molecular sieve can be maintained, and the appropriate ratio of B / L acid can be reduced, so that the molecular sieve can exert its hydrogen transfer ability and inhibit the polymerization reaction of oxygen-containing compounds. The low coke yield can increase the carbon atom utilization rate of oxygen-containing compounds.
[0067] This indicates that the catalyst provided by the present invention can effectively improve the deoxygenation rate of guaiacol and inhibit the formation of carbon deposits when applied to the co-catalytic cracking process of guaiacol and tetralin.
[0068] Of course, the above description is not a limitation of the present invention, and the present invention is not limited to the above examples. Changes, modifications, additions or substitutions made by technicians in this technical field within the essential scope of the present invention should also fall within the protection scope of the present invention.
Claims
1. A method for preparing a catalyst, characterized in that: The catalyst comprises a metal active component, a molecular sieve, and an H3PO4 solution, wherein the metal active component is one or more of CeO2, ZrO2, Nb2O3, and La2O3, and the molecular sieve is an H-type Y molecular sieve with a silicon-aluminum mass ratio of 1.4 to 10:1 and a sodium oxide mass fraction of 0.8%; the molecular sieve is modified by using the metal active component or the metal active component and H3PO4 as a catalyst for co-catalytic cracking of biomass pyrolysis oil and petroleum fractions; The preparation method of the catalyst comprises the following steps: (1) Add molecular sieve into deionized water and stir to obtain a uniform slurry; (2) adding a metal salt to the uniform slurry prepared in step (1), stirring the slurry to be uniform, stirring, aging, and drying the slurry, wherein the stirring, aging, and drying time is 6 to 12 hours, the drying temperature is 90 to 150° C., and the drying time is 2 to 12 hours to obtain a catalyst precursor; the metal salt is one or more of a soluble cerium salt, a soluble lanthanum salt, a soluble zirconium salt, and a soluble niobium salt; (3) calcining the catalyst precursor obtained in step (2) to obtain a first modified molecular sieve; Alternatively, after calcining the catalyst precursor obtained in step (2), H3PO4 solution is added dropwise thereto, wherein the concentration of the H3PO4 solution is 0.6 mol / L, the rate of addition is 1 drop per second, and the impregnation time is 6 to 12 hours. After standing, impregnating, aging, drying, and calcining, a second modified molecular sieve is obtained; (4) The first modified molecular sieve or the second modified molecular sieve is subjected to hydrothermal treatment to obtain a first catalyst or a second catalyst; wherein the hydrothermal treatment is a steam treatment at 600-800° C. for 4-17 hours; The metal oxide accounts for 5 to 50% of the mass of the prepared first catalyst or the second catalyst; the phosphorus element accounts for 0.5 to 5% of the mass of the prepared second catalyst.
2. The method for preparing a catalyst according to claim 1, characterized in that: The soluble cerium salt is Ce(NO3)4·6H2O, the soluble lanthanum salt is La(NO3)3·6H2O, the soluble zirconium salt is Zr(NO3)4·5H2O, and the soluble niobium salt is C2H2NbO4.
3. The method for preparing a catalyst according to claim 1, characterized in that: In the step (3), the calcination temperature is 500-700° C. and the calcination time is 4-12 hours.
4. Use of the catalyst prepared by the method according to any one of claims 1 to 3 to inhibit bio-oil polymerization and improve hydrogen transfer deoxygenation ability in the process of co-refining biomass pyrolysis oil and / or its model compound with petroleum fractions and / or VGO, characterized in that: The reaction temperature is 450~550℃; The mass space velocity of the reaction raw materials is 5~60h -1 ; The reaction raw materials are 5-20wt% guaiacol and tetralin.