Ceramic substrate green body coating slurry and preparation method and application thereof
By coating the green coating slurry of ceramic substrate prepared by specific components and processes on the ceramic substrate, the problems of concave and convexity and wrinkles on the ceramic surface after sintering are solved, and the flatness and high pass rate of the ceramic substrate surface are achieved.
Patent Information
- Application Number
- CN202411047376.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-08-01
AI Technical Summary
The existing slurry is coated on the green ceramic substrate by screen printing, and the surface of the sintered ceramic still has concave and convexity and wrinkles, affecting the surface flatness and pass rate.
A ceramic substrate green coating slurry, including boron nitride, hydrogenated castor oil, ethyl cellulose, PVB and triethanolamine, is prepared by specific mixing and ball milling to form a uniform slurry , and coated on the ceramic substrate by screen printing process to ensure uniform distribution and tight fit of the surface.
The flatness and high pass rate of the surface of the ceramic substrate are achieved, the concave and convexity and wrinkles are avoided after sintering, and the surface quality of the ceramic substrate is improved.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the field of ceramics, and in particular to a ceramic substrate green body coating slurry, a preparation method and an application thereof. Background Art
[0002] In recent years, semiconductor devices have developed rapidly in the direction of high power, high frequency and integration. The heat generated by semiconductor devices is the key factor causing the failure of semiconductor devices, and the thermal conductivity of the insulating substrate is the key to affecting the heat dissipation of the overall semiconductor devices. In addition, in the fields of electric vehicles and high-speed railways, semiconductor devices often face complex mechanical environments such as bumps and vibrations during use, which puts strict requirements on the mechanical reliability of the materials used. The excellent mechanical properties of ceramic materials make them stand out.
[0003] Among them, silicon nitride ceramics are the structural ceramic materials with the best comprehensive performance. The theoretical thermal conductivity of ceramics is very high, and it has the potential to become a high thermal conductivity substrate. Excellent mechanical properties and good high thermal conductivity potential make silicon nitride ceramics have great market prospects in the application of high-end semiconductor devices, especially high-power semiconductor device substrates.
[0004] At present, tape casting is a molding method for preparing high-quality ceramic substrates. The tape casting method has high production efficiency, easy production continuity and automation, and is more suitable for industrial large-scale production. The tape casting process is to coat the slurry on the ceramic to form a film with a smooth surface and uniform thickness, and then dry it to make a green sheet with good toughness.
[0005] The ceramic substrate green body prepared by tape casting process needs to be coated with a layer of isolation powder, and then debinding and sintering are carried out. The coating effect of isolation powder is closely related to the surface state of the substrate blank. If the powder is not evenly coated, the substrate surface will be uneven and warping and other defects will occur; if the powder is not dispersed well and agglomerated particles appear, pits and other defects will appear on the surface of the substrate after sintering.
[0006] Screen printing technology has the advantages of large batches, low prices, high efficiency, and good printing quality, and is widely used in circuit boards, textiles, ceramics, packaging, etc. However, the existing slurry is coated on the green ceramic substrate by screen printing, and the sintered ceramic surface still has bumps and wrinkles. Summary of the invention
[0007] Therefore, the technical problem to be solved by the present invention is to overcome the problem that the existing slurry is coated on the ceramic substrate green body by screen printing, and the ceramic surface obtained by sintering still has bumps and wrinkles, thereby providing a ceramic substrate green body coating slurry and a preparation method and application thereof.
[0008] The first aspect of the present invention protects a ceramic substrate green body coating slurry, which includes the following components in percentage by weight based on the mass of the slurry: 10-55wt% boron nitride, 0-5wt% hydrogenated castor oil, 0-0.28wt% ethyl cellulose, 0.001-1.1wt% PVB, 2-25wt% triethanolamine, and 30-60wt% solvent.
[0009] In the present invention, the PVB is polyvinyl butyral.
[0010] Furthermore, based on the mass of the slurry, the following components are included in percentage by mass: 20-50wt% boron nitride, 0.001-4wt% hydrogenated castor oil, 0.001-0.2wt% ethyl cellulose, 0.0015-0.8wt% PVB, 5-15wt% triethanolamine, and 20-40wt% of the solvent.
[0011] According to the present invention, the solvent is selected from at least one of terpineol, diethylene glycol butyl ether, dimethyl phthalate, isopropanol, and dimethyl sulfoxide (DMSO).
[0012] According to the present invention, the number average molecular weight of the PVB is 16000-60000 g / mol.
[0013] According to the present invention, the number average molecular weight of the PVB is one of 16000 g / mol, 30000 g / mol and 60000 g / mol.
[0014] The second aspect of the present invention protects a method for preparing the aforementioned ceramic substrate green body coating slurry, wherein the specific steps of the preparation method include:
[0015] (1) first mixing all raw materials except boron nitride to obtain a mixture;
[0016] (2) The mixture is mixed with boron nitride for a second time to obtain a ceramic substrate green body coating slurry.
[0017] In the present invention, all the raw materials except boron nitride include hydrogenated castor oil, ethyl cellulose, PVB, triethanolamine and solvent or PVB, triethanolamine and solvent or hydrogenated castor oil, PVB, triethanolamine and solvent or ethyl cellulose, PVB, triethanolamine and solvent.
[0018] In the present invention, the content of each component is consistent with the protection content of the first aspect of the present invention, and will not be repeated here; after the first mixing, a clear, particle-free, and precipitate-free homogeneous mixture is obtained.
[0019] In the present invention, the temperature of the first mixing is 25-30° C., and the time of the first mixing is 10-30 min.
[0020] In the present invention, the first mixing method is a conventional mixing method in the art, and it only needs to be able to mix evenly.
[0021] According to the present invention, the second mixing method includes ball milling, stirring or grinding.
[0022] In the present invention, the specific reaction instrument is a conventional instrument in the art, and typically, but not limitingly, a three-roller grinder is used for the grinding.
[0023] In the present invention, the temperature of the second mixing is 25-30°C.
[0024] According to the present invention, the second mixing time is 30-80 minutes.
[0025] The third aspect of the present invention protects the use of the aforementioned ceramic substrate green body coating slurry or the aforementioned prepared ceramic substrate green body coating slurry in the sintering of ceramic green bodies.
[0026] According to the present invention, the specific steps of the application are: coating the ceramic substrate green body coating slurry on the ceramic substrate green body, drying it, and then performing ceramic sintering.
[0027] According to the present invention, the drying temperature is 70-120° C., and the drying time is 5-40 minutes.
[0028] In the present invention, the ceramic substrate green body includes an alumina ceramic substrate green body, a silicon nitride ceramic substrate green body, an aluminum nitride ceramic substrate green body, and preferably a silicon nitride ceramic substrate green body or a zirconium oxide toughened alumina (ZTA) ceramic substrate green body.
[0029] According to the present invention, the thickness of the ceramic substrate green body is 0.3-1.0 mm.
[0030] According to the present invention, the coating is performed by a screen printing process.
[0031] According to the present invention, the specific conditions of the screen printing process are: the printing screen mesh is made of stainless steel or polyester, the screen mesh number is 100-500 mesh, the screen tension is 22-30N, and the screen angle is 22.5-24°; the printing pressure is 0.3-0.7MPa, the printing spacing is 0.8-3.5mm, and the printing size is (120-260)mm×(120-190)mm.
[0032] In the present invention, the printed ceramic substrate green body is dried in a dust-free and ventilated environment at 100-120° C. for 10-120 minutes.
[0033] The technical solution of the present invention has the following advantages:
[0034] 1. The present invention provides a ceramic substrate green body coating slurry, which includes the following components in percentage by weight based on the slurry mass: 10-55wt% boron nitride, 0-5wt% hydrogenated castor oil, 0-0.28wt% ethyl cellulose, 0.001-1.1wt% PVB, 2-25wt% triethanolamine, and 30-60wt% solvent; the specific components and amounts of the slurry enable the slurry to fit tightly to the ceramic substrate green body when applied to the surface of the ceramic substrate green body; the specific components and amounts enable the slurry to be evenly distributed on the surface of the ceramic substrate green body when applied to the surface of the ceramic substrate green body, so that the surface of the sintered ceramic substrate is smooth and the qualified rate is high.
[0035] 2. The present invention provides a method for preparing a coating slurry for a ceramic substrate green body, wherein the specific steps of the preparation method include: (1) first mixing all raw materials except boron nitride to obtain a mixture; (2) second mixing the mixture with boron nitride to obtain a coating slurry for a ceramic substrate green body; the mixing method can fully dissolve the raw materials, thereby making the solvent system more evenly mixed, and when it is applied to the surface of the ceramic substrate green body, it can fit tightly, and the slurry is evenly distributed on the surface of the green body, so that the surface of the sintered ceramic substrate is smooth and the qualified rate is high.
[0036] 3. The specific second mixing method in the present invention can fully mix the slurry to improve the uniformity of the overall performance of the slurry, and avoid the difference in powder coating due to the performance difference of each part of the slurry during use, thereby affecting the surface morphology of the ceramic substrate.
[0037] 4. The specific second mixing time in the present invention can further fully mix the slurry to improve the uniformity of the overall performance of the slurry, prevent the problem of uneven powder coating caused by performance differences among various parts of the slurry, and thus ensure the integrity and consistency of the surface morphology of the ceramic substrate.
[0038] 5. The screen printing process used in the present invention can further improve the accuracy of slurry coating (powder coating amount and powder coating thickness), improve work efficiency, and further ensure the uniformity of powder coating, so that the green body remains flat during the sintering process, and the surface of the sintered ceramic substrate is flat and the qualified rate is high. DETAILED DESCRIPTION
[0039] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0040] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0041] The number average molecular weight of PVB-1 is 16000 g / mol;
[0042] The number average molecular weight of PVB-2 is 30,000 g / mol;
[0043] The number average molecular weight of PVB-3 is 60000 g / mol.
[0044] Example 1
[0045] This embodiment provides a ceramic substrate green body coating slurry and a preparation method and application thereof, and the specific steps are as follows:
[0046] (1) adding hydrogenated castor oil, ethyl cellulose, PVB-2, triethanolamine, terpineol and dimethyl phthalate (the mass ratio of terpineol to dimethyl phthalate is 4:1) for first mixing at a temperature of 25° C. for a mixing time of 15 min to obtain a clear homogeneous mixture without particles or precipitation;
[0047] (2) adding boron nitride to the mixture and grinding the mixture at a grinding temperature of 25° C. for a grinding time of 50 min to obtain a ceramic substrate green body coating slurry;
[0048] Based on the mass of the slurry, the following components are included in percentage by mass: 45wt% boron nitride, 0.01wt% hydrogenated castor oil, 0.2wt% ethyl cellulose, 0.5wt% PVB-2, 6.29wt% triethanolamine, 48wt% terpineol and dimethyl phthalate;
[0049] (3) The ceramic substrate green body coating slurry is coated on the ceramic substrate green body by screen printing process. The printing screen is made of polyester, the mesh number of the screen is 300 mesh, the screen tension is 26N, the mesh angle is 22.5°, the printing pressure is 0.4MPa, the printing spacing is 0.98mm, the printing size is consistent with the green body sheet size of 260×140mm, and the green body sheet thickness is 0.45mm. The printed ceramic substrate green body is dried in a dust-free and ventilated environment at 120°C for 10 minutes. After the ceramic substrate green body is dried, the coating thickness of the slurry is 9.6μm and the coating mass of the slurry is 0.35g.
[0050] Example 2
[0051] This embodiment provides a ceramic substrate green body coating slurry and a preparation method and application thereof, and the specific steps are as follows:
[0052] (1) adding hydrogenated castor oil, ethyl cellulose, PVB-2, triethanolamine, terpineol and dimethyl phthalate (the mass ratio of terpineol to dimethyl phthalate is 8:1) for first mixing at a temperature of 25° C. for a mixing time of 15 min to obtain a clear homogeneous mixture without particles or precipitation;
[0053] (2) adding boron nitride to the mixture and ball milling at a temperature of 25° C. for 50 min to obtain a ceramic substrate green body coating slurry;
[0054] Based on the mass of the slurry, the following components are included in percentage by mass: 45wt% boron nitride, 0.01wt% hydrogenated castor oil, 0.2wt% ethyl cellulose, 0.5wt% PVB-2, 6.29wt% triethanolamine, 48wt% terpineol and dimethyl phthalate;
[0055] (3) The ceramic substrate green body coating slurry is coated on the ceramic substrate green body by screen printing process. The printing screen is made of polyester, the mesh number of the screen is 300 mesh, the screen tension is 26N, the mesh angle is 22.5°, the printing pressure is 0.4MPa, the printing spacing is 0.98mm, the printing size is consistent with the green body sheet size of 260×140mm, and the green body sheet thickness is 0.45mm. The printed ceramic substrate green body is dried in a dust-free and ventilated environment at 120°C for 20min. After the ceramic substrate green body is dried, the coating thickness of the slurry is 9.3μm and the coating mass of the slurry is 0.34g.
[0056] Example 3
[0057] This embodiment provides a ceramic substrate green body coating slurry and a preparation method and application thereof, and the specific steps are as follows:
[0058] (1) adding hydrogenated castor oil, ethyl cellulose, PVB-2, triethanolamine, terpineol and dimethyl phthalate (the mass ratio of terpineol to dimethyl phthalate is 4:1) for first mixing at a temperature of 25° C. for a mixing time of 15 min to obtain a clear homogeneous mixture without particles or precipitation;
[0059] (2) adding boron nitride to the mixture and stirring at a temperature of 25° C. for 50 min to obtain a ceramic substrate green body coating slurry;
[0060] Based on the mass of the slurry, the following components are included in the composition by mass percentage: 50wt% boron nitride, 0.01wt% hydrogenated castor oil, 0.2wt% ethyl cellulose, 0.5wt% PVB-2, 6.29wt% triethanolamine, 43wt% terpineol and dimethyl phthalate;
[0061] (3) The ceramic substrate green body coating slurry is coated on the ceramic substrate green body by screen printing process. The printing screen is made of polyester, the mesh number of the screen is 300 mesh, the screen tension is 26N, the mesh angle is 22.5°, the printing pressure is 0.4MPa, the printing spacing is 0.98mm, the printing size is consistent with the green body sheet size of 260×140mm, and the green body sheet thickness is 0.45mm. The printed ceramic substrate green body is dried in a dust-free and ventilated environment at 120°C for 30 minutes. After the ceramic substrate green body is dried, the coating thickness of the slurry is 9.9μm and the coating mass of the slurry is 0.36g.
[0062] Example 4
[0063] This embodiment provides a ceramic substrate green body coating slurry and a preparation method and application thereof, and the specific steps are as follows:
[0064] (1) adding hydrogenated castor oil, ethyl cellulose, PVB-2, triethanolamine, terpineol and dimethyl phthalate (the mass ratio of terpineol to dimethyl phthalate is 4:1) for first mixing at a temperature of 25° C. for a mixing time of 15 min to obtain a clear homogeneous mixture without particles or precipitation;
[0065] (2) adding boron nitride to the mixture and ball milling at a temperature of 25° C. for a grinding time of 40 min to obtain a ceramic substrate green body coating slurry;
[0066] Based on the mass of the slurry, the following components are included in percentage by mass: 45wt% boron nitride, 0.01wt% hydrogenated castor oil, 0.2wt% ethyl cellulose, 0.5wt% PVB-2, 6.29wt% triethanolamine, 48wt% terpineol and dimethyl phthalate;
[0067] (3) The ceramic substrate green body coating slurry is coated on the ceramic substrate green body by screen printing process. The printing screen is made of polyester, the mesh number of the screen is 300 mesh, the screen tension is 26N, the mesh angle is 22.5°, the printing pressure is 0.4MPa, the printing spacing is 0.98mm, the printing size is consistent with the green body sheet size of 260×140mm, and the green body sheet thickness is 0.45mm. The printed ceramic substrate green body is dried in a dust-free and ventilated environment at 120°C for 5 minutes. After the ceramic substrate green body is dried, the coating thickness of the slurry is 9.6μm and the coating mass of the slurry is 0.35g.
[0068] Example 5
[0069] This embodiment provides a ceramic substrate green body coating slurry and a preparation method and application thereof, and the specific steps are as follows:
[0070] (1) adding hydrogenated castor oil, ethyl cellulose, PVB-2, triethanolamine, terpineol and dimethyl phthalate (the mass ratio of terpineol to dimethyl phthalate is 4:1) for first mixing at a temperature of 25° C. for a mixing time of 15 min to obtain a clear homogeneous mixture without particles or precipitation;
[0071] (2) adding boron nitride to the mixture and ball milling at a temperature of 25° C. for 30 min to obtain a ceramic substrate green body coating slurry;
[0072] Based on the mass of the slurry, the following components are included in percentage by mass: 35wt% boron nitride, 0.01wt% hydrogenated castor oil, 0.2wt% ethyl cellulose, 0.5wt% PVB-2, 6.29wt% triethanolamine, 58wt% terpineol and dimethyl phthalate;
[0073] (3) The ceramic substrate green body coating slurry is coated on the ceramic substrate green body by screen printing process. The printing screen is made of polyester, the mesh number of the screen is 300 mesh, the screen tension is 26N, the mesh angle is 22.5°, the printing pressure is 0.4MPa, the printing spacing is 0.98mm, the printing size is consistent with the green body sheet size of 260×140mm, and the green body sheet thickness is 0.45mm. The printed ceramic substrate green body is dried in a dust-free and ventilated environment at 120°C for 15min. After the ceramic substrate green body is dried, the coating thickness of the slurry is 7.7μm and the coating mass of the slurry is 0.28g.
[0074] Example 6
[0075] This embodiment provides a ceramic substrate green body coating slurry and a preparation method and application thereof, and the specific steps are as follows:
[0076] (1) adding hydrogenated castor oil, ethyl cellulose, PVB-2, triethanolamine, terpineol and dimethyl phthalate (the mass ratio of terpineol to dimethyl phthalate is 4:1) for first mixing at a temperature of 25° C. for a mixing time of 15 min to obtain a clear homogeneous mixture without particles or precipitation;
[0077] (2) adding boron nitride to the mixture and stirring at a temperature of 25° C. for 50 min to obtain a ceramic substrate green body coating slurry;
[0078] Based on the mass of the slurry, the following components are included in percentage by mass: 45wt% boron nitride, 0.01wt% hydrogenated castor oil, 0.2wt% ethyl cellulose, 0.5wt% PVB-2, 6.29wt% triethanolamine, 48wt% terpineol and dimethyl phthalate;
[0079] (3) The ceramic substrate green body coating slurry is coated on the ceramic substrate green body by screen printing process. The printing screen is made of polyester, the mesh number of the screen is 400 mesh, the screen tension is 26N, the mesh angle is 22.5°, the printing pressure is 0.4MPa, the printing spacing is 0.98mm, the printing size is consistent with the green body sheet size of 260×140mm, and the green body sheet thickness is 0.45mm. The printed ceramic substrate green body is dried in a dust-free and ventilated environment at 120°C for 15min. After the ceramic substrate green body is dried, the coating thickness of the slurry is 6.87μm and the coating mass of the slurry is 0.25g.
[0080] Example 7
[0081] This embodiment provides a ceramic substrate green body coating slurry and a preparation method and application thereof, and the specific steps are as follows:
[0082] (1) adding hydrogenated castor oil, ethyl cellulose, PVB-2, triethanolamine, terpineol and dimethyl phthalate (the mass ratio of terpineol to dimethyl phthalate is 4:1) for first mixing at a temperature of 25° C. for a mixing time of 15 min to obtain a clear homogeneous mixture without particles or precipitation;
[0083] (2) adding boron nitride to the mixture and ball milling at a temperature of 25° C. for 40 min to obtain a ceramic substrate green body coating slurry;
[0084] Based on the mass of the slurry, the following components are included in percentage by mass: 45wt% boron nitride, 0.01wt% hydrogenated castor oil, 0.2wt% ethyl cellulose, 0.5wt% PVB-2, 6.29wt% triethanolamine, 48wt% terpineol and dimethyl phthalate;
[0085] (3) The ceramic substrate green body coating slurry is coated on the ceramic substrate green body by screen printing process. The printing screen is made of polyester, the mesh number of the screen is 250 mesh, the screen tension is 24N, the mesh angle is 22.5°, the printing pressure is 0.4MPa, the printing spacing is 0.98mm, the printing size is consistent with the green body sheet size of 260×140mm, and the green body sheet thickness is 0.45mm. The printed ceramic substrate green body is dried in a dust-free and ventilated environment at 120℃ for 20min. After the ceramic substrate green body is dried, the coating thickness of the slurry is 12.9μm and the coating mass of the slurry is 0.47g.
[0086] Example 8
[0087] This embodiment provides a ceramic substrate green body coating slurry and a preparation method and application thereof, and the specific steps are as follows:
[0088] (1) adding hydrogenated castor oil, ethyl cellulose, PVB-2, triethanolamine, terpineol and dimethyl phthalate (the mass ratio of terpineol to dimethyl phthalate is 4:1) for first mixing at a temperature of 25° C. for a mixing time of 15 min to obtain a clear homogeneous mixture without particles or precipitation;
[0089] (2) adding boron nitride to the mixture and ball milling at a temperature of 25° C. for 60 min to obtain a ceramic substrate green body coating slurry;
[0090] Based on the mass of the slurry, the following components are included in percentage by mass: 45wt% boron nitride, 0.01wt% hydrogenated castor oil, 0.2wt% ethyl cellulose, 0.5wt% PVB-2, 6.29wt% triethanolamine, 48wt% terpineol and dimethyl phthalate;
[0091] (3) The ceramic substrate green body coating slurry is coated on the ceramic substrate green body by screen printing process. The printing screen is made of polyester, the mesh number of the screen is 300 mesh, the screen tension is 26N, the mesh angle is 22.5°, the printing pressure is 0.5MPa, the printing spacing is 0.98mm, the printing size is consistent with the green body sheet size of 260×140mm, and the green body sheet thickness is 0.45mm. The printed ceramic substrate green body is dried in a dust-free and ventilated environment at 120°C for 25min. After the ceramic substrate green body is dried, the coating thickness of the slurry is 10.44μm and the coating mass of the slurry is 0.38g.
[0092] Example 9
[0093] This embodiment provides a ceramic substrate green body coating slurry and a preparation method and application thereof, and the specific steps are as follows:
[0094] (1) adding hydrogenated castor oil, ethyl cellulose, PVB-2, triethanolamine, terpineol and dimethyl phthalate (the mass ratio of terpineol to dimethyl phthalate is 4:1) for first mixing at a temperature of 25° C. for a mixing time of 15 min to obtain a clear homogeneous mixture without particles or precipitation;
[0095] (2) adding boron nitride to the mixture and ball milling at a temperature of 25° C. for 60 min to obtain a ceramic substrate green body coating slurry;
[0096] Based on the mass of the slurry, the following components are included in percentage by mass: 45wt% boron nitride, 0.01wt% hydrogenated castor oil, 0.2wt% ethyl cellulose, 0.5wt% PVB-2, 6.29wt% triethanolamine, 48wt% terpineol and dimethyl phthalate;
[0097] (3) The ceramic substrate green body coating slurry is coated on the ceramic substrate green body by screen printing process. The printing screen is made of polyester, the mesh number of the screen is 300 mesh, the screen tension is 26N, the mesh angle is 22.5°, the printing pressure is 0.5MPa, the printing spacing is 0.98mm, the printing size is consistent with the green body sheet size of 260×140mm, and the green body sheet thickness is 0.45mm. The printed ceramic substrate green body is dried in a dust-free and ventilated environment at 100°C for 25min. After the ceramic substrate green body is dried, the coating thickness of the slurry is 10.01μm and the coating mass of the slurry is 0.37g.
[0098] Example 10
[0099] This embodiment provides a ceramic substrate green body coating slurry and a preparation method and application thereof, and the specific steps are as follows:
[0100] (1) adding hydrogenated castor oil, ethyl cellulose, PVB-2, triethanolamine, terpineol and dimethyl phthalate (the mass ratio of terpineol to dimethyl phthalate is 4:1) for first mixing at a temperature of 25° C. for a mixing time of 15 min to obtain a clear homogeneous mixture without particles or precipitation;
[0101] (2) adding boron nitride to the mixture and ball milling at a temperature of 25° C. for 60 min to obtain a ceramic substrate green body coating slurry;
[0102] Based on the mass of the slurry, the following components are included in percentage by mass: 45wt% boron nitride, 0.01wt% hydrogenated castor oil, 0.2wt% ethyl cellulose, 0.5wt% PVB-2, 6.29wt% triethanolamine, 48wt% terpineol and dimethyl phthalate;
[0103] (3) The ceramic substrate green body coating slurry is coated on the ceramic substrate green body by screen printing process. The printing screen is made of polyester, the mesh number of the screen is 250 mesh, the screen tension is 26N, the mesh angle is 22.5°, the printing pressure is 0.4MPa, the printing spacing is 0.98mm, the printing size is consistent with the green body sheet size of 260×140mm, and the green body sheet thickness is 0.45mm. The printed ceramic substrate green body is dried in a dust-free and ventilated environment at 120℃ for 20min. After the ceramic substrate green body is dried, the coating thickness of the slurry is 12.9μm and the coating mass of the slurry is 0.47g.
[0104] Embodiment 11
[0105] This embodiment provides a ceramic substrate green body coating slurry and a preparation method and application thereof, and the specific steps are as follows:
[0106] (1) adding ethyl cellulose, PVB-2, triethanolamine and terpineol for first mixing at a mixing temperature of 25° C. for a mixing time of 15 min to obtain a mixture;
[0107] (2) Step (2) is carried out in the manner of Example 1;
[0108] Based on the mass of the slurry, the components include the following mass percentages: boron nitride 45wt%, ethyl cellulose 0.21wt%, PVB-2 0.5wt%, triethanolamine 3.29wt%, pineneol 51wt%;
[0109] (3) Step (3) is carried out in the manner of Example 1.
[0110] Example 12
[0111] This embodiment provides a ceramic substrate green body coating slurry and a preparation method and application thereof, and the specific steps are as follows:
[0112] (1) adding ethyl cellulose, PVB-2, triethanolamine, terpineol and dibutyl phthalate (the mass ratio of terpineol to dibutyl phthalate is 8:2) for first mixing at a temperature of 25° C. for a mixing time of 15 min to obtain a mixture;
[0113] (2) Step (2) is carried out in the manner of Example 1;
[0114] Based on the mass of the slurry, the following components are included in percentage by mass: 53wt% boron nitride, 0.2wt% ethyl cellulose, 0.5wt% PVB-2, 9.3wt% triethanolamine, 37wt% pineneol and dibutyl phthalate;
[0115] (3) Step (3) is carried out in the manner of Example 1.
[0116] Example 13
[0117] This embodiment provides a ceramic substrate green body coating slurry and a preparation method and application thereof, and the specific steps are as follows:
[0118] (1) Step (1) is carried out in the manner of Example 1;
[0119] (2) adding boron nitride to the mixture and stirring at a temperature of 25° C. for 50 min to obtain a ceramic substrate green body coating slurry;
[0120] Based on the mass of the slurry, the following components are included in percentage by mass: 45wt% boron nitride, 0.01wt% hydrogenated castor oil, 0.2wt% ethyl cellulose, 0.5wt% PVB-2, 6.29wt% triethanolamine, 48wt% terpineol and dimethyl phthalate;
[0121] (3) Step (3) is carried out in the manner of Example 1.
[0122] Embodiment 14
[0123] This embodiment provides a ceramic substrate green body coating slurry and a preparation method and application thereof, and the specific steps are as follows:
[0124] (1) adding hydrogenated castor oil, PVB-2, triethanolamine, terpineol and dimethyl phthalate (the mass ratio of terpineol to dimethyl phthalate is 4:1) for first mixing at a temperature of 25° C. for 15 min to obtain a clear homogeneous mixture without particles or precipitation;
[0125] (2) Step (2) is carried out in the manner of Example 1;
[0126] Based on the mass of the slurry, the following components are included in percentage by mass: 45wt% boron nitride, 0.01wt% hydrogenated castor oil, 0.5wt% PVB-2, 6.29wt% triethanolamine, 48.2wt% terpineol and dimethyl phthalate;
[0127] (3) Step (3) is carried out in the same manner as in Example 1.
[0128] Embodiment 15
[0129] This embodiment provides a ceramic substrate green body coating slurry and a preparation method and application thereof, and the specific steps are as follows:
[0130] (1) adding PVB-2, triethanolamine, terpineol and dimethyl phthalate (the mass ratio of terpineol to dimethyl phthalate is 4:1) for first mixing at a temperature of 25° C. for 15 min to obtain a homogeneous mixture without particles or precipitation;
[0131] (2) Step (2) is carried out in the manner of Example 1;
[0132] Based on the mass of the slurry, the following components are included in percentage by mass: 45wt% boron nitride, 0.5wt% PVB-2, 6.29wt% triethanolamine, 48.21wt% terpineol and dimethyl phthalate;
[0133] (3) Step (3) is carried out in the manner of Example 1.
[0134] Example 16
[0135] This embodiment provides a ceramic substrate green body coating slurry and a preparation method and application thereof, and the specific steps are as follows:
[0136] The method of Example 1 is the same, except that "PVB-1" is used to replace "PVB-2".
[0137] Embodiment 17
[0138] This embodiment provides a ceramic substrate green body coating slurry and a preparation method and application thereof, and the specific steps are as follows:
[0139] The method of Example 1 is the same, except that "PVB-3" is used to replace "PVB-2".
[0140] Comparative Example 1
[0141] This comparative example provides a ceramic substrate green body coating slurry and a preparation method and application thereof, and the specific steps are as follows:
[0142] (1) adding hydrogenated castor oil, ethyl cellulose, PVB-2, triethanolamine, terpineol and dimethyl phthalate (the mass ratio of terpineol to dimethyl phthalate is 4:1) for first mixing at a temperature of 25° C. for a mixing time of 15 min to obtain a clear homogeneous mixture without particles or precipitation;
[0143] (2) adding boron nitride to the mixture and grinding the mixture at a grinding temperature of 25° C. for a grinding time of 50 min to obtain a ceramic substrate green body coating slurry;
[0144] Based on the mass of the slurry, the following components are included in percentage by mass: 45wt% boron nitride, 0.01wt% hydrogenated castor oil, 2wt% ethyl cellulose, 0.5wt% PVB-2, 6.29wt% triethanolamine, 46.2wt% terpineol and dimethyl phthalate;
[0145] (3) Step (3) is carried out in the manner of Example 1.
[0146] Comparative Example 2
[0147] This comparative example provides a ceramic substrate green body coating slurry and a preparation method and application thereof, and the specific steps are as follows:
[0148] (1) adding tributyl citrate, ethyl cellulose, PVB-2, triethanolamine, terpineol and dimethyl phthalate (the mass ratio of terpineol to dimethyl phthalate is 4:1) for first mixing at a temperature of 25° C. for a mixing time of 15 min to obtain a clear homogeneous mixture without particles or precipitation;
[0149] (2) Step (2) is carried out in the manner of Example 1;
[0150] Based on the mass of the slurry, the following components are included in percentage by mass: 45wt% boron nitride, 0.01wt% tributyl citrate, 0.2wt% ethyl cellulose, 0.5wt% PVB-2, 6.29wt% triethanolamine, 48wt% terpineol and dimethyl phthalate;
[0151] (3) Step (3) is carried out in the manner of Example 1.
[0152] Comparative Example 3
[0153] This comparative example provides a ceramic substrate green body coating slurry and a preparation method and application thereof, and the specific steps are as follows:
[0154] (1) adding hydrogenated castor oil, phenolic resin, PVB-2, triethanolamine, terpineol and dimethyl phthalate (the mass ratio of terpineol to dimethyl phthalate is 4:1) for first mixing at a temperature of 25° C. for 15 min to obtain a clear homogeneous mixture without particles or precipitation;
[0155] (2) Step (2) is carried out in the manner of Example 1;
[0156] Based on the mass of the slurry, the following components are included in percentage by mass: 45wt% boron nitride, 0.01wt% hydrogenated castor oil, 0.2wt% phenolic resin, 0.5wt% PVB-2, 6.29wt% triethanolamine, 48wt% pine alcohol and dimethyl phthalate;
[0157] (3) Step (3) is carried out in the manner of Example 1.
[0158] Comparative Example 4
[0159] This comparative example provides a ceramic substrate green body coating slurry and a preparation method and application thereof, and the specific steps are as follows:
[0160] (1) adding hydrogenated castor oil, ethyl cellulose, PAA, triethanolamine, terpineol and dimethyl phthalate (the mass ratio of terpineol to dimethyl phthalate is 4:1) for first mixing at a temperature of 25° C. for a mixing time of 15 min to obtain a clear homogeneous mixture without particles or precipitation;
[0161] (2) Step (2) is carried out in the manner of Example 1;
[0162] Based on the mass of the slurry, the following components are included in percentage by mass: 45wt% boron nitride, 0.01wt% hydrogenated castor oil, 0.2wt% ethyl cellulose, 0.5wt% PAA, 6.29wt% triethanolamine, 48wt% terpineol and dimethyl phthalate;
[0163] (3) Step (3) is carried out in the manner of Example 1.
[0164] Comparative Example 5
[0165] This comparative example provides a ceramic substrate green body coating slurry and a preparation method and application thereof, and the specific steps are as follows:
[0166] (1) adding hydrogenated castor oil, ethyl cellulose, PVB-2, acrylate, terpineol and dimethyl phthalate (the mass ratio of terpineol to dimethyl phthalate is 4:1) for first mixing at a temperature of 25° C. for a mixing time of 15 min to obtain a clear homogeneous mixture without particles or precipitation;
[0167] (2) Step (2) is carried out in the manner of Example 1;
[0168] Based on the mass of the slurry, the following components are included in percentage by mass: 45wt% boron nitride, 0.01wt% hydrogenated castor oil, 0.2wt% ethyl cellulose, 0.5wt% PVB-2, 6.29wt% acrylate, 48wt% pineneol and dimethyl phthalate;
[0169] (3) Step (3) is carried out in the manner of Example 1.
[0170] Test Case
[0171] The slurries obtained in the examples and comparative examples were tested:
[0172] The specific test method of viscosity test is: use a rotational viscometer to perform viscosity test at a limited ambient temperature of 25°C;
[0173] The specific test method for thixotropy is: using a rheometer to perform a thixotropy test under a limited ambient temperature condition of 25°C.
[0174] 200 pieces of dried ceramic substrate green sheets were sintered. The specific sintering method was as follows: stack the green sheets in 10 layers in a boron nitride crucible device and sinter them at a sintering temperature of 1900°C to obtain ceramic substrates for testing:
[0175] The specific test method for the ratio of concave and convex is as follows: use a 3D profile scanner to scan a ceramic substrate with a size of (120-260) × (120-190) mm, and define pits with a depth of > 0.3 mm and a diameter of > 2 mm as concave points; define protrusions with a height of > 0.3 mm and a diameter of > 2 mm as convex points. The formula for calculating the ratio of concave and convex is the number of green sheets containing concave and convex pieces / all green sheets × 100%.
[0176] The specific test method for the wrinkle ratio is: use a 3D profile scanner to scan a ceramic substrate with a size of (120-260) × (120-190) mm, and define long strips with a depth of > 0.3 mm, a length of > 1 cm, and a width of > 2 mm as wrinkles. The wrinkle ratio is wrinkled blanks / all blanks × 100%.
[0177] Table 1
[0178]
[0179] By comparing the embodiment with comparative examples 1-5, it can be seen that when the slurry with specific components and dosage of the present invention is applied to the surface of the ceramic substrate green body, it can fit closely with the ceramic substrate green body and be evenly distributed, so that the surface of the sintered ceramic substrate is smooth and the qualified rate is high.
[0180] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.
Claims
1. A ceramic substrate green body coating slurry, characterized in that: Based on the mass of the slurry, the composition is composed of the following components in percentage by mass: 20-50wt% of boron nitride, 0.001-4wt% of hydrogenated castor oil, 0.001-0.2wt% of ethyl cellulose, 0.0015-0.8wt% of PVB, 5-15wt% of triethanolamine, and 30-60wt% of solvent.
2. The slurry according to claim 1, characterized in that The solvent is selected from at least one of terpineol, dimethyl sulfoxide, diethylene glycol butyl ether, dimethyl phthalate, and isopropyl alcohol; The number average molecular weight of the PVB is 16000-60000 g / mol.
3. The slurry according to claim 2, characterized in that The number average molecular weight of the PVB is one of 16000 g / mol, 30000 g / mol and 60000 g / mol.
4. A method for preparing a ceramic substrate green body coating slurry according to any one of claims 1 to 3, characterized in that: The specific steps of the preparation method include: (1) first mixing all raw materials except boron nitride to obtain a mixture; (2) The mixture is mixed with boron nitride for a second time to obtain a ceramic substrate green body coating slurry.
5. The preparation method according to claim 4, characterized in that: The second mixing method includes ball milling and stirring; The second mixing time is 30-80 min.
6. Use of the ceramic substrate green body coating slurry described in any one of claims 1 to 3 or the ceramic substrate green body coating slurry prepared by the preparation method described in claim 4 or 5 in sintering ceramic green bodies.
7. The use according to claim 6, characterized in that: The specific application steps are: coating the ceramic substrate green body coating slurry on the ceramic substrate green body, drying it, and then sintering the ceramic.
8. The use according to claim 7, characterized in that: The green body thickness of the ceramic substrate is 0.3-1.0 mm; The drying temperature is 70-120° C., and the drying time is 5-40 min.
9. The use according to claim 7, characterized in that: The coating is performed by screen printing.
10. The use according to claim 9, characterized in that: The specific conditions of the screen printing process are: the mesh number of the screen is 100-500 meshes, the screen tension is 22-30N, the mesh angle is 22.5-24°; the printing pressure is 0.3-0.7MPa, and the printing spacing is 0.8-3.5mm.