A kind of ablation-resistant lightweight heat-insulating silicon-based nano thermal protection material and preparation method thereof

Si-B-O-C aerogel is prepared through two-step acid-base catalytic and supercritical drying technology, which solves the problem of insufficient thermal insulation performance of thermal insulation tile materials in the prior art, achieves efficient thermal protection effect, and provides a kind of Lightweight thermally insulated silicon-based nano-thermal protection material with temperature resistance, heat insulation and high mechanical strength.

CN118561616BActive Publication Date: 2024-11-19WUZHEN LABORATORY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411045734.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-19
Estimated Expiration
2044-08-01

AI Technical Summary

Technical Problem

The existing rigid thermal insulation tile/SiO2 aerogel composite materials have insufficient microstructure control of the cracking products in the pores, resulting in poor thermal insulation performance, insufficient temperature resistance, low mechanical strength, and high thermal conductivity. It requires a It can combine heat resistance, heat insulation and high mechanical strength thermal protection materials.

Method used

Si-B-O-C aerogel was prepared by sol impregnating rigid heat insulation tiles through two steps of acid-base catalysis, forming a filled aerogel with beaded model structure, with low linear ablation recuperation rate, and was prepared by supercritical drying process. Ablation-resistant lightweight thermally insulated silicon-based nano-thermal protection material with excellent thermal insulation properties.

Benefits of technology

The ablation characteristic of effectively taking away the incoming heat flow at high temperature is achieved, forming a liquid protective film to reduce the ablation rate, significantly improving the thermal insulation performance and ablation resistance, and obtaining a lightweight and efficient thermal protection material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118561616B_ABST
    Figure CN118561616B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of aircraft thermal protection materials. Aiming at the problem that thermal protection materials cannot have both temperature resistance, heat insulation and high mechanical strength, the present invention provides an ablation-resistant lightweight heat-insulating silicon-based nano thermal protection material and a preparation method thereof. The matrix of the thermal protection material is a rigid heat-insulating tile, and the gaps inside the rigid heat-insulating tile are filled with aerogel; the aerogel is an aerogel made of precursors alkoxysilane, tetrafunctional siloxane and borate, and has a beaded model structure. The average pore size of the aerogel is 20-50 nm, and the specific surface area is 500-2000 m 2 / g; the line ablation retreat rate of the thermal protection material is less than 0.002 mm / s. The preparation method is that the precursor is subjected to acid-base two-step catalysis to obtain a beaded model sol; the sol is used to impregnate the rigid thermal insulation tile, and the rigid thermal insulation tile filled with aerogel is obtained after aging, solvent replacement, and supercritical drying. The thermal protection material of the present invention has extremely low ablation thermal protection effect and excellent thermal protection performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of aircraft thermal protection materials, and in particular to an ablation-resistant, lightweight, heat-insulating silicon-based nano thermal protection material and a preparation method thereof. Background Art

[0002] Ceramic fiber rigid thermal insulation tile materials have good thermal insulation and mechanical properties and are widely used in reusable protection systems for the thermal outer surfaces of spacecraft. For example, patent CN105272322A discloses a lightweight, high-temperature resistant ceramic fiber rigid thermal insulation tile and a manufacturing method thereof, wherein the thermal insulation tile comprises ceramic fiber and boron oxide, wherein the ceramic fiber comprises quartz fiber, alumina fiber and yttria-stabilized zirconia fiber.

[0003] Since the pores in the fiber matrix of the thermal insulation tile are interconnected, aerogel or resin can be compounded into the pores through a vacuum-assisted impregnation process to give the thermal insulation tile better thermal protection performance. For example, patents such as US6770582 and US2002 / 0061396A1 disclose methods for preparing lightweight thermal insulation tile composite silica aerogel materials; NASA Ames Research Center has developed a lightweight ceramic-based ablative thermal protection material - Silicone Impregnated Reusable Ceramic Ablator (SIRCA) (Kelly E. Parmenter, et. al, Compressive Response of Lightweight Ceramic Ablators: Silicone Impregnated Reusable Ceramic Ablator. [J] Journal of Spacecraft and Rockets, 2002, 39(2):290-290.DOI:10.2514 / 2.3811.). SIRCA material has good mechanical properties and ceramicizes after ablation. It is used as the leading edge of the wings of hypersonic aircraft verification aircraft such as the US X-33 and X-34, and has been verified in actual flight engineering.

[0004] However, the current rigid insulation tile / SiO 2 Aerogel composite materials do not control the microstructure of the cracking products in the pores, and have insufficient thermal insulation performance, insufficient temperature resistance, and low mechanical strength; SIRCA materials have high thermal conductivity and require additional thermal insulation materials to be arranged inside them. Therefore, an ideal solution is needed. Summary of the invention

[0005] In order to overcome the problem that thermal protection materials cannot have temperature resistance, heat insulation and high mechanical strength, the present invention provides an ablation-resistant lightweight thermal insulation silicon-based nano thermal protection material and a preparation method thereof. Rigid thermal insulation tiles are impregnated with sol to obtain rigid thermal insulation tiles filled with aerogel. The aerogel particles have a better beaded model structure and an extremely low linear ablation retreat rate.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] A light-weight, ablation-resistant, heat-insulating silicon-based nano-thermal protection material, wherein the substrate is a rigid heat-insulating tile, and the gaps inside the rigid heat-insulating tile are filled with aerogel; the aerogel is a Si-BOC aerogel made from precursors alkoxysilane, tetrafunctional siloxane and borate, and presents a beaded model structure; the average pore size of the aerogel is 20-50 nm, and the specific surface area is 500-2000 m 2 / g; the linear ablation retreat rate of the thermal protection material is less than 0.002 mm / s.

[0008] Preferably, the alkoxysilane is composed of R 1 R 2 -Si-(OR 3 ) 2 and R 4 H-Si-(OR 5 ) 2 Composition, R 1 , R 2 , R 4 is one of methyl, ethyl, propyl, butyl, octadecyl, perfluorosubstituted octadecyl, vinyl, isopropyl, allyl, phenyl, styryl, and cumyl, and R 3 , R 5 It is one of methyl, ethyl, propyl, butyl and isopropyl.

[0009] Preferably, R 1 R 2 -Si-(OR 3 ) 2 , R 4 H-Si-(OR 5 ) 2 , the molar ratio of tetrafunctional siloxane and borate is 1:1:(3-7):(0.6-0.9).

[0010] Preferably, the tetrafunctional siloxane is one of ethyl orthosilicate, methyl orthosilicate and polyethyl silicate; and the borate is one of tributyl borate, triethyl borate and trimethyl borate.

[0011] The present invention also provides a method for preparing the ablation-resistant lightweight heat-insulating silicon-based nano thermal protection material, comprising the following steps:

[0012] (1) The precursor undergoes two-step acid-base catalysis to obtain a beaded model sol;

[0013] (2) Rigid thermal insulation tiles are impregnated with sol, and after aging, solvent replacement, and supercritical drying, rigid thermal insulation tiles filled with aerogel are obtained.

[0014] Preferably, the conditions for acid catalysis in the acid-base two-step catalysis are: adding an acidic catalyst to adjust the pH value to 2-4, and stirring for 2-8 h; the conditions for base catalysis are: dropping a basic catalyst to adjust the pH value to 6-8, and stirring for 20-30 min.

[0015] Preferably, the alkaline catalyst contains a main catalyst and a sub-catalyst, the main catalyst is one of ammonia water, 1-ethanolamine, urea, and acetonitrile, and the sub-catalyst is one of ammonium fluoride, tetrabutylammonium fluoride, and tetramethylammonium fluoride.

[0016] Preferably, the preparation method of the rigid thermal insulation tile is: mix 1% to 5% by mass of boron nitride, 50% to 99% by mass of quartz fiber and 0% to 49% by mass of fiber reinforcement with water, filter and obtain a solid mixture, dry and sinter the solid mixture to obtain a rigid thermal insulation tile matrix; the fibers in the fiber reinforcement are selected from one or more of alumina fibers, mullite fibers, aluminum silicate fibers, zirconium oxide fibers and yttrium aluminum garnet fibers.

[0017] Preferably, the impregnation is vacuum impregnation, injecting the sol into the pores of the rigid insulation tile.

[0018] Preferably, the aging is performed for 24-30 h; the solvent is replaced with anhydrous ethanol, and fresh anhydrous ethanol is replaced every 7-9 h, and this is repeated 4 to 6 times.

[0019] Preferably, the parameters of supercritical drying are: controlling the temperature in the kettle to 40-80°C, the pressure to 8-12 MPa, and releasing the pressure in the kettle at a rate of 20-30 kPa / min after 25-35 min.

[0020] Therefore, the beneficial effects of the present invention are as follows: the thermal protection material obtained by the present invention has (1) similar ablation characteristics to SIRCA because the gel contains Si-R bonds, the Si-C bonds break at high temperatures, and the borosilicate resin is cracked to release hydrocarbon small molecule gases, which can effectively take away the incident heat flux. Since the material is an aerogel prepared using a supercritical drying process, its thermal insulation performance is one order of magnitude better than that of the SIRCA material. (2) The boron element uniformly distributed in the material matrix is ​​oxidized to generate boron oxide in a high-temperature oxygen environment, and the boron oxide reacts with SiO 2 、Al 2 O 3Oxide ceramics such as quartz and tantalum can form a low-melting-point solid solution liquid film. Therefore, during the ablation process of the composite material, a liquid protective film is formed on the surface of the material to prevent oxygen atoms from diffusing into the interior of the material, thereby reducing the ablation rate of the material and obtaining an ablation-resistant thermal protection material. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is the SEM image of the plane direction of the ultrafine ceramic fiber rigid insulation tile.

[0022] Figure 2 This is the SEM image of the ultrafine ceramic fiber rigid insulation tile in the thickness direction.

[0023] Figure 3 This is a SEM image of the ablation-resistant, lightweight, heat-insulating silicon-based nano thermal protection material of Example 1, with a magnification of 1000 times.

[0024] Figure 4 This is a partially enlarged SEM image of the Si-BOC aerogel in the ablation-resistant, lightweight, heat-insulating silicon-based nano thermal protection material of Example 1, with a magnification of 50,000 times.

[0025] Figure 5 This is a graph showing the BET adsorption and pore structure test results of Si-BOC aerogel in the ablation-resistant, lightweight, thermally insulating silicon-based nano thermal protection material of Example 1.

[0026] Figure 6 This is a local magnified SEM of the Si-BOC aerogel prepared by the one-step acid catalysis method in the comparative example, with a magnification of 20,000 times.

[0027] Figure 7 This is the response curve of the back temperature of the sample of the ablation-resistant lightweight heat-insulating silicon-based nano thermal protection material of Example 1 under the oxygen-acetylene flame ablation conditions of 1200°C front temperature and 30 minutes of continuous burning.

[0028] Figure 8 This is a comparison diagram of the surface of the ablation-resistant lightweight heat-insulating silicon-based nano thermal protection material of Example 1 before and after oxygen-acetylene ablation. DETAILED DESCRIPTION

[0029] The technical solution of the present invention is further described below through specific embodiments.

[0030] In the present invention, unless otherwise specified, the raw materials and equipment used can be purchased from the market or are commonly used in the art. The methods in the embodiments, unless otherwise specified, are all conventional methods in the art. Unless otherwise specified, parts are by weight, temperatures are expressed in ° C or at ambient temperature, and pressures are atmospheric pressure or near atmospheric pressure. There are many variations and combinations of reaction conditions (such as component concentrations, desired solvents, solvent mixtures, temperatures, pressures, and other reaction ranges) and conditions that can be used to optimize the purity and yield of the product obtained by the method, and only reasonable routine experiments will be required to optimize such method conditions.

[0031] Example

[0032] A light-weight, ablation-resistant silicon-based nano-thermal protection material, wherein the substrate is a rigid thermal insulation tile, and the gaps inside the rigid thermal insulation tile are filled with aerogel; the aerogel is Si-BOC aerogel, presenting a beaded model structure, with an average pore size of 20-50 nm and a specific surface area of ​​500-2000 m 2 / g; the linear ablation retreat rate of the thermal protection material is less than 0.002 mm / s.

[0033] The method for preparing the ablation-resistant, lightweight, heat-insulating silicon-based nano thermal protection material comprises the following steps:

[0034] (1) R 1 R 2 -Si-(OR 3 ) 2 , R 4 H-Si-(OR 5 ) 2 , tetrafunctional siloxane and borate as precursors, and the sol is obtained by acid-base two-step catalysis

[0035] R 1 R 2 -Si-(OR 3 ) 2 In, R 1 , R 2 is the same or different combination of methyl, ethyl, propyl, butyl, octadecyl, perfluoro-substituted octadecyl, vinyl, isopropyl, allyl, phenyl, styryl, cumene, etc., R 3 It is one of methyl, ethyl, propyl, butyl and isopropyl;

[0036] R 4 H-Si-(OR 5 ) 2 In, R 4 is one of methyl, ethyl, propyl, butyl, octadecyl, perfluorosubstituted octadecyl, vinyl, isopropyl, allyl, phenyl, styryl, cumene, etc., R5 It is one of methyl, ethyl, propyl, butyl and isopropyl. The active hydrogen in this component tends to react with R in the first component at high temperature. 1 , R 2 Elimination reaction occurs, thereby removing small hydrocarbon molecules and taking away the incident heat flux. However, the R group (R 1 -R 5 ) cannot be methyl at the same time. If both are methyl, the hydrolysis speed will be fast and the gelation reaction speed will also be fast;

[0037] Tetrafunctional siloxane is one of ethyl orthosilicate (Si-28), methyl orthosilicate, and polyethyl silicate (Si-40). Tetrafunctional siloxane acts as a crosslinking agent in the co-hydrolysis system;

[0038] The borate ester is one of tributyl borate, triethyl borate and trimethyl borate. The borate ester provides a boron source and also acts as a cross-linking agent.

[0039] (1.1) R 1 R 2 -Si-(OR 3 ) 2 , R 4 H-Si-(OR 5 ) 2 , tetrafunctional siloxane and borate are mixed in a molar ratio of 1:1:(3-7):(0.6-0.9), ethanol and 1M nitric acid aqueous solution are added to adjust the pH value to 2-4, and the mixture is stirred for 2-8 h to obtain a hydrolyzate.

[0040] (1.2) Add an alkaline catalyst dropwise to the hydrolyzate, adjust the pH value to 6-8, and stir for 20-30 min to obtain a sol. The alkaline catalyst is a mixture of a main catalyst and a secondary catalyst, the main catalyst is one of ammonia water, 1-ethanolamine, urea, and acetonitrile, and the secondary catalyst is one of ammonium fluoride, tetrabutylammonium fluoride, and tetramethylammonium fluoride. An environment with a pH value of 6-8 is more conducive to the formation of gel particles with a fine particle size (20-30 nm), and the grown aerogel structure is more uniform and has better thermal insulation performance.

[0041] (2) The rigid thermal insulation tile is impregnated with sol, and the product is obtained after aging, solvent replacement, and supercritical drying.

[0042] The present invention does not limit rigid thermal insulation tiles. Preferably, the preparation method of rigid thermal insulation tiles is as follows: 1-5% by mass of boron nitride, 50%-99% by mass of quartz fiber and 0%-49% by mass of fiber reinforcement are mixed with water and then filtered to obtain a solid mixture, the solid mixture is dried and sintered to obtain a rigid thermal insulation tile matrix; the fibers in the fiber reinforcement are selected from one or more of alumina fibers, mullite fibers, aluminum silicate fibers, zirconium oxide fibers and yttrium aluminum garnet fibers. (2.1) Before the sol in step (1.2) gels, open the vacuum-assisted impregnation tooling as soon as possible to inject glue into the pores of the rigid thermal insulation tiles; maintain the absolute pressure of the vacuum tank at 5-50 kPa, and let it stand for 24-30 hours to allow the gel to age;

[0043] (2.2) Open the vacuum tank, take out the rigid insulation tile filled with borosilicate resin alcohol gel, and place it in anhydrous ethanol for solvent replacement; replace with fresh anhydrous ethanol every 7-9 hours, and repeat at least 4-6 times;

[0044] (2.3) Place the thermal insulation tile / borosilicate resin alcohol gel composite material after solvent replacement into CO 2 The supercritical drying kettle is used to start the supercritical drying process; the temperature in the kettle is controlled to be 40-80°C and the pressure is controlled to be 8-12 MPa, and the pressure in the kettle is released at a rate of 20-30 kPa / min after 25-35 minutes. The sample is taken out from the supercritical drying kettle to obtain a rigid thermal insulation tile filled with aerogel, that is, the ablation-resistant lightweight thermal insulation silicon-based thermal protection material described in the present invention.

[0045] Compared with the prior art, the differences of the present invention are as follows: ① The present invention uses an acid-base two-step method to catalyze sol-gel, and the obtained aerogel particles have a better beaded model structure. The prior art uses a one-step acid catalysis method to achieve gelation, which is more inclined to form a worm-like chain. ② The prior art uses atmospheric pressure heating to dry the wet gel, and has a high-temperature carbonization post-treatment. The density of the carbon ceramic after multiple sol-gel-carbonization densification treatments will be significantly improved. The present invention is to obtain an integrated heat-insulating composite material. After obtaining the aerogel, no subsequent carbonization treatment is performed. The hydrocarbon groups remaining on the side chains of the resin play a role in ablation heat protection during the service of the material. ③ In the preparation process of SIRCA, the silicone resin / toluene solution is directly impregnated and cured, and the solvent toluene is evaporated. This solvent evaporation process will leave a large number of micron-sized finger-like holes on the outer surface of SIRCA. Therefore, in actual use, the outer surface of SIRCA needs to be further densified and coated. The material obtained by the present invention is a uniform nano-skeleton-nanopore structure, which has better thermal insulation performance than SIRCA.

[0046] Example 1

[0047] A method for preparing an ablation-resistant, lightweight, heat-insulating silicon-based nano thermal protection material, comprising the following steps:

[0048] (1) R 1 R 2 -Si-(OR 3 ) 2 , R 4 H-Si-(OR 5 ) 2 , tetrafunctional siloxane and borate as precursors, and the sol is obtained by acid-base two-step catalysis

[0049] R 1 R 2 -Si-(OR 3 ) 2 In, R 1 , R 2 is methyl, R 3 is ethyl; R 1 R 2 -Si-(OR 3 ) 2 R is dimethyldiethoxysilane. 4 H-Si-(OR 5 ) 2 In, R 4 is methyl, R 5 is ethyl; R 4 H-Si-(OR 5 ) 2 The tetrafunctional siloxane is ethyl orthosilicate (Si-28). The borate ester is trimethyl borate.

[0050] (1.1) 18.6 g (0.125 mol) of dimethyldiethoxysilane, 156.2 g (0.75 mol) of ethyl orthosilicate, 23 g (0.1 mol) of trimethyl borate, 16.8 g (0.125 mol) of methyldiethoxysilane, 90 g (5 mol) of H 2 O was added to 368.5 g (8 mol) of ethanol, and 53 g of 1 M hydrochloric acid was added to adjust the pH value to 2, and stirred for 2 h to obtain a hydrolyzate;

[0051] (1.2) Add 97.1 g of 0.5 M ammonia water dropwise to the hydrolyzate, adjust the pH to 7, and continue stirring for 3 min.

[0052] (1.3) Continue to add 10 g of 1 M NH 4 F aqueous solution and continue stirring for 20 min to obtain a sol.

[0053] (2) The rigid thermal insulation tile is impregnated with the sol, and the product is obtained after aging, solvent replacement and supercritical drying.

[0054] The preparation method of the rigid thermal insulation tile is as follows: 80g of quartz fiber, 5g of boron nitride powder, 20g of alumina fiber, and 10g of zirconia fiber are added into deionized water and mixed evenly, and the mixture is filtered after stirring for 2 hours, and the mixture is pressed into a specified size and then dried and sintered to obtain the quartz fiber rigid thermal insulation tile;

[0055] The apparent density of the rigid insulation tile is 0.24 g / cm 3 , size is 150mm×150mm×10mm. SEM image in plane direction is as follows Figure 1 As shown, there are pores inside that can be filled. The SEM image in the thickness direction is shown in Figure 2 As shown, it can be observed that the fibers are clearly oriented along the plane direction.

[0056] (2.1) Before the sol in step (1.2) gels, open the vacuum-assisted impregnation tooling and inject glue into the pores of the rigid insulation tile; maintain the absolute pressure of the vacuum tank at 50 kPa and let it stand for 24 hours to allow the gel to age;

[0057] (2.2) Open the vacuum tank, take out the rigid insulation tile filled with borosilicate resin alcohol gel, and place it in anhydrous ethanol for solvent replacement; replace with fresh anhydrous ethanol every 8 hours, and repeat 5 times;

[0058] (2.3) Place the thermal insulation tile / borosilicate resin alcohol gel composite material after solvent replacement into CO 2 The supercritical drying kettle is used to start the supercritical drying process; the temperature in the kettle is controlled to be 40°C and the pressure is controlled to be 9 MPa, and the pressure in the kettle is released at a rate of 20 kPa / min after 30 minutes. The sample is taken out from the supercritical drying kettle to obtain a rigid thermal insulation tile filled with aerogel, that is, the ablation-resistant lightweight thermal insulation silicon-based thermal protection material described in the present invention.

[0059] SEM image of ablation-resistant lightweight thermal insulation silicon-based thermal protection material Figure 3 As shown in the figure, it can be seen that the Si-BOC aerogel is fully filled in the pores of the rigid insulation tile, and no micron-sized pores are observed. Figure 4 This is a locally enlarged SEM image of Si-BOC aerogel filled in ablation-resistant lightweight thermal insulation silicon-based thermal protection material, with a magnification of 50,000 times. The Si-BOC aerogel catalyzed by the acid-base two-step method presents a typical beaded (pearl necklace) model structure. Figure 5 The BET adsorption and pore structure test results of Si-BOC aerogels show an average pore size of 30-40 nm and a specific surface area of ​​850 m 2 / g.

[0060] The performance of the ablation-resistant, lightweight, heat-insulating silicon-based nano thermal protection material prepared in this embodiment was characterized. The density was 320 kg / m 3 The compressive strength in the thickness direction is 3.0 MPa (compressive strain 5%); the short-term temperature resistance can reach 2000 ℃, the long-term temperature resistance can reach 1200 ℃, and the equivalent thermal conductivity at room temperature is 0.022 W / (m•K). Figure 7 It is the response curve of the back temperature of the composite material under the oxygen-acetylene flame ablation conditions of 1200 ℃ front temperature and 30 min continuous burning. The sample size is 150mm×150mm×10mm. Figure 8 This is a comparison of the surface of the ablation-resistant light-weight heat-insulating silicon-based nano thermal protection material before and after oxygen-acetylene ablation, and the linear ablation retreat rate is 0.00193 mm / s. It can be seen that the ablation-resistant light-weight heat-insulating silicon-based nano thermal protection material prepared by the present invention is lightweight, has excellent ablation resistance and heat insulation performance, and is an excellent thermal protection material.

[0061] Example 2

[0062] A method for preparing an ablation-resistant, lightweight, heat-insulating silicon-based nano thermal protection material, comprising the following steps:

[0063] (1) R 1 R 2 -Si-(OR 3 ) 2 , R 4 H-Si-(OR 5 ) 2 , tetrafunctional siloxane and borate as precursors, and the sol is obtained by acid-base two-step catalysis

[0064] R 1 R 2 -Si-(OR 3 ) 2 In, R 1 is methyl, R 2 Ethyl, R 3 is propyl; R 1 R 2 -Si-(OR 3 ) 2 It is methylethyldipropoxysilane. 4 H-Si-(OR 5 ) 2 In, R 4 Ethyl, R 5 is butyl; R 4 H-Si-(OR 5 ) 2 The tetrafunctional siloxane is methyl orthosilicate. The borate ester is tributyl borate.

[0065] (1.1) 0.125 mol of methylethyldipropoxysilane, 0.375 mol of methyl orthosilicate, 0.075 mol of tributyl borate, 0.125 mol of ethyldibutoxysilane, and 5 mol of H 2 O was added to 8 mol ethanol, 1 M hydrochloric acid was added, the pH value was adjusted to 3, and stirred for 4 h to obtain a hydrolyzate;

[0066] (1.2) Add 0.5 M ammonia water dropwise to the hydrolyzate, adjust the pH to 6, and continue stirring for 2 min;

[0067] (1.3) Continue to add 1M NH 4 F aqueous solution and continue stirring for 20 min to obtain a sol.

[0068] (2) The rigid insulation tile is impregnated with sol, and the product is obtained after aging, solvent replacement, and supercritical drying.

[0069] (2.1) Before the sol in step (1.2) gels, open the vacuum-assisted impregnation tooling and inject glue into the pores of the rigid thermal insulation tile (same as in Example 1); maintain the absolute pressure of the vacuum tank at 5 kPa and let it stand for 28 hours to allow the gel to age;

[0070] (2.2) Open the vacuum tank, take out the rigid insulation tile filled with borosilicate resin alcohol gel, and place it in anhydrous ethanol for solvent replacement; replace with fresh anhydrous ethanol every 7 hours, and repeat 6 times;

[0071] (2.3) Place the thermal insulation tile / borosilicate resin alcohol gel composite material after solvent replacement into CO 2 The supercritical drying kettle is used to start the supercritical drying process; the temperature in the kettle is controlled to be 60°C and the pressure is 8 MPa, and the pressure in the kettle is released at a rate of 25 kPa / min after 35 minutes. The sample is taken out from the supercritical drying kettle to obtain a rigid thermal insulation tile filled with aerogel, that is, the ablation-resistant lightweight thermal insulation silicon-based thermal protection material described in the present invention.

[0072] Example 3

[0073] A method for preparing an ablation-resistant, lightweight, heat-insulating silicon-based nano thermal protection material, comprising the following steps:

[0074] (1) R 1 R 2 -Si-(OR 3 ) 2 , R 4 H-Si-(OR 5 ) 2 , tetrafunctional siloxane and borate as precursors, and the sol is obtained by acid-base two-step catalysis

[0075] R 1 R 2 -Si-(OR 3 ) 2 In, R 1 For vinyl, R 2 is phenyl, R 3 is methyl; R 1 R 2 -Si-(OR 3 ) 2 is vinylphenyl dimethoxysilane. 4 H-Si-(OR 5 ) 2 In, R 4 is octadecyl, R 5 is methyl; R 4 H-Si-(OR 5 ) 2 The tetrafunctional siloxane is polyethyl silicate (Si-40). The borate ester is tributyl borate.

[0076] (1.1) 0.125 mol of vinylphenyl dimethoxysilane, 0.875 mol of polyethyl silicate (Si-40), 0.1125 mol of tributyl borate, 0.125 mol of octadecyl dimethoxysilane, and 5 mol of H 2 O was added to 8 mol ethanol, 1 M hydrochloric acid was added, the pH value was adjusted to 4, and stirred for 8 h to obtain a hydrolyzate;

[0077] (1.2) Add 0.5 M ammonia water dropwise to the hydrolyzate, adjust the pH to 8, and continue stirring for 5 min;

[0078] (1.3) Continue to add 1M NH 4 F aqueous solution and continue stirring for 20 min to obtain a sol.

[0079] (2) The rigid insulation tile is impregnated with sol, and the product is obtained after aging, solvent replacement, and supercritical drying.

[0080] (2.1) Before the sol in step (1.2) gels, open the vacuum-assisted impregnation tooling and inject glue into the pores of the rigid thermal insulation tile (same as in Example 1); maintain the absolute pressure of the vacuum tank at 20 kPa and let it stand for 30 hours to allow the gel to age;

[0081] (2.2) Open the vacuum tank, take out the rigid insulation tile filled with borosilicate resin alcohol gel, and place it in anhydrous ethanol for solvent replacement; replace it with fresh anhydrous ethanol every 9 hours, and repeat 4 times;

[0082] (2.3) Place the thermal insulation tile / borosilicate resin alcohol gel composite material after solvent replacement into CO 2 The supercritical drying kettle is started; the temperature in the kettle is controlled to be 80°C and the pressure is controlled to be 12 MPa, and the pressure in the kettle is released at a rate of 30 kPa / min after 35 minutes. The sample is taken out from the supercritical drying kettle to obtain a rigid thermal insulation tile filled with aerogel, that is, the ablation-resistant lightweight thermal insulation silicon-based thermal protection material described in the present invention.

[0083] Example 4

[0084] The difference from Example 1 is that the base catalyst in step (1) does not contain NH 4 F aqueous solution. Specifically:

[0085] (1) R 1 R 2 -Si-(OR 3 ) 2 , R 4 H-Si-(OR 5 ) 2 , tetrafunctional siloxane and borate as precursors, and the sol is obtained by acid-base two-step catalysis

[0086] R 1 R 2 -Si-(OR 3 ) 2 In, R 1 , R 2 is methyl, R 3 is ethyl; R 1 R 2 -Si-(OR 3 ) 2 R is dimethyldiethoxysilane. 4 H-Si-(OR 5 ) 2 In, R 4 is methyl, R 5 is ethyl; R 4 H-Si-(OR 5 ) 2 The tetrafunctional siloxane is ethyl orthosilicate (Si-28). The borate ester is trimethyl borate.

[0087] (1.1) 18.6 g (0.125 mol) of dimethyldiethoxysilane, 156.2 g (0.75 mol) of ethyl orthosilicate, 23 g (0.1 mol) of trimethyl borate, 16.8 g (0.125 mol) of methyldiethoxysilane, 90 g (5 mol) of H 2O was added to 368.5 g (8 mol) of ethanol, and 53 g of 1 M hydrochloric acid was added to adjust the pH value to 2, and stirred for 2 h to obtain a hydrolyzate;

[0088] (1.2) Add 97.1 g of 0.5 M ammonia water dropwise to the hydrolyzate, adjust the pH to 9, and continue stirring for 3 min.

[0089] (1.3) Continue to add 10 g of 1 M NH 4 F aqueous solution and continue stirring for 20 min to obtain a sol.

[0090] Step (2) is the same as in Example 1.

[0091] Comparative Example 1

[0092] Compared with Example 1, the precursor for preparing the sol in step (1) is only TEOS (tetraethoxysilane). Specifically:

[0093] (1.1) 20.83 g (0.1 mol) TEOS and 9 g (0.5 mol) H 2 O was added to 36.8 g (0.8 mol) of ethanol, 4.67 g of 1 M hydrochloric acid was added, the pH value was adjusted to 2, and stirred for 2 h to obtain a hydrolyzate;

[0094] (1.2) Add 9.85 g of 0.5 M ammonia water dropwise to the hydrolyzate, adjust the pH to 7, and continue stirring for 3 min.

[0095] (1.3) Continue to add 1 g of 1M NH 4 F aqueous solution, and continue stirring for 30 s to obtain a transparent alcohol gel.

[0096] If the gelation is too fast, it will not be conducive to providing a time window for the vacuum impregnation process. The resulting alcohol gel is completely rigid and cannot be used for the impregnation in step (2).

[0097] Comparative Example 2

[0098] Compared with Example 1, the precursors for preparing the sol in step (1) only contain TEOS (tetraethoxysilane) and DMDES (dimethyldiethoxysilane) in an equal molar ratio. Specifically:

[0099] (1.1) 10.83 g (0.05 mol) TEOS, 7.41 g (0.05 mol) DMDES and 8.1 g (0.45 mol) H 2 O was added to 36.8 g (0.8 mol) of ethanol, 4.67 g of 1 M hydrochloric acid was added, the pH value was adjusted to 2, and stirred for 2 h to obtain a hydrolyzate;

[0100] (1.2) Add 9.85 g of 0.5 M ammonia water dropwise to the hydrolyzate, adjust the pH to 7, and continue stirring for 3 min.

[0101] (1.3) Continue to add 1 g of 1M NH 4 F aqueous solution, continue stirring to obtain a milky white alcohol gel, and the complete gel time is ≥48h.

[0102] The obtained product is a microphase-separated silicone resin, and the gel obtained after supercritical drying of the opaque gel contains a large number of micron-sized pores.

[0103] Comparative Example 3

[0104] Compared with Example 1, the precursors for preparing the sol in step (1) are only TEOS and DMDES in a molar ratio of 3:1. Specifically:

[0105] (1.1) 15.62 g (0.075 mol) TEOS, 3.71 g (0.025 mol) DMDES and 9 g (0.5 mol) H 2 O was added to 36.8 g (0.8 mol) of ethanol, and 5.3 g of 1 M hydrochloric acid was added to adjust the pH value to 2, and stirred for 2 h to obtain a hydrolyzate;

[0106] (1.2) Add 9.71 g of 0.5 M ammonia water dropwise to the hydrolyzate, adjust the pH to 7, and continue stirring for 3 min.

[0107] (1.3) Continue to add 1 g of 1M NH 4 F aqueous solution, and continued stirring to obtain a milky white alcohol gel with a gelation time of 12 h.

[0108] Step (2) is the same as in Example 1.

[0109] The obtained aerogel has a certain degree of flexibility and elasticity, which is a relatively ideal gel state.

[0110] Comparative Example 4

[0111] Compared with Example 1, the precursors for preparing the sol in step (1) are TEOS, DMDES and MDES (methyldiethoxysilane) in a molar ratio of 6:1:1. Specifically:

[0112] (1.1) 15.62 g (0.075 mol) TEOS, 1.86 g (0.0125 mol) DMDES, 1.68 g (0.0125 mol) MDES and 9 g (0.5 mol) H 2O was added to 36.8 g (0.8 mol) of ethanol, and 5.3 g of 1 M hydrochloric acid was added to adjust the pH value to 2, and stirred for 2 h to obtain a hydrolyzate;

[0113] (1.2) Add 9.71 g of 0.5 M ammonia water dropwise to the hydrolyzate, adjust the pH to 7, and continue stirring for 3 min.

[0114] (1.3) Continue to add 1 g of 1M NH 4 F aqueous solution, and continued stirring to obtain a milky white alcohol gel with a gelation time of 12 h.

[0115] Step (2) is the same as in Example 1.

[0116] The obtained aerogel has a certain degree of flexibility and elasticity, which is a relatively ideal gel state.

[0117] Comparative Example 5

[0118] The difference from Example 1 is that the methyldiethoxysilane in step (1) is replaced by methyldimethoxysilane, that is, the R group of the precursor is methyl.

[0119] The gelation speed is too fast, only 1 to 2 minutes, which is not conducive to leaving a time window for the operator to inject the glue. The system releases heat violently during the gelation process, the system temperature rises, and methanol is produced in the system, which is prone to explosion accidents.

[0120] Comparative Example 6

[0121] The difference from Example 1 is that a one-step acid catalysis method is used in step (1). Specifically:

[0122] 18.6 g (0.125 mol) of dimethyldiethoxysilane, 156.2 g (0.75 mol) of ethyl orthosilicate, 23 g (0.1 mol) of trimethyl borate, 16.8 g (0.125 mol) of methyldiethoxysilane, 90 g (5 mol) of H 2 O was added to 368.5 g (8 mol) ethanol and stirred for 10 min. Then 53 g of 1 M hydrochloric acid was added to adjust the pH value to 5-6. After stirring for 5-8 min, gelation occurred.

[0123] Step (2) is the same as in Example 1.

[0124] The aerogel structure is as follows: Figure 6 As shown, Figure 4 The beaded model aerogel has different particle sizes and pore sizes of 20~50nm. The prepared aerogel is mainly worm-like chains, and the particle size and pore size of the particles are ≥100nm, which is a subgel (Xerogel).

[0125] Comparative Example 7

[0126] The difference from Example 1 is that the precursor for preparing the sol in step (1) is R 4 H-Si-(OR 5 ) 2 , tetrafunctional siloxane and borate. Specifically:

[0127] (1) R 4 H-Si-(OR 5 ) 2 , tetrafunctional siloxane and borate as precursors, and the sol is obtained by acid-base two-step catalysis

[0128] R 4 H-Si-(OR 5 ) 2 In, R 4 is methyl, R 5 is ethyl; R 4 H-Si-(OR 5 ) 2 The tetrafunctional siloxane is ethyl orthosilicate (Si-28). The borate ester is trimethyl borate.

[0129] (1.1) 156.2 g (0.75 mol) of ethyl orthosilicate, 23 g (0.1 mol) of trimethyl borate, 16.8 g (0.125 mol) of methyldiethoxysilane, 90 g (5 mol) of H 2 O was added to 368.5 g (8 mol) of ethanol, and 53 g of 1 M hydrochloric acid was added to adjust the pH value to 2, and stirred for 2 h to obtain a hydrolyzate;

[0130] (1.2) Add 97.1 g of 0.5 M ammonia water dropwise to the hydrolyzate, adjust the pH to 7, and continue stirring for 3 min.

[0131] (1.3) Continue to add 10 g of 1M NH 4 F aqueous solution and continue stirring for 20 min to obtain a sol.

[0132] Step (2) is the same as in Example 1.

[0133] Comparative Example 8

[0134] The difference from Example 1 is that in step (1), alkali is added to adjust the pH value to 9. Specifically:

[0135] (1) R 1 R 2 -Si-(OR 3 ) 2 , R4 H-Si-(OR 5 ) 2 , tetrafunctional siloxane and borate as precursors, and the sol is obtained by acid-base two-step catalysis

[0136] R 1 R 2 -Si-(OR 3 ) 2 In, R 1 , R 2 is methyl, R 3 is ethyl; R 1 R 2 -Si-(OR 3 ) 2 R is dimethyldiethoxysilane. 4 H-Si-(OR 5 ) 2 In, R 4 is methyl, R 5 is ethyl; R 4 H-Si-(OR 5 ) 2 The tetrafunctional siloxane is ethyl orthosilicate (Si-28). The borate ester is trimethyl borate.

[0137] (1.1) 18.6 g (0.125 mol) of dimethyldiethoxysilane, 156.2 g (0.75 mol) of ethyl orthosilicate, 23 g (0.1 mol) of trimethyl borate, 16.8 g (0.125 mol) of methyldiethoxysilane, 90 g (5 mol) of H 2 O was added to 368.5 g (8 mol) of ethanol, and 53 g of 1 M hydrochloric acid was added to adjust the pH value to 2, and stirred for 2 h to obtain a hydrolyzate;

[0138] (1.2) Add 97.1 g of 0.5 M ammonia water dropwise to the hydrolyzate, adjust the pH to 9, and continue stirring for 3 min.

[0139] (1.3) Continue to add 10 g of 1 M NH 4 F aqueous solution and continue stirring for 20 min to obtain a sol.

[0140] Step (2) is the same as in Example 1.

[0141] Performance Testing

[0142] The thermal properties of the thermal protection materials prepared in each embodiment and comparative example were tested, and the test methods were as follows: ① The equivalent thermal conductivity at room temperature was tested using the test method of GB / T 10294-2008; ② The line ablation retreat rate was tested using the ablation material ablation test method: GJB 323A-1996. The results are shown in the following table:

[0143]

[0144] It can be seen from the above table that, compared with the rigid thermal insulation tile filled with aerogel, the thermal protection material prepared in each embodiment of the present invention significantly improves the thermal protection performance.

[0145] Compared with Example 1, Comparative Example 3 does not add R 4 H-Si-(OR 5 ) 2 and borate, comparative example 4 did not add borate, comparative example 7 did not add R 1 R 2 -Si-(OR 3 ) 2 Dimethyldiethoxysilane, the effect is not as good as that of Example 1, indicating that the four precursors must cooperate with each other to produce a gel with good thermal performance, especially a low line ablation retreat rate. In Example 1, since the gel contains Si-R bonds, the Si-C bonds break at high temperatures, and the borosilicate resin is cracked to release hydrocarbon small molecules, which can effectively take away the incident heat flux; the boron element evenly distributed in the material matrix is ​​oxidized to generate boron oxide in a high-temperature oxygen environment, and the boron oxide reacts with SiO 2 、Al 2 O 3 Oxide ceramics such as quartz and tantalum can form a low-melting-point solid solution liquid film. Therefore, during the ablation process of the composite material, a liquid protective film is formed on the surface of the material to prevent oxygen atoms from diffusing into the interior of the material, thereby reducing the ablation rate of the material.

[0146] The aerogel of Comparative Example 6 was prepared by a one-step acid catalysis method. The aerogel was mainly a worm-like chain, and the particle size and pore size of the colloid particles were ≥100nm; the aerogel prepared by the acid-base two-step method in Example 1 was a beaded model, and the particle size and pore size were 20~50nm; because the pore size of the worm-like chain was about 100nm, which was larger than the mean free path of air molecules of 70nm, it was impossible to completely inhibit gas phase heat conduction, so the thermal protection performance of the beaded model of the present invention was better than that of the worm-like chain material. The pH value of Comparative Example 8 was not within the preferred range when preparing the gel, and the pH value was adjusted by adding alkali in Example 4 when preparing the gel without using a secondary catalyst, which affected the size and uniformity of the beaded model of the gel, which was ultimately manifested as a decrease in the thermal performance of the thermal protection material. Therefore, the preparation parameters must be within the preferred range to achieve better results.

[0147] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.

Claims

1. An ablation-resistant, lightweight, heat-insulating silicon-based nano-thermal protection material, characterized in that: The substrate is a rigid thermal insulation tile, and the internal gap of the rigid thermal insulation tile is filled with aerogel; the aerogel precursor is R 1 R 2 -Si-(OR 3 2. R 4 H-Si-(OR 5 )2. Tetrafunctional siloxane and borate, R 1 , R 2 , R 4 is selected from methyl, ethyl, propyl, butyl, octadecyl, perfluorosubstituted octadecyl, vinyl, isopropyl, allyl, phenyl, styryl, cumene, R 3 , R 5 Selected from methyl, ethyl, propyl, butyl, isopropyl; aerogel presents a beaded model structure, with an average pore size of 20-50nm and a specific surface area of ​​500-2000m 2 / g; the thermal protection material line ablation retreat rate is less than 0.002mm / s.

2. The ablation-resistant, lightweight, heat-insulating silicon-based nano thermal protection material according to claim 1, characterized in that: The tetrafunctional siloxane is one of ethyl orthosilicate, methyl orthosilicate and polyethyl orthosilicate.

3. The ablation-resistant, lightweight, heat-insulating silicon-based nano thermal protection material according to claim 1, characterized in that: The borate ester is one of tributyl borate, triethyl borate and trimethyl borate.

4. The method for preparing the ablation-resistant, lightweight, heat-insulating silicon-based nano thermal protection material according to any one of claims 1 to 3, characterized in that: The following steps are involved: (1) The precursor undergoes two-step acid-base catalysis to obtain a beaded model sol; (2) Rigid thermal insulation tiles are impregnated with sol, and after aging, solvent replacement, and supercritical drying, rigid thermal insulation tiles filled with aerogel are obtained.

5. The method for preparing an ablation-resistant, lightweight, heat-insulating silicon-based nano thermal protection material according to claim 4, characterized in that: The conditions for acid catalysis in the acid-base two-step catalysis are: adding an acid catalyst to adjust the pH to 2-4, and stirring for 2-8 h.

6. The method for preparing the ablation-resistant, lightweight, heat-insulating silicon-based nano thermal protection material according to claim 4 or 5, characterized in that: The conditions for base catalysis in the acid-base two-step catalysis are: add a base catalyst dropwise to adjust the pH to 6-8, and stir for 20-30 min.

7. The method for preparing an ablation-resistant, lightweight, heat-insulating silicon-based nano thermal protection material according to claim 6, characterized in that: The alkaline catalyst contains a main catalyst and a sub-catalyst. The main catalyst is one of ammonia water, 1-ethanolamine, urea and acetonitrile, and the sub-catalyst is one of ammonium fluoride, tetrabutylammonium fluoride and tetramethylammonium fluoride.

8. The method for preparing an ablation-resistant, lightweight, heat-insulating silicon-based nano thermal protection material according to claim 4, characterized in that: The impregnation is vacuum impregnation, and the sol is injected into the pores of the rigid insulation tile.

9. The method for preparing an ablation-resistant, lightweight, heat-insulating silicon-based nano thermal protection material according to claim 4, characterized in that: Aging for 24-30 h; replace the solvent with anhydrous ethanol, replace with fresh anhydrous ethanol every 7-9 h, and repeat 4-6 times.

10. The method for preparing the ablation-resistant, lightweight, heat-insulating silicon-based nano thermal protection material according to claim 4, 8 or 9, characterized in that: The parameters of supercritical drying are: controlling the temperature in the kettle to 40~80℃ and the pressure to 8~12 MPa, and releasing the pressure in the kettle at a rate of 20~30 kPa / min after 25~35 minutes.