A copper or copper alloy refining agent, copper or copper alloy and preparation method of both

Through the deep deoxygenation of copper alloy refining agent of B and Mg elements, the problems of copper alloy oxidation and porosity are solved, the conductivity and mechanical properties are improved, and the efficient production of copper alloy castings is achieved.

CN118563112BActive Publication Date: 2024-11-08烟台杰科金属有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411059901.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-08
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

Copper and copper alloys are easily oxidized during non-vacuum smelting, resulting in material brittleness and pore formation. The existing deoxidation methods are costly or polluted by the environment, and it is difficult to control the content of oxygen and hydrogen, affecting the conductive and mechanical properties of the castings.

Method used

Using copper or copper alloy refining agent with B and Mg elements, the coating structure of Cu-B alloy and Cu-Mg alloy is used to deeply deoxygenate using the high melting point of B and the activeness of Mg to control the content of B and Mg to increase the content of B and Mg. Conductivity and mechanical properties, and particles are prepared by ball milling and sintering processes to optimize the deoxygenation effect.

Benefits of technology

It realizes efficient deoxygenation of copper and copper alloys, improves conductive and mechanical properties, reduces operators' control accuracy requirements for the amount of refining agent added, reduces the generation of oxides, and enhances the high-temperature oxidation resistance and work hardening capabilities of castings. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118563112B_ABST
    Figure CN118563112B_ABST
Patent Text Reader

Abstract

The present invention provides a copper or copper alloy refining agent, copper or copper alloy and a preparation method thereof, which belongs to the technical field of metal smelting. The refining agent is composed of B, Mg and Cu; wherein the mass ratio of B to Mg is 1:3.8-4.5; and the mass fraction of B in the refining agent does not exceed 0.4%. The melt is efficiently deoxidized by Mg, and deep deoxidation is performed by utilizing the easy diffusion of B, and the contents of B and Mg are limited, so that B and Mg have little effect on the conductivity of the metal conductor. At the same time, the added elements only contain B and Mg, ensuring that there will be no significant impact on the composition of copper and copper alloys, refining the structure grains, and improving the mechanical properties of the product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal smelting, and in particular relates to a refining agent for copper or copper alloy, copper or copper alloy and a preparation method of the two. Background Art

[0002] There are many types of cast copper and copper alloys, mainly including pure copper including oxygen-free copper, bronze, brass, white copper, etc. Among them, copper alloys that do not use zinc as the main element are collectively called bronze. Alloys with aluminum as the main element are called aluminum bronze, copper alloys with tin as the main element are called tin bronze, and there are other types of bronze, such as beryllium bronze, lead bronze, manganese bronze, etc. Copper alloys with zinc as the main element are called brass, and white copper is a copper alloy with nickel as the main element.

[0003] When melting in non-vacuum conditions, copper and copper alloys are easily oxidized by oxygen in the furnace gas at high temperatures. The oxidation product is cuprous oxide, with a density of 6g / m 3 , melting point 1235℃, dissolved in molten metal, as the temperature drops, it will form α+Cu with α phase 2 O eutectoids, such as Figure 1 As shown in the figure, the shiny part is its eutectic, which will cause the material to be brittle and react with hydrogen, and produce pores in the casting after solidification.

[0004] Therefore, it is necessary to thoroughly deoxidize. There are many traditional deoxidation methods, such as precipitation deoxidation, diffusion deoxidation, and intermediate alloy deoxidation. The most commonly used is intermediate alloy deoxidation. For electrical equipment, lithium copper is used for deoxidation, but the disadvantage is that the dosage is large and the cost is high. Non-high-conductivity copper materials are generally deoxidized with phosphorus copper (such as 14% phosphorus copper). The price is cheap, but the disadvantage is also obvious. The reaction is violent, and phosphorus pentoxide is generated to pollute the environment. The amount of addition is uncontrollable. If too much is added, the residual phosphorus in the molten metal will react with the water in the mold to produce hydrogen that penetrates into the casting, and the conductivity drops sharply; if too little is added, the residual oxygen and trace amounts of hydrogen will also cause pores in the casting.

[0005] Although aluminum bronze and low-end brass do not need to be deoxidized, micro-alloying is necessary to produce high-quality castings. Taking aluminum bronze as an example, in normal casting production, aluminum bronze will produce α+γ2 eutectoid when solidified. The grain size will continue to grow in sand casting with poor cooling conditions, seriously affecting the plasticity and toughness of the material, making the ordinary aluminum bronze produced domestically fail to achieve the performance of imported materials. Summary of the invention

[0006] In order to solve the above problems, the present invention provides a copper or copper alloy refining agent, copper or copper alloy and a preparation method of the two. The melt is efficiently deoxidized by Mg, and deep deoxidation is performed by utilizing the easy diffusion of B, and the content of B and Mg is limited, so that B and Mg have little effect on the conductivity of the metal conductor. At the same time, the added elements only contain B and Mg, ensuring that there will be no significant impact on the composition of copper and copper alloys, refining the structure grains, and improving the mechanical properties of the product.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0008] The invention provides a copper or copper alloy refining agent, which consists of B, Mg and Cu; wherein the mass ratio of B to Mg is 1:3.8-4.5; and the mass fraction of B in the refining agent does not exceed 0.4%.

[0009] Furthermore, the refining agent is prepared by Cu-B alloy and Cu-Mg alloy.

[0010] Furthermore, the refining agent is a particle of a Cu-B alloy core coated with a Cu-Mg alloy; the size of the particle is 5-15 mm.

[0011] The present invention provides a method for preparing the above-mentioned refining agent, comprising: crushing and screening Cu-Mg alloy and Cu-B alloy, weighing Cu-Mg alloy powder and Cu-B alloy particles that meet the particle size requirements according to proportion; bonding a predetermined mass of Cu-Mg alloy powder to the Cu-B alloy particles, drying and sintering; and vibrating and screening the sintered product.

[0012] Furthermore, the pulverizing process is to ball mill the Cu-Mg alloy and the Cu-B alloy by a ball mill; in the screening process, Cu-B alloy particles with a particle size of 1-5 mm are screened out, and Cu-Mg alloy powder with a particle size less than 15 µm is screened out.

[0013] Furthermore, a predetermined mass of Cu-Mg alloy powder is bonded to the Cu-B alloy particles, including spraying an organic binder on the Cu-B alloy particles and then mixing and sieving the Cu-Mg alloy powder, repeating the above process until the mass ratio of the bonded Cu-Mg alloy powder to the Cu-B alloy particles meets the requirements, and then drying and sintering are performed.

[0014] Furthermore, the drying process is: keeping warm at 100-200°C for at least 5 minutes; the sintering process is: sintering at 900-1000°C for 10-30 minutes in a vacuum or inert gas atmosphere.

[0015] Furthermore, materials are weighed according to the element ratio of copper or copper alloy and heated to a temperature not exceeding the melting point of 120° C. and kept warm until all the materials are melted; the above-mentioned refining agent is added in an amount of 8-15% of the mass of the molten metal and reacted for 2-8 minutes; the refined molten metal is poured.

[0016] Furthermore, when preparing high-performance copper, electrolytic copper with a copper content of more than 99.5% is added, and after melting, it is oxidized with an oxygenating tube for 5-10 minutes, degassed with dry inert gas for 10-20 minutes, and then the composition is tested and a refining agent is added.

[0017] The present invention provides high-performance copper or copper alloy, and the high-performance copper or copper alloy is prepared by the above-mentioned preparation method.

[0018] The beneficial effects brought by the technical solution provided by the embodiment of the present invention include:

[0019] 1. The conductivity of copper and copper alloys is improved by deoxidation. Compared with the original components, the conductivity attenuation does not exceed 1%. The melting point of boron is as high as 2300℃, but the melting point of its oxide is only 460℃. Compared with other deoxidizing materials, its dosage is very small, usually 0.3 parts per thousand, but it is effective enough. When the content of boron in the molten metal reaches 0.015%, it will change the conductivity of the material. The deoxidation effect of B is equivalent to 1.7-2 times of metallic lithium and phosphorus and 3.5 times of magnesium. Mg is used as a deoxidizer more than boron. Its metal activity is strong and it forms magnesium oxide with oxygen in air or molten metal. The density is 3.58g / cm 3 It is easy to float, deoxidizes more quickly, is cheap, and is suitable for rapid deoxidation before pouring to ensure that the residual magnesium content in the melt is 0.05-0.09%. Any entrainment, splashing, and oxides formed by oxidation are greatly reduced, further improving the electrical conductivity of copper and copper alloys and reducing the amount of B element.

[0020] 2. The strength, elongation at break and hardness of the prepared copper and copper alloys are greatly improved. B, as an element insoluble in molten metal, has a very strong grain refining effect. Its dispersion increases the nucleation rate and refines the grains during the metal solidification process, thereby improving the comprehensive properties of the metal. Mg is more active than other elements such as Al and Zn, and will preferentially combine with oxygen to reduce the burning loss of the material and improve the high-temperature oxidation resistance of the material. For deformed copper alloys, it improves the work hardening ability of copper and copper alloys.

[0021] 3. The refining agent provided by the present invention reduces the operator's requirements for the control accuracy of the amount of refining agent added. A large amount of Mg is added to remove a large proportion of oxygen. The easy diffusibility of the B element is utilized to further improve the removal of oxygen. A trace amount of the B element refines the grain structure and synergistically improves the mechanical properties of copper and copper alloys with the Mg element. When the addition amount is 8-15% of the mass of the molten metal, the conductivity of copper and copper alloys can be attenuated within 1% and have excellent mechanical properties, thereby increasing the process window and reducing the operating pressure of the operator.

[0022] 4. Finally, the refining agent has a small density difference with copper and copper alloys. Under the action of inertia and gravity, it enters the melt to a greater depth, further improving the deoxidation ability of Mg and B in the melt and avoiding excessive Mg and even B being oxidized on the surface of the melt. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0024] Figure 1 It is a metallographic diagram of copper with eutectoid in the prior art;

[0025] Figure 2 This is a microstructure morphology diagram of the plate prepared in Example 7 of the present invention;

[0026] Figure 3 This is the microstructure morphology of the plate prepared in Comparative Example 6 of the present invention. DETAILED DESCRIPTION

[0027] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments.

[0028] A first aspect of the present invention provides a refining agent for copper and copper alloys, the refining agent consisting of B, Mg and Cu; wherein the mass ratio of B to Mg is 1:3.8-4.5; and the mass fraction of B in the refining agent does not exceed 0.4%.

[0029] The refining agent provided by the present invention only includes B and Mg elements. First, the conductivity of copper and copper alloys is improved by deoxidation. Compared with the original components, the conductivity attenuation does not exceed 1%. The melting point of boron is as high as 2300°C, but the melting point of its oxide is only 460°C. Compared with other deoxidizing materials, its dosage is very small, usually 0.3 per ten thousand, but it is effective enough. When the content of boron in the molten metal reaches 0.015%, the conductivity of the material will be changed. The deoxidation effect of B is equivalent to 1.7-2 times of metallic lithium and phosphorus and 3.5 times of magnesium dosage. Mg is used as a deoxidizer in an amount greater than boron. Its metal activity is strong, and it forms magnesium oxide with oxygen in the air or molten metal, with a density of 3.58g / cm 3 , easy to float, deoxidation is faster, the price is cheap, and it is suitable for rapid deoxidation before pouring to ensure that the residual magnesium content in the melt is 0.05-0.09%. Any air entrainment, splashing, and oxides formed by oxidation are greatly reduced, further improving the electrical conductivity of copper and copper alloys, and reducing the amount of B element; secondly, the strength, elongation at break and hardness of the prepared copper and copper alloys are greatly improved. B, as an element insoluble in molten metal, has a very strong grain refining effect. Its dispersed distribution increases the nucleation rate and refines the grains during the metal solidification process, thereby improving the comprehensive properties of the metal. The metal activity of Mg is higher than that of other elements such as Al and Zn. It will preferentially combine with oxygen, reduce the burning loss of the material, and improve the high-temperature oxidation resistance of the material. For deformed copper alloys, it improves the processing hardness of copper and copper alloys. Thirdly, the refining agent provided by the present invention reduces the operator's control accuracy requirement for the amount of refining agent added, a large amount of Mg is added, a large proportion of oxygen is removed, and the easy diffusibility of B element is utilized to further improve the removal of oxygen, and a trace amount of B element refines the grain structure and synergistically improves the mechanical properties of copper and copper alloys with Mg element. When the addition amount is 8-15% of the mass of the metal melt, the conductivity of copper and copper alloys can be attenuated within 1% and have excellent mechanical properties, which increases the process window and reduces the operating pressure of the operator; finally, the density difference between the refining agent and copper and copper alloys is not large. Under the action of inertia and gravity, the depth of entering the melt is large, which further improves the deoxidation ability of Mg and B in the melt, and avoids excessive Mg, and even B being oxidized on the surface of the melt.

[0030] Furthermore, the refining agent is prepared by Cu-B alloy and Cu-Mg alloy. The refining agent is prepared by alloy, which reduces the burning problem in the preparation process.

[0031] Furthermore, the refining agent is a particle with a Cu-B alloy core coated with a Cu-Mg alloy; the size of the particle is 5-15 mm. By coating the Cu-B alloy core with a Cu-Mg alloy, the Mg element is melted first and deoxidized on a large scale, preventing B from being over-oxidized, and failing to perform a deep deoxidation treatment after deoxidation of the Mg element, and the over-oxidation of the B element reduces the nucleation rate during the metal solidification process, and failing to cooperate with the Mg element to improve the mechanical properties of copper and copper alloys. Secondly, the particle size is limited to 5-15 mm to ensure melting within the preset time, to prevent the particle size from being too small and melting too fast, even if the Mg element has a strong reducing ability, the B element is over-consumed due to its strong diffusion ability; secondly, the average size cannot be limited to be too large, which increases the melting time of the refining agent, so that the amount of air diffused into the melt increases with time, and the consumption of the Mg element is too large. It should be pointed out that the technical solution limits the size of the particles to 5-15 mm, not the average size of 5-15 mm, that is, the size of the particles can be within 5-15 mm, can be 5-6 mm, 6-7 mm or 14-15 mm, but the size of the particles cannot be less than 5 mm or greater than 15 mm. The above sizes are obtained by screening the particles through a sieve.

[0032] The present invention also provides a method for preparing the above-mentioned refining agent, comprising:

[0033] S1: The Cu-Mg alloy and the Cu-B alloy are crushed and sieved, and a certain proportion of Cu-Mg alloy powder and Cu-B alloy particles meeting the particle size requirements are weighed according to the proportion.

[0034] The pulverizing process is to ball-mill the Cu-Mg alloy and the Cu-B alloy by a ball mill. The amount of the Cu-Mg alloy and the Cu-B alloy is not limited here, and they only need to be pulverized. Even if the Cu-B alloy particles have edges and corners, they are partially oxidized in advance during the oxidation process, but the amount of oxidation is small, and the subsequent deep deoxidation and grain refinement requirements are still met. The pulverizing preferably uses a ball mill. The ball milling process can grind the edges and corners of the alloy particles, so that the Cu-Mg alloy powder and the Cu-B alloy particles are more spherical, so as to reduce the probability of the B element being oxidized in advance.

[0035] The ball milling process is as follows: the rotation speed is 300-500r / min, the ball milling time is at least 20min, and the material-ball ratio is 1:1.5-2.0.

[0036] In the screening process, Cu-B alloy particles with a particle size of 1-5 mm are screened out, and Cu-Mg alloy powder with a particle size less than 15 μm is screened out. Screening can be performed by a sieve, for example, the mesh size of the first sieve is 5 mm, and Cu-B alloy particles with a size greater than 5 mm are screened out, and the mesh size of the second sieve is 1 mm, and Cu-B alloy particles with a size less than 1 mm are screened out to obtain Cu-B alloy particles with a particle size of 1-5 mm. Cu-Mg alloy powder is screened out with a particle size of not less than 15 μm, so that the Cu-Mg alloy powder can be bonded to the Cu-B alloy particles.

[0037] S2: a predetermined mass of Cu-Mg alloy powder is bonded to the Cu-B alloy particles, and then dried and sintered.

[0038] A predetermined mass of Cu-Mg alloy powder is bonded to Cu-B alloy particles, including spraying an organic binder on the Cu-B alloy particles and then mixing and sieving the Cu-Mg alloy powder, repeating the above process until the mass ratio of the bonded Cu-Mg alloy powder to the Cu-B alloy particles meets the requirements, and then drying and sintering are performed.

[0039] The organic binder in the present application is a volatile organic substance, such as formaldehyde, ethanol, etc., which will not produce C residue in the matrix after volatilization, thereby reducing the amount of oxygen penetration.

[0040] Specifically, the Cu-B alloy particles are placed on a sieve, an organic binder is sprayed, and then Cu-Mg alloy powder is sprinkled on the Cu-B alloy particles. The sieve is shaken, and excess Cu-Mg alloy powder is sieved out through the sieve. The spraying of the organic binder and the sprinkling of the Cu-Mg alloy powder are repeated until the desired ratio is reached.

[0041] Specifically, the required ratio is calculated in the following manner: first determine the mass of the Cu-B alloy particles, calculate the total mass of the Cu-Mg alloy powder minus the mass removed by the sieve, and obtain the mass of the Cu-Mg alloy powder bonded to the Cu-B alloy particles. If the mass of the Cu-B alloy particles and the mass of the bonded Cu-Mg alloy powder meet the above ratio requirement, the process ends.

[0042] The drying process is: keeping the temperature at 100-200°C for at least 5 minutes;

[0043] The sintering process is: sintering at 900-1000° C. for 10-30 minutes in a vacuum or inert gas atmosphere.

[0044] S3: the sintered product is crushed and sieved.

[0045] The frequency during the vibration process does not exceed 50Hz, and particles with a size greater than 15mm and less than 5mm are screened out.

[0046] The present invention also provides a method for preparing high-performance copper or copper alloy, comprising:

[0047] S10: weigh the material according to the element ratio of copper or copper alloy and heat it to a temperature not exceeding 120° C. of the melting point and keep it warm until the material is completely melted.

[0048] S20: adding the above refining agent or the refining agent prepared by the above preparation method, wherein the amount of the refining agent added is 8-15% of the mass of the metal melt and reacting for 2-8 minutes;

[0049] S30 is to pour the refined molten metal.

[0050] Specifically, when preparing high-performance copper, electrolytic copper with a copper content of more than 99.5% is added, and after melting, it is oxidized with an oxygenating tube for 5-10 minutes, degassed with dry inert gas for 10-20 minutes, and then the composition is tested and a refining agent is added. It can be seen that the present application reduces the requirements for the quality of pure copper, and still has a good effect when pure copper with more impurities is used to prepare pure copper.

[0051] The present invention also provides a high-performance copper or copper alloy, wherein the high-performance copper or copper alloy is prepared by the above-mentioned preparation method.

[0052] In order to better illustrate the embodiments of the present invention, the present invention is further described in detail below through specific examples.

[0053] Example 1

[0054] The embodiment of the present invention provides a method for preparing high-performance copper, the size of which is 1500*500*50mm, the smelting equipment is: medium-frequency coreless induction furnace + graphite crucible, the ingredients are: electrolytic copper with a copper content of 99.5%, all materials are cut into small pieces as much as possible, and the smelting aid is: a graphite-based covering agent. It includes:

[0055] S10 first adds dry electrolytic copper to fill the entire furnace, leaving as little space as possible. Start smelting, when the raw materials are red hot or after low-temperature power supply for 30 minutes, add covering agent for smelting, the thickness of the covering layer is about 10cm, smelt as quickly as possible, heat to 1180℃ and keep warm until all materials are completely melted into liquid.

[0056] S20: adding a refining agent in an amount of 10% of the mass of the molten metal and reacting for 2 minutes.

[0057] The preparation method of the refining agent is: Cu-B alloy and Cu-Mg alloy are prepared by melting in a vacuum environment, wherein the mass ratio of B to Mg is 1:3.8, the mass fraction of B in the refining agent is 0.4%, the mass fraction of Mg is 1.52%, and the size of the refining agent is 5-10 mm.

[0058] S30 is to pour the refined molten metal.

[0059] The furnace temperature is 1200℃, and it is poured into a ladle for slagging. The pouring temperature is about 1160℃.

[0060] The oxygen content of the melt was detected before and after the addition of the refining agent, and the conductivity of the prepared pure copper plate was measured.

[0061] Example 2

[0062] The embodiment of the present invention provides a method for preparing high-performance copper, the size of which is 1500*500*50mm, the smelting equipment is: medium-frequency coreless induction furnace + graphite crucible, the ingredients are: electrolytic copper with a copper content of 99.5%, all materials are cut into small pieces as much as possible, and the smelting aid is: a graphite-based covering agent. It includes:

[0063] S10 first adds dry electrolytic copper to fill the entire furnace, leaving as little space as possible. Start smelting, when the raw materials are red hot or after low-temperature power supply for 30 minutes, add covering agent for smelting, the thickness of the covering layer is about 10cm, smelt as quickly as possible, heat to 1180℃ and keep warm until all materials are completely melted into liquid.

[0064] S20: adding a refining agent in an amount of 8% of the mass of the molten metal and reacting for 4 minutes.

[0065] The preparation method of the refining agent is: Cu-B alloy and Cu-Mg alloy are prepared by melting in a vacuum environment, wherein the mass ratio of B to Mg is 1:4, the mass fraction of B in the refining agent is 0.3%, the mass fraction of Mg is 1.2%, and the size of the refining agent is 5-8 mm.

[0066] S30 is to pour the refined molten metal.

[0067] The furnace temperature is 1200℃, and it is poured into a ladle for slagging. The pouring temperature is about 1160℃.

[0068] The oxygen content of the melt was detected before and after the addition of the refining agent, and the conductivity of the prepared pure copper plate was measured.

[0069] Example 3

[0070] The embodiment of the present invention provides a method for preparing high-performance copper, the size of which is 1500*500*50mm, the smelting equipment is: medium-frequency coreless induction furnace + graphite crucible, the ingredients are: electrolytic copper with a copper content of 99.5%, all materials are cut into small pieces as much as possible, and the smelting aid is: a graphite-based covering agent. It includes:

[0071] S10 first adds dry electrolytic copper to fill the entire furnace, leaving as little space as possible. Start smelting, when the raw materials are red hot or after low-temperature power supply for 30 minutes, add covering agent for smelting, the thickness of the covering layer is about 10cm, smelt as quickly as possible, heat to 1180℃ and keep warm until all materials are completely melted into liquid.

[0072] S20: adding a refining agent in an amount of 15% of the mass of the molten metal and reacting for 8 minutes.

[0073] The preparation method of the refining agent is: Cu-B alloy and Cu-Mg alloy are prepared by smelting in a vacuum environment, wherein the mass ratio of B to Mg is 1:4.5, the mass fraction of B in the refining agent is 0.3%, the mass fraction of Mg is 1.35%, and the size of the refining agent is 10-15 mm.

[0074] S30 is to pour the refined molten metal.

[0075] The furnace temperature is 1200℃, and it is poured into a ladle for slagging. The pouring temperature is about 1160℃.

[0076] The oxygen content of the melt was detected before and after the addition of the refining agent, and the conductivity of the prepared pure copper plate was measured.

[0077] Example 4

[0078] Different from Example 1, in this embodiment, the preparation method of the refining agent is: ball milling and sieving the Cu-Mg alloy and the Cu-B alloy, wherein Cu-B alloy particles with a particle size of 2-3 mm are sifted out, and Cu-Mg alloy powder with a particle size less than 15 µm is sifted out, and Cu-Mg alloy powder and Cu-B alloy particles that meet the particle size requirements are weighed according to a mass ratio of B to Mg of 1:3.8; a predetermined mass of Cu-Mg alloy powder is bonded to the Cu-B alloy particles, and then dried and sintered; and the sintered product is vibrated and sieved.

[0079] The oxygen content of the melt was detected before and after the addition of the refining agent, and the conductivity of the prepared pure copper plate was measured.

[0080] Example 5

[0081] Different from Example 2, in this example, the preparation method of the refining agent is: ball milling and sieving the Cu-Mg alloy and the Cu-B alloy, wherein Cu-B alloy particles with a particle size of 1-5 mm are sifted out, and Cu-Mg alloy powder with a particle size less than 10 µm is sifted out, and Cu-Mg alloy powder and Cu-B alloy particles that meet the particle size requirements are weighed according to a mass ratio of B to Mg of 1:4; a predetermined mass of Cu-Mg alloy powder is bonded to the Cu-B alloy particles, and then dried and sintered; and the sintered product is vibrated and sieved.

[0082] The oxygen content of the melt was detected before and after the addition of the refining agent, and the conductivity of the prepared pure copper plate was measured.

[0083] Example 6

[0084] Different from Example 3, in this embodiment, the preparation method of the refining agent is: ball milling and sieving the Cu-Mg alloy and the Cu-B alloy, wherein Cu-B alloy particles with a particle size of 1-4 mm are sifted out, and Cu-Mg alloy powder with a particle size less than 15 µm is sifted out, and Cu-Mg alloy powder and Cu-B alloy particles that meet the particle size requirements are weighed according to a mass ratio of B to Mg of 1:4.5; a predetermined mass of Cu-Mg alloy powder is bonded to the Cu-B alloy particles, and then dried and sintered; and the sintered product is vibrated and sieved.

[0085] The oxygen content of the melt was detected before and after the addition of the refining agent, and the conductivity of the prepared pure copper plate was measured.

[0086] Example 7

[0087] The embodiment of the present invention provides a method for preparing high-performance ZCuAl10Fe3, with a size of 1500*500*70mm, a smelting equipment: a medium-frequency coreless induction furnace + a graphite crucible, ingredients: pure aluminum ingots, low-carbon steel sheets, the rest is electrolytic copper, and a smelting aid is cryolite powder. It includes:

[0088] S10 first adds all the aluminum ingots, and then puts low-carbon steel sheets on top of the aluminum ingots, making full use of the aluminum heat reaction to reduce the smelting temperature. The remaining space is filled with electrolytic copper materials, and the furnace is loaded without leaving any gaps. Start smelting. When the charge gradually melts, add electrolytic copper in time to avoid excessive smelting temperature. Melt as quickly as possible. After all melts, heat to 1180℃. Then degassing and refining are carried out. Dry high-purity argon or nitrogen is filled into the molten metal for 10-20 minutes, and the insulation temperature is increased to 1185℃. Samples are taken for testing and the composition is removed with cryolite powder.

[0089] S20: adding a refining agent, wherein the amount of the refining agent added is 15% of the mass of the metal melt and the reaction is continued for 2 minutes.

[0090] The preparation method of the refining agent comprises the following steps: ball milling and sieving Cu-Mg alloy and Cu-B alloy, wherein Cu-B alloy particles with a particle size of 1-5 mm are sifted out, and Cu-Mg alloy powder with a particle size of less than 15 μm is sifted out, and Cu-Mg alloy powder and Cu-B alloy particles meeting the particle size requirements are weighed according to a mass ratio of B to Mg of 1:3.8; a predetermined mass of Cu-Mg alloy powder is bonded to Cu-B alloy particles, and then dried and sintered; and the sintered product is vibrated and sieved.

[0091] S30 is to pour the refined molten metal.

[0092] The furnace temperature is 1190℃ and the pouring temperature is controlled above 1130℃.

[0093] The oxygen content of the melt before and after the addition of refining agent was detected, and its mechanical properties were measured.

[0094] The sand casting process is used to cut the prepared products, such as Figure 2 As shown, the structure is fine and uniform, without shrinkage cavities and segregation, and the grain size is small.

[0095] Example 8

[0096] The embodiment of the present invention provides a method for preparing high-performance ZCuSn5Pb5Zn5 copper, the size of which is 1500*500*100mm, the smelting equipment is: medium frequency coreless induction furnace + graphite crucible, the ingredients are: tin ingot, lead ingot, zinc ingot, the rest is electrolytic copper, all materials are cut into small pieces as much as possible, and the smelting aid is: a graphite-based covering agent. It includes:

[0097] Add zinc ingots at the bottom of S10, cover it with pure copper and recycled materials. After the zinc is melted, gradually add pure copper and remaining recycled materials, melt them all, then add tin and lead ingots, adjust the composition after all are melted, take samples to test the composition and gas content. If the gas content is too high, lower the smelting temperature to below 980 degrees Celsius to make the bubbles float up and escape, or pass argon gas for refining to quickly cool down.

[0098] S20: adding a refining agent in an amount of 15% of the mass of the molten metal and reacting for 5 minutes.

[0099] The preparation method of the refining agent comprises the following steps: ball milling and sieving Cu-Mg alloy and Cu-B alloy, wherein Cu-B alloy particles with a particle size of 1-3 mm are sifted out, and Cu-Mg alloy powder with a particle size of less than 10 μm is sifted out, and Cu-Mg alloy powder and Cu-B alloy particles meeting the particle size requirements are weighed according to a mass ratio of B to Mg of 1:4; a predetermined mass of Cu-Mg alloy powder is bonded to Cu-B alloy particles, and then dried and sintered; and the sintered product is vibrated and sieved.

[0100] S30 is to pour the refined molten metal.

[0101] The furnace temperature is 1200℃, and it is poured into a ladle for slagging. The pouring temperature is about 1100℃.

[0102] The oxygen content of the melt was measured before and after the addition of the refining agent.

[0103] Example 9

[0104] The embodiment of the present invention provides a method for preparing a brass H70 plate, the size of which is 1500*500*100mm, the smelting equipment is: a medium frequency coreless induction furnace, the ingredients are: electrolytic copper with a copper content of 99.5%, zinc ingots, the materials are cut into small pieces as much as possible, and the smelting aid is: a graphite-based covering agent. It includes:

[0105] S10 first adds dry electrolytic copper to fill the entire furnace, leaving as little space as possible. Start smelting, when the raw materials are red hot or after low-temperature power supply for 30 minutes, add zinc ingots and cover agent for smelting. The thickness of the cover layer is about 10cm. Smelt as quickly as possible, heat to 1180℃ and keep warm until everything is completely melted into liquid.

[0106] S20: adding a refining agent in an amount of 8% of the mass of the molten metal and reacting for 3 minutes.

[0107] The preparation method of the refining agent comprises the following steps: ball milling and sieving Cu-Mg alloy and Cu-B alloy, wherein Cu-B alloy particles with a particle size of 1-2 mm are sifted out, and Cu-Mg alloy powder with a particle size of less than 15 μm is sifted out, and Cu-Mg alloy powder and Cu-B alloy particles meeting the particle size requirements are weighed according to a mass ratio of B to Mg of 1:4.5; a predetermined mass of Cu-Mg alloy powder is bonded to Cu-B alloy particles, and then dried and sintered; and the sintered product is vibrated and sieved.

[0108] S30 is to pour the refined molten metal.

[0109] The furnace temperature is 1200℃, and it is poured into a ladle for slagging. The pouring temperature is about 1160℃.

[0110] The oxygen content of the melt was measured before and after the addition of the refining agent.

[0111] Comparative Example 1

[0112] Different from Example 1, in this comparative example, phosphor copper is used as a refining agent, the added amount of P in the phosphor copper is the same as the total molar amount of Mg and B, and the particle size is 5-15 mm.

[0113] The oxygen content of the melt was detected before and after the addition of the refining agent, and the conductivity of the prepared pure copper plate was measured.

[0114] Comparative Example 2

[0115] Different from Example 1, in this comparative example, the preparation method of the refining agent is: Cu-B alloy and Cu-Mg alloy are prepared by smelting in a vacuum environment, wherein the mass ratio of B to Mg is 1:3.5.

[0116] The oxygen content of the melt was detected before and after the addition of the refining agent, and the conductivity of the prepared pure copper plate was measured.

[0117] Comparative Example 3

[0118] Different from Example 1, in this comparative example, the preparation method of the refining agent is: Cu-B alloy and Cu-Mg alloy are prepared by smelting in a vacuum environment, wherein the mass ratio of B to Mg is 1:4.6.

[0119] The oxygen content of the melt was detected before and after the addition of the refining agent, and the conductivity of the prepared pure copper plate was measured.

[0120] Comparative Example 4

[0121] Different from Example 4, in this comparative example, Cu-Mg alloy powder and Cu-B alloy particles meeting the particle size requirements were weighed according to a mass ratio of B to Mg of 1:3.5.

[0122] The oxygen content of the melt was detected before and after the addition of the refining agent, and the conductivity of the prepared pure copper plate was measured.

[0123] Comparative Example 5

[0124] Different from Example 4, in this comparative example, Cu-Mg alloy powder and Cu-B alloy particles meeting the particle size requirements were weighed according to a mass ratio of B to Mg of 1:4.6, and the conductivity of the prepared pure copper plate was measured.

[0125] Comparative Example 6

[0126] Different from Example 7, in this comparative example, phosphor copper is used as a refining agent, the added amount of P in the phosphor copper is the same as the total molar amount of Mg and B, and the particle size is 5-15 mm.

[0127] The oxygen content of the melt before and after the addition of the refining agent is detected, and its mechanical properties are measured. The prepared products are cut using the sand casting process, such as Figure 3 As shown, there are pores in the structure, and the grain size is larger than that in Example 7 as can be seen by the naked eye. In the smelting of tin bronze, the use of the refining agent of this formula increases the supercooling of the components, shortens the solidification range of the material, and greatly reduces the shrinkage ratio.

[0128] The data detected by the above examples and comparative examples are shown in Table 1.

[0129] Table 1 Test data of examples and comparative examples

[0130]

[0131] It can be seen from Examples 1-3 and Examples 4-6 that the use of particles with a Cu-Mg alloy coated with a Cu-B alloy core as a refining agent can make the Cu-Mg alloy and the Cu-B alloy coordinate with each other, and cooperate to improve the ability to remove oxygen; from Example 1 and Comparative Examples 1-5, it can be seen that the deoxidation effect of P-Cu is much weaker than the combination of Cu-Mg and Cu-B in the present application, and when the element ratio of Mg to B is not appropriate, the synergistic deoxidation effect between the two is weakened.

[0132] According to the national standard GB / T1176-2013, the mechanical properties of ZCuAl10Fe3 are found, and the mechanical properties are shown in Table 2.

[0133]

[0134] It can be seen that the mechanical properties of ZCuAl10Fe3 (Example 7) prepared in the present application are far greater than those specified in the national standard, which is mainly attributed to the extremely low oxygen content, which reduces the formation of brittle phases and improves the mechanical properties of the organization. On the other hand, Mg and B temper the organization, making the grains refined and the mechanical properties enhanced.

[0135] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a refining agent, characterized in that: The refining agent is composed of B, Mg and Cu; wherein the mass ratio of B to Mg is 1:3.8-4.5; and the mass fraction of B in the refining agent does not exceed 0.4%; The refining agent is prepared by Cu-B alloy and Cu-Mg alloy; The refining agent is a particle of a Cu-B alloy core coated with a Cu-Mg alloy; the size of the particle is 5-15 mm; include: The Cu-Mg alloy and the Cu-B alloy are crushed and sieved, and Cu-Mg alloy powder and Cu-B alloy particles meeting the particle size requirements are weighed according to a proportion; A predetermined mass of Cu-Mg alloy powder is bonded to Cu-B alloy particles, and then dried and sintered; The sintered product can be crushed and sieved.

2. The preparation method according to claim 1, characterized in that: The pulverizing process is to ball mill the Cu-Mg alloy and the Cu-B alloy by a ball mill; In the screening process, Cu-B alloy particles with a particle size of 1-5 mm are screened out, and Cu-Mg alloy powder with a particle size less than 15 μm is screened out.

3. The preparation method according to claim 1, characterized in that: A predetermined mass of Cu-Mg alloy powder is bonded to Cu-B alloy particles, including spraying an organic binder on the Cu-B alloy particles and then mixing and sieving the Cu-Mg alloy powder, repeating the above process until the mass ratio of the bonded Cu-Mg alloy powder to the Cu-B alloy particles meets the requirements, and then drying and sintering are performed.

4. The preparation method according to claim 3, characterized in that: The drying process is: keeping the temperature at 100-200°C for at least 5 minutes; The sintering process is: sintering at 900-1000° C. for 10-30 minutes in a vacuum or inert gas atmosphere.

5. A method for preparing high-performance copper or copper alloy, characterized in that it comprises: Weigh the material according to the element ratio of copper or copper alloy and heat it to a temperature not exceeding 120°C of the melting point and keep it warm until the material is completely melted; Adding a refining agent prepared by the preparation method according to any one of claims 1 to 4, wherein the amount of the refining agent added is 8-15% of the mass of the metal melt and reacting for 2-8 minutes; The refined molten metal can be poured.

6. The preparation method according to claim 5, characterized in that: include: When preparing high-performance copper, electrolytic copper with a copper content of more than 99.5% is added, and after melting, it is oxidized with an oxygen-filled tube for 5-10 minutes, degassed with dry inert gas for 10-20 minutes, and then the composition is tested and refining agents are added.

7. A high performance copper or copper alloy, characterized in that: The high-performance copper or copper alloy is prepared by the preparation method described in any one of claims 5-6.