Copper substrate-molybdenum composite coating conductive wear-resistant material and preparation method thereof
Through a combination of laser cladding and embedding infiltration technology, Si-S-C-Al quaternary alloy powder is used to prepare a high-performance copper matrix-molybdenum composite coating on the surface of the copper alloy, which solves the problem of poor oxidation resistance of the molybdenum coating. , achieving high hardness, high wear resistance and improved conductivity, suitable for applications under extreme working conditions.
Patent Information
- Application Number
- CN202411036448.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-07-31
AI Technical Summary
The additive molybdenum coating on the surface of copper alloy has poor oxidation resistance, which limits its application in extreme working conditions. Existing technologies such as electroplating and thermal spraying have problems with low bonding strength and high porosity.
Using a method that combines laser cladding and embedding infiltration, Si-S-C-Al quaternary alloy powder is used to prepare a copper matrix-molybdenum composite coating with high hardness, high wear resistance, and high conductivity on the surface of the copper matrix. It is composited by red and blue light. Laser cladding technology directly prepares molybdenum coating on the surface of copper alloy, and performs embedding and infiltration treatment on the surface to form a dense compound-sulfide-carbide-aluminide cermet composite coating.
Significantly improves the comprehensive performance of the molybdenum composite coating, including hardness, wear resistance and oxidation resistance, solving the service problem of the molybdenum coating under extreme working conditions. The wear resistance is several times higher than that of the copper matrix, and the wear reduction effect is Significant improvement.
Smart Images

Figure CN118563314B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of preparing a coating on a copper substrate, and in particular to a copper substrate-molybdenum composite coating conductive wear-resistant material and a preparation method thereof. Background Art
[0002] Copper and copper alloys are widely used in aerospace, marine transportation, electronics and other fields due to their high electrical and thermal conductivity. However, due to the low hardness and poor wear resistance of copper and copper alloys, their application under extreme working conditions is greatly limited. Common copper alloy surface modification technologies include electroplating technology, thermal spraying technology and laser cladding technology. Electroplating technology faces many challenges. For example, the bonding between the metal film and the substrate is usually in a non-metallurgical state, which makes the metal film easy to peel off. At the same time, the hardness and wear resistance are poor, and the formed metal film is relatively loose. In contrast, thermal spraying technology can obtain a relatively thick coating, but the coating is only mechanically bonded to the substrate, with low bonding strength, and is prone to falling off and failure under high loads. In addition, the porosity of the thermal spray coating is high, resulting in reduced performance.
[0003] Molybdenum has many excellent properties, such as high melting point (2620℃), low electrical resistance and high thermal conductivity, high elastic modulus and small thermal expansion coefficient. Its excellent high-temperature mechanical properties have led many scholars at home and abroad to study the additive molybdenum coating on the surface of copper alloys. Due to the poor oxidation resistance of molybdenum, the service of molybdenum coating under extreme working conditions is seriously affected.
[0004] Therefore, how to add molybdenum coating on the surface of copper alloy and overcome the shortcomings of molybdenum's poor oxidation resistance is a technical problem that needs to be solved at present. Summary of the invention
[0005] The purpose of the present invention is to provide a copper substrate-molybdenum composite coating conductive wear-resistant material and a preparation method thereof. The present invention adopts a method combining laser cladding and embedding infiltration to prepare a coating with high comprehensive performance such as high hardness, high wear resistance, high conductivity and high oxidation resistance, providing a new idea for high-performance coating technology on copper surface; and the coating prepared by the present invention using Si-SC-Al quaternary alloy powder is better than the coating prepared by any of the above-mentioned metals alone. The Si-SC-Al quaternary alloy powders used in the present invention have a synergistic effect, which can significantly improve the comprehensive performance of the molybdenum composite coating, solving the technical problem of adding molybdenum coating on the surface of copper alloy and overcoming the poor oxidation resistance of molybdenum.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] The first aspect of the present invention is to provide a method for preparing a copper substrate-molybdenum composite coating conductive wear-resistant material, comprising the following steps:
[0008] Step (1): preparing a molybdenum coating on the surface of a copper substrate by laser cladding to obtain a copper substrate-molybdenum coating material;
[0009] Step (2): embedding the copper substrate-molybdenum coating material in a composite powder, and calcining under a protective atmosphere to obtain a copper substrate-molybdenum composite coating material; the composite powder comprises NaF, Al2O3 and Si-CS-Al quaternary alloy powder;
[0010] The Si-CS-Al quaternary alloy powder contains Si 10wt%~70wt%, C 10wt%~70wt%, S 10wt%~70wt%, Al 10wt%~70wt%; for example, it contains Si 10wt%, 20wt%, 30wt%, 40wt%, 50wt%, 60wt%, 70wt%; for example, it contains C 10wt%, 20wt%, 30wt%, 40wt%, 50wt%, 60wt%, 70wt%; for example, it contains S 10wt%, 20wt%, 30wt%, 40wt%, 50wt%, 60wt%, 70wt%; for example, it contains Al 10wt%, 20wt%, 30wt%, 40wt%, 50wt%, 60wt%, 70wt%;
[0011] The laser used in the laser cladding is a red-blue composite laser.
[0012] The sum of the masses of Si, C, S and Al in the Si-CS-Al quaternary alloy powder of the present invention is 100%.
[0013] The present invention adopts the red-blue light composite laser cladding technology to directly prepare a molybdenum coating on the copper surface, and then adopts the embedding infiltration technology to prepare a molybdenum compound-sulfide-carbide-aluminide metal ceramic composite coating on the surface of the molybdenum coating. The present invention adopts a method combining laser cladding and embedding infiltration to prepare a coating with high comprehensive properties such as high hardness, high wear resistance, high conductivity and high oxidation resistance, providing a new idea for high-performance coating technology on copper surface.
[0014] As a preferred embodiment, in step (1), the copper matrix is selected from at least one of a chromium-zirconium-copper alloy, a dispersion-strengthened copper alloy or a tin-bronze alloy; and / or,
[0015] In terms of mass fraction, the composite powder contains 25% to 30% NaF, 55% to 60% Al2O3, and 10% to 20% Si-CS-Al quaternary alloy powder; for example, the composite powder contains 25%, 26%, 27%, 28%, 29%, and 30% NaF; 55%, 56%, 57%, 58%, 69%, and 60% Al2O3; and 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, and 20% Si-CS-Al quaternary alloy powder;
[0016] The sum of the masses of NaF, Al2O3, and Si-CS-Al quaternary alloy powder in the composite powder of the present invention is 100%;
[0017] Preferably, the composite powder contains, by mass fraction, 25% NaF, 60% Al2O3, and 15% (Si-CS-Al) quaternary alloy powder.
[0018] As a preferred embodiment, the chromium-zirconium-copper alloy is selected from at least one of C18150 chromium-zirconium-copper, C18200 chromium-zirconium-copper, C15000 chromium-zirconium-copper, C17510 chromium-zirconium-copper or C15010 chromium-zirconium-copper; and / or,
[0019] The dispersion-strengthened copper alloy is selected from at least one of C15715 dispersion-strengthened copper, C15740 dispersion-strengthened copper, and C15760 dispersion-strengthened copper; and / or,
[0020] The tin bronze alloy is selected from at least one of C51000 tin bronze alloy, C52100 tin bronze alloy, C54400 tin bronze alloy and C90300 tin bronze alloy.
[0021] As a preferred embodiment, the laser cladding in step (1) includes the following steps:
[0022] Step (a): placing a laser head on the surface of the copper substrate to be clad;
[0023] Step (b): conveying molybdenum powder to the surface of the copper substrate to be clad;
[0024] Step (c): a laser head emits a red-blue composite laser to the surface of the copper substrate to be clad and provided with molybdenum powder, so as to prepare a molybdenum coating on the surface of the copper substrate and obtain a copper substrate-molybdenum coating material.
[0025] As a preferred embodiment, in step (a), the laser head is offset in the X-axis direction, with an angle of 80°-85° with the surface of the copper substrate to be clad; and / or,
[0026] The distance between the laser head and the surface of the copper substrate to be clad is 15mm-20mm; and / or,
[0027] Step (b), the feeding pressure of molybdenum powder is 0.5MPa~2MPa; and / or,
[0028] The feeding rate of molybdenum powder is 6-15g / min; and / or,
[0029] Step (c), in the red and blue composite laser, the infrared laser power is 3000-4500W; the blue laser power is 300-1000W; and / or, the wavelength of the blue laser is a laser beam of 420-450nm; the wavelength of the infrared laser is 700-1300nm; and / or,
[0030] The movement speed of the laser head in the X-axis direction is 14mm / s-20mm / s; and / or,
[0031] In laser cladding, the laser head adopts an I-shaped reciprocating motion.
[0032] The powder feeding method in the present invention adopts the existing commonly used powder feeding method. Preferably, the powder feeding method adopts an annular powder feeding method; the powder feeding nozzle adopts an annular powder feeding nozzle.
[0033] Laser cladding is a technology used for surface strengthening. Its principle is to use a high-density laser beam to apply high power to the substrate surface, and through the process of rapid melting and rapid cooling, a layer of metal material is clad on the body material. By controlling parameters such as laser power, scanning speed and powder speed, a good metallurgical bond between the substrate and the cladding material can be achieved, thereby significantly improving the hardness, wear resistance and oxidation resistance of the substrate. Therefore, laser cladding technology can be effectively used to prepare copper alloy surface coatings.
[0034] As a preferred embodiment, in step (2), the method for preparing Si-CS-Al quaternary alloy powder comprises the following steps:
[0035] Si powder, C powder, Al powder and S powder were ball-milled and then spray-dried to obtain Si-CS-Al quaternary alloy powder.
[0036] As a preferred embodiment, the rotation speed of the ball mill is 600r / min-1500r / min; and / or,
[0037] The ball milling time is 10h-30h; and / or,
[0038] During spray drying, the inlet temperature of the dryer is 30°C-300°C, the outlet temperature is 30°C-140°C, and the rotation speed is 2000-40000 r / min. Preferably, the inlet temperature is 200°C, the outlet temperature is 100°C, and the rotation speed is 15000 r / min.
[0039] The invention prepares Si-SC-Al mixed particle powder by ball milling and spray drying.
[0040] As a preferred embodiment, in step (2),
[0041] The calcination temperature is 950°C-1200°C; such as 950°C, 1000°C, 1050°C, 1100°C, 1150°C, 1200°C;
[0042] The roasting time is 6-8h; such as 6, 7, 8h
[0043] The calcination is carried out at -0.1MPa~-0.6MPa, such as -0.1MPa, -0.2MPa, -0.3MPa, -0.4MPa, -0.5MPa, -0.6MPa.
[0044] The second aspect of the present invention is to provide a copper substrate-molybdenum composite coating material prepared by the method described in the first aspect of the present invention.
[0045] As a preferred embodiment, in the copper substrate-molybdenum composite coating material, the surface of the copper substrate is a molybdenum composite coating, and the molybdenum composite coating includes Mo, MoSi2, MoS2, AlMo3 and MoC.
[0046] Molybdenum compounds not only improve the oxidation resistance of molybdenum coatings, but also have many excellent high-temperature mechanical properties such as high hardness, high wear resistance and high conductivity. Therefore, preparing molybdenum compounds on the surface of molybdenum coatings has become an effective means to improve the hardness, conductivity, wear resistance and ablation resistance of molybdenum coatings. Due to the poor oxidation resistance of molybdenum, the service of molybdenum coatings under extreme working conditions is seriously affected.
[0047] When preparing refractory metal molybdenum coating on copper surface, electroplating or spraying techniques will cause problems such as difficult forming, pores and poor bonding, while laser cladding can achieve metallurgical bonding of copper and refractory metals. Secondly, the existing technology for laser cladding molybdenum coating on copper alloy surface is infrared laser cladding, and the reflectivity of copper substrate to infrared laser is as high as 90%. Therefore, when laser cladding molybdenum coating on copper alloy surface, it is necessary to laser clad the transition layer on the surface of copper substrate, which makes the process complicated.
[0048] The present invention adopts red-blue light composite laser cladding technology to directly perform laser cladding on the surface of copper alloy, and uses blue light laser to open a molten pool on the surface of copper substrate, which can enhance the substrate's absorption of laser energy, and cooperates with infrared laser to directly prepare molybdenum coating on the surface of copper substrate, which simplifies the process and provides a new technical means to solve the problem of difficult forming of molybdenum coating by laser cladding on the surface of copper alloy due to the non-solid solution of copper and molybdenum.
[0049] Furthermore, on the basis of directly adopting red-blue light composite laser cladding to prepare molybdenum coating, the present invention further performs surface strengthening technology on the molybdenum coating, performs embedding infiltration on the molybdenum coating prepared by the red-blue light composite laser cladding technology, and prepares a continuous, dense, and well-bonded molybdenum compound coating on the basis of the molybdenum coating, thereby improving the comprehensive properties of the molybdenum coating such as hardness, conductivity and wear resistance, providing new ideas and technical basis for the existing research on the preparation of molybdenum coating on the surface of copper alloys, greatly improving the comprehensive properties of the existing molybdenum coating prepared on the surface of copper alloys, filling the gap in the combination of laser cladding and embedding infiltration technology for preparing molybdenum coating on the surface of copper alloys, and having very important significance for the field of copper alloy surface strengthening technology.
[0050] In summary, the present invention first uses laser cladding to prepare a high-melting-point molybdenum coating on the surface of a low-melting-point copper alloy, which can improve the performance of the joint and the overall coating, prepares a Si-SC-Al mixture by ball milling and spray drying, and then prepares a composite powder by using NaF, Al2O3 and Si-CS-Al quaternary alloy powder. Finally, based on the composite powder, a suitable embedding process is adjusted to prepare a layer of dense molybdenum compound-sulfide-carbide-aluminide metal ceramic composite coating on the surface of the copper-molybdenum coating sample to obtain a copper substrate-molybdenum composite coating material.
[0051] Compared with the prior art, the present invention has the following advantages:
[0052] The molybdenum coatings prepared in the prior art are mostly uneven and not dense. The present invention firstly adopts the red-blue composite laser cladding technology to directly prepare a continuous and dense high-melting-point, refractory alloy molybdenum coating on the surface of the copper alloy.
[0053] In order to solve the problems of poor conductivity, reduced wear resistance and poor ablation resistance caused by easy oxidation of molybdenum coating, the present invention further performs embedding infiltration treatment on the molybdenum coating, and prepares continuous and dense compounds containing MoSi2, MoS2, AlMo3 and MoC molybdenum on the surface of the molybdenum coating, thereby greatly improving the surface hardness, wear resistance, friction reduction, conductivity and ablation resistance of the coating.
[0054] In the embedding infiltration process, the present invention proposes for the first time to combine powders of four different elements into a new Si-CSA quaternary powder for embedding infiltration; and the coating prepared by the present invention using Si-SC-Al quaternary alloy powder is better than the coating prepared by any of the above-mentioned metals alone. The Si-SC-Al quaternary alloy powders used in the present invention have a synergistic effect and can significantly improve the comprehensive performance of the molybdenum composite coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0055] Figure 1 Schematic diagram of Si-SC-Al quaternary alloy powder prepared by the present invention;
[0056] Figure 2 This is a technical introduction of the combination of laser cladding and embedded infiltration of the present invention;
[0057] Figure 3 The surface morphology of the molybdenum coating after the two-step technology of laser cladding and embedded infiltration in Example 1 of the present invention;
[0058] Figure 4 It is a schematic diagram of the laser head of the present invention being offset in the X-axis direction. DETAILED DESCRIPTION
[0059] The present invention is further described in detail below through the accompanying drawings and specific embodiments.
[0060] Example 1
[0061] 1. Remove the surface oxide layer and impurities; then use anhydrous ethanol to clean the surface of the copper-based workpiece, and blow dry it with a hair dryer to obtain a copper substrate with a clean surface, and place the copper substrate on the horizontal workbench surface. Use a red and blue light laser cladding fiber laser to laser clad the copper substrate with molybdenum powder. The copper substrate used is C18150 chromium zirconium copper. The molybdenum powder is dried before cladding. The drying temperature is 120°C and the time is 1h. The powder feeding method is coaxial powder feeding.
[0062] 2. The coating preparation equipment uses a red-blue composite laser cladding system equipped with a coaxial powder feeder. The protective gas flow rate is set to 9 g / min. According to the characteristics of laser cladding, the focus of the blue laser is overlapped with the powder convergence point of the powder outlet at the minimum spot on the workpiece, and the height is measured with a vernier caliper to make iron sheets of the same length, which is convenient for determining the laser focus when repeating the laser cladding experiment later. The positive focal amount is 16mm.
[0063] 3. Place the copper substrate on the workbench, slowly move the laser head to 16mm above the copper substrate, and tilt it slightly toward the X axis (such as Figure 4As shown in the figure, horizontal X direction), the angle between the laser and the copper substrate is 85°. For the scanning speed of the Y axis, the protective gas pressure is controlled to be 0.5MPa and the powder feeding flow rate is 8g / min. After repeated experiments and comparisons, it is determined that the scanning speed in the Y axis direction is 0.25m / s, which can avoid the accumulation of powder in the Y axis and facilitate the formation of a smooth, continuous and dense cladding layer. The infrared laser power is 4300W (wavelength is 854nm) and the blue laser power is 800W (wavelength is 415 nm), the spot diameter is 1.3mm, the laser head movement speed in the X-axis direction is 15mm / s, the dried copper alloy powder is poured into the powder feeder, the local powder feeding is turned on for early powder feeding, and after observing the powder outlet, the powder feeder console is changed to external control, the infrared light and blue light water cooler are turned on, and the protective gas pressure is controlled to 0.5MPa. The controller uses the laser head to move back and forth, and the molybdenum powder delivered by the powder feeder is laser clad in an I-shaped manner with a red-blue composite blue light laser. The overlap rate in the laser cladding is 70%, and the thickness of the cladding layer is 1.2mm. The above steps are to prepare a molybdenum coating on the surface of the copper substrate by laser cladding to obtain a copper substrate-molybdenum coating material.
[0064] 4. Cut the sample with an electric spark cutter to obtain a copper-molybdenum sample (i.e., copper substrate-molybdenum coating material) with a length, width, and height of 10mm×10mm×15mm. Wash the sample in alcohol for 15 minutes, and dry the washed sample with a hair dryer for later use.
[0065] Preparation of Si-SC-Al quaternary alloy powder: Si powder, C powder, Al powder and S powder (mass ratio of 3:2:2:3) were ball-milled for 25 h at a speed of 900 r / min, and Si-CS-Al quaternary alloy powder was obtained by spray drying (its structural schematic diagram is shown in Figure 1 As shown in the figure), during spray drying, the inlet temperature of the dryer is 200℃, the outlet temperature is 100℃, and the rotation speed is 15000 r / min.
[0066] The schematic diagram of Si-SC-Al quaternary alloy powder prepared by the above steps is as follows Figure 1As shown in the figure, the powders (Si-SC-Al, NaF, Al2O3) are mixed uniformly in a mass ratio of (15:25:60) and pre-placed in a corundum crucible, the copper substrate-molybdenum coating material sample is buried in the silicon-infiltrated powder, the crucible is sealed with high-temperature resistant glue, the crucible is placed in a vacuum furnace protected by argon gas, the crucible is placed in a heating tube, the flanges on both sides of the heating tube are installed and then vacuumed, the port pressure gauge reading drops to -0.4MPa and then continues to evacuate for about 20min, then argon is introduced for atmosphere protection of the embedding process, the temperature of the vacuum furnace is adjusted to 1200℃, the insulation time is 6h, and the vacuum furnace is cooled to room temperature, the sample is taken out of the crucible to obtain a copper substrate-molybdenum composite coating material; the sample is cleaned with alcohol, and the comprehensive performance of the sample is analyzed.
[0067] The technical introduction of the combination of laser cladding and embedding infiltration of the present invention is as follows Figure 2 As shown, in the copper substrate-molybdenum coating material obtained after laser cladding of the present invention, the molybdenum coating (cladding layer) is well formed without unmelted particles and cracks. In the molybdenum composite coating treated by embedding technology, Si-SC-Al quaternary alloy powder infiltrates, decomposes and combines between molybdenum grains to form dense metal ceramic composite coatings such as MoSi2, MoS2, AlMo3 and MoC (i.e. Figure 2 The Mo compound shown in FIG. 1 is used to prepare a copper substrate-molybdenum composite coating material, wherein the surface morphology of the molybdenum composite coating is as shown in FIG. Figure 3 shown.
[0068] The molybdenum composite coating of the present invention has a high melting point, high hardness, high wear resistance and good ablation resistance, and its overall thickness is about 1.5 mm. The molybdenum composite coating has excellent wear resistance and friction reduction. The wear resistance is 5 times higher than that of the copper substrate (C18150 chromium zirconium copper), and the friction reduction effect is 2 times higher.
[0069] Example 2
[0070] 1. Remove the surface oxide layer and impurities; then use anhydrous ethanol to clean the surface of the copper-based workpiece, and blow dry it with a hair dryer to obtain a copper substrate with a clean surface, and place the copper substrate on the horizontal workbench surface. Use a red and blue light laser cladding fiber laser to laser clad the copper substrate with molybdenum powder. The copper substrate is (C18150 chromium zirconium copper) chromium zirconium copper. The molybdenum powder is dried before cladding. The drying temperature is 120°C and the time is 1h. The powder feeding method is coaxial powder feeding.
[0071] 2. The coating preparation equipment uses a red-blue composite laser cladding system equipped with a coaxial powder feeder. The protective gas flow rate is set to 9 g / min. According to the characteristics of laser cladding, the focus of the blue laser is overlapped with the powder convergence point of the powder outlet at the minimum spot on the workpiece, and the height is measured with a vernier caliper to make iron sheets of the same length, which is convenient for determining the laser focus when repeating the laser cladding experiment later. The positive focal amount is 16mm.
[0072] 3. Place the copper substrate on the workbench, slowly move the laser head to 16mm above the copper substrate, and tilt it slightly toward the X axis (such as Figure 4 As shown in the figure, horizontal X direction), the angle between the laser and the copper substrate is 85°. For the scanning speed of the Y axis, the protective gas pressure is controlled to be 0.5MPa, and repeated experiments are carried out for comparison. It is determined that the scanning speed in the Y axis direction is 0.25m / s, which can avoid the accumulation of powder in the Y axis and facilitate the formation of a flat, continuous and dense cladding layer. The infrared laser power is 4100W (wavelength is 854nm), the blue laser power is 500W (wavelength is 415nm), and the spot diameter is 1.3 mm, the laser head movement speed in the X-axis direction is 15mm / s, the dried copper alloy powder is poured into the powder feeder, the local powder feeding is turned on for early powder feeding, and after observing the powder discharge from the powder outlet, the powder feeder console is changed to external control, the infrared and blue light water coolers are turned on, and the protective gas pressure is controlled to 0.5MPa, and the powder feeding flow rate is 8g / min. The controller uses the laser head to reciprocate, and the red and blue light composite blue light laser is used to perform I-shaped laser cladding on the molybdenum powder sent by the powder feeder. The overlap rate is 70%.
[0073] 4. Cut the sample with an electric spark cutter to obtain a copper-molybdenum sample with a length, width and height of 10mm×10mm×15mm. Wash the sample in alcohol for 15 minutes, and blow dry the washed sample with a hair dryer for later use.
[0074] Preparation of Si-SC-Al quaternary alloy powder: Si powder, C powder, Al powder and S powder (mass ratio of 3:1:2:4) were ball milled for 25 hours at a speed of 800 r / min. Si-CS-Al quaternary alloy powder was obtained by spray drying. During spray drying, the inlet temperature of the dryer was 200°C, the outlet temperature was 100°C, and the rotation speed was 14000 r / min.
[0075] The schematic diagram of Si-SC-Al quaternary alloy powder prepared by the above steps is as follows Figure 1As shown in the figure, the powders (Si-SC-Al, NaF, Al2O3) are mixed uniformly in a mass ratio of (17:28:55) and pre-placed in a corundum crucible, the sample is buried in the quaternary powder, the crucible is sealed with high-temperature resistant glue, the crucible is placed in a vacuum furnace protected by argon gas, the crucible is placed in a heating tube, the flanges on both sides of the heating tube are installed and then vacuumed, the port pressure gauge reading drops to -0.4MPa and then continues to evacuate for about 20min, then argon is introduced for atmosphere protection of the embedding process, the temperature of the vacuum furnace is adjusted to 1050℃, the insulation time is 8h, and the vacuum furnace is cooled to room temperature, the sample is taken out of the crucible to obtain a copper matrix-molybdenum composite coating material; the sample is cleaned with alcohol, and the comprehensive performance of the sample is analyzed.
[0076] In the copper substrate-molybdenum coating material obtained after laser cladding of the present invention, the molybdenum coating (cladding layer) is well formed without unmelted particles and cracks. In the molybdenum composite coating treated by the embedding technology, the Si-SC-Al quaternary alloy powder penetrates, decomposes and combines between the molybdenum grains to generate dense metal ceramic composite coatings such as MoSi2, MoS2, AlMo3 and MoC, thereby obtaining a copper substrate-molybdenum composite coating material.
[0077] The molybdenum composite coating of the present invention has a high melting point, high hardness, high wear resistance and good ablation resistance, and its overall thickness is about 1.5 mm. The molybdenum composite coating has excellent wear resistance and friction reduction. The wear resistance is 5.5 times higher than that of the copper substrate (C18150 chromium zirconium copper), and the friction reduction effect is 2.5 times higher.
[0078] Example 3
[0079] The preparation method of Example 3 is basically the same as that of Example 1, except that:
[0080] The Si-SC-Al quaternary alloy powder Si-SC-Al, NaF, and Al2O3 prepared in Example 1 were uniformly mixed in a mass ratio of (15:25:60) and pre-placed in a corundum crucible, the copper-molybdenum sample was buried in the silicon-infiltrated powder, the crucible was sealed with high-temperature resistant glue, the crucible was placed in a vacuum furnace protected by argon gas, the crucible was placed in a heating tube, the flanges on both sides of the heating tube were installed and vacuum treatment was performed, and the port pressure gauge reading dropped to -0.4MPa and then continued to evacuate for about 20min, and then argon gas was introduced to provide atmosphere protection for the embedding process, the temperature of the vacuum furnace was adjusted to 1000°C, the insulation time was 6h, and the vacuum furnace was cooled to room temperature, the sample was taken out of the crucible, the sample was cleaned with alcohol, and the comprehensive performance of the sample was analyzed.
[0081] In the copper substrate-molybdenum coating material obtained after laser cladding of the present invention, the molybdenum coating (cladding layer) is well formed without unmelted particles and cracks. In the molybdenum composite coating treated by the embedding technology, the Si-SC-Al quaternary alloy powder penetrates, decomposes and combines between the molybdenum grains to generate dense metal ceramic composite coatings such as MoSi2, MoS2, AlMo3 and MoC, thereby obtaining a copper substrate-molybdenum composite coating material.
[0082] The molybdenum composite coating of the present invention has a high melting point, high hardness, high wear resistance and good ablation resistance. The overall thickness of the overall coating is about 1.6 mm. The molybdenum composite coating has excellent wear resistance and friction reduction. The wear resistance is improved by 4.9 times compared with the copper substrate (C18150 chromium zirconium copper), and the friction reduction effect is improved by 2.4 times.
[0083] Example 4
[0084] The preparation method of Example 4 is basically the same as that of Example 1, except that:
[0085] The Si-SC-Al quaternary alloy powder Si-SC-Al, NaF, and Al2O3 prepared in Example 1 were uniformly mixed in a mass ratio of (15:25:60) and pre-placed in a corundum crucible, the copper-molybdenum sample was buried in the silicon-infiltrated powder, the crucible was sealed with high-temperature resistant glue, the crucible was placed in a vacuum furnace protected by argon gas, the crucible was placed in a heating tube, the flanges on both sides of the heating tube were installed and vacuum treatment was performed, and the port pressure gauge reading dropped to -0.4MPa and then continued to evacuate for about 20min, and then argon gas was introduced to provide atmosphere protection for the embedding process, the temperature of the vacuum furnace was adjusted to 950°C, the insulation time was 6h, and the vacuum furnace was cooled to room temperature, the sample was taken out of the crucible, the sample was cleaned with alcohol, and the comprehensive performance of the sample was analyzed.
[0086] In the copper substrate-molybdenum coating material obtained after laser cladding of the present invention, the molybdenum coating (cladding layer) is well formed without unmelted particles and cracks. In the molybdenum composite coating treated by the embedding technology, the Si-SC-Al quaternary alloy powder penetrates, decomposes and combines between the molybdenum grains to generate dense metal ceramic composite coatings such as MoSi2, MoS2, AlMo3 and MoC, thereby obtaining a copper substrate-molybdenum composite coating material.
[0087] The molybdenum composite coating of the present invention has a high melting point, high hardness, high wear resistance and good ablation resistance, and its overall thickness is about 1.4 mm. The molybdenum composite coating has excellent wear resistance and friction reduction. The wear resistance is 4.2 times higher than that of the copper substrate (C18150 chromium zirconium copper), and the friction reduction effect is 2.1 times higher.
[0088] Comparative Example 1
[0089] It adopts the same technical solution as Example 1, with the only difference being that the composite powder is replaced by Si, NaF, and Al2O3, and the proportions thereof (according to the mass ratio of 15:25:60) are the same as those in Example 1.
[0090] Further analysis of the sample prepared in Comparative Example 1 showed that the wear resistance of the coating was improved by 2.5 times compared with the copper substrate, and the friction reduction effect was improved by 0.5 times.
[0091] Comparative Example 2
[0092] It adopts the same technical solution as Example 1, with the only difference being that the composite powder is replaced by C, NaF, and Al2O3, and the proportions thereof (according to the mass ratio of 15:25:60) are the same as those in Example 1.
[0093] Further analysis of the sample prepared in Comparative Example 2 showed that the wear resistance of the coating was 2.4 times higher than that of the copper substrate, and the friction reduction effect was 0.9 times higher.
[0094] Comparative Example 3
[0095] It adopts the same technical solution as Example 1, with the only difference being that the composite powder is replaced by S, NaF, and Al2O3, and the proportions thereof (according to the mass ratio of 15:25:60) are the same as those in Example 1.
[0096] Further analysis of the sample prepared in Comparative Example 3 showed that the wear resistance of the coating was improved by 3.6 times compared with the copper substrate, and the friction reduction effect was improved by 1.2 times.
[0097] Comparative Example 4
[0098] It adopts the same technical solution as Example 1, with the only difference being that the composite powder is replaced by Al, NaF, and Al2O3, and the proportions thereof (according to the mass ratio of 15:25:60) are the same as those in Example 1.
[0099] Further analysis of the sample prepared in Comparative Example 4 showed that the wear resistance of the coating was 2.5 times higher than that of the copper substrate, and the friction reduction effect was 1.1 times higher.
[0100] The performance of the composite coatings prepared in the above examples and comparative examples was analyzed, and the specific results are shown in Table 1.
[0101] Table 1
[0102]
[0103] By comparing the results of Example 1 and Comparative Examples 1-4 in the above table, it can be seen that the coating prepared by the Si-SC-Al quaternary alloy powder of the present invention is better than the coating prepared by any of the above-mentioned alloys alone. There is a synergistic effect between Si, S, C, and Al in the Si-SC-Al quaternary alloy powder used in the present invention, which can significantly improve the comprehensive performance of the molybdenum composite coating.
[0104] In summary, the present invention prepares a molybdenum composite compound coating with high hardness, high melting point, good wear resistance and friction reduction, high conductivity and excellent anti-ablation performance on the surface of the copper alloy.
[0105] The above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A method for preparing a copper substrate-molybdenum composite coating conductive wear-resistant material, characterized in that: The following steps are involved: Step (1): preparing a molybdenum coating on the surface of a copper substrate by laser cladding to obtain a copper substrate-molybdenum coating material; Step (2): embedding the copper substrate-molybdenum coating material in a composite powder, and calcining under a protective atmosphere to obtain a copper substrate-molybdenum composite coating material; the composite powder comprises NaF, Al2O3 and Si-CS-Al quaternary alloy powder; The Si-CS-Al quaternary alloy powder contains Si 10wt%~70wt%, C 10wt%~70wt%, S 10wt%~70wt%, Al10wt%~70wt%; In terms of mass fraction, the composite powder contains 25% to 30% NaF, 55% to 60% Al2O3, and 10% to 20% Si-CS-Al quaternary alloy powder; The laser cladding in step (1) includes the following steps: Step (a): placing a laser head on the surface of the copper substrate to be clad; Step (b): conveying molybdenum powder to the surface of the copper substrate to be clad; Step (c): a laser head emits a red-blue composite laser to the surface of the copper substrate to be clad and provided with molybdenum powder, so as to prepare a molybdenum coating on the surface of the copper substrate, thereby obtaining a copper substrate-molybdenum coating material; In step (a), the laser head is offset in the X-axis direction, with an angle of 80°-85° with the surface of the copper substrate to be clad; The distance between the laser head and the surface of the copper substrate to be clad is 15mm-20mm; Step (b), the powder feeding gas pressure of the molybdenum powder is 0.5MPa~2MPa; The feeding rate of molybdenum powder is 6-15 g / min; Step (c), the laser used in the laser cladding is a red-blue composite laser, in which the infrared laser power is 3000-4500W; the blue laser power is 300-1000W; the wavelength of the blue laser is a laser beam of 420-450nm; and the wavelength of the infrared laser is 700-1300nm; The movement speed of the laser head in the X-axis direction is 14mm / s-20mm / s; In laser cladding, the laser head adopts an I-shaped reciprocating motion; In step (2), The calcination temperature is 1000°C-1200°C; The roasting time is 6-8h; The calcination is carried out at -0.1MPa~-0.6MPa.
2. The method for preparing the copper substrate-molybdenum composite coating conductive wear-resistant material according to claim 1, characterized in that: In step (1), the copper matrix is selected from at least one of a chromium-zirconium-copper alloy, a dispersion-strengthened copper alloy or a tin-bronze alloy.
3. The method for preparing the copper substrate-molybdenum composite coating conductive wear-resistant material according to claim 2, characterized in that: The chromium zirconium copper alloy is selected from at least one of C18150 chromium zirconium copper, C18200 chromium zirconium copper, C15000 chromium zirconium copper, C17510 chromium zirconium copper or C15010 chromium zirconium copper; and / or, The dispersion-strengthened copper alloy is selected from at least one of C15715 dispersion-strengthened copper, C15740 dispersion-strengthened copper, and C15760 dispersion-strengthened copper; and / or, The tin bronze alloy is selected from at least one of C51000 tin bronze alloy, C52100 tin bronze alloy, C54400 tin bronze alloy and C90300 tin bronze alloy.
4. The method for preparing the copper substrate-molybdenum composite coating conductive wear-resistant material according to claim 1, characterized in that: In step (2), the method for preparing Si-CS-Al quaternary alloy powder comprises the following steps: Si powder, C powder, Al powder and S powder were ball-milled and then spray-dried to obtain Si-CS-Al quaternary alloy powder.
5. The method for preparing the copper substrate-molybdenum composite coating conductive wear-resistant material according to claim 4, characterized in that: The rotation speed of the ball mill is 600r / min-1500r / min; and / or, The ball milling time is 10h-30h; and / or, During spray drying, the air inlet temperature of the dryer is 30℃-300℃, the air outlet temperature is 30℃-140℃, and the rotation speed is 2000-40000 r / min.
6. A copper substrate-molybdenum composite coating material prepared by the method according to any one of claims 1 to 5.
7. The copper substrate-molybdenum composite coating material according to claim 6, characterized in that: In the copper substrate-molybdenum composite coating material, the surface of the copper substrate is a molybdenum composite coating, and the molybdenum composite coating includes Mo, MoSi2, MoS2, AlMo3 and MoC.