A kind of epoxy resin positive photoresist based on alkali deactivation mechanism and preparation method

By using an epoxy resin positive photoresist based on an alkali deactivation mechanism in the photoresist, combined with high-toughness modified epoxy resin and specific components, the problems of insufficient sensitivity and stability of traditional photoresists are solved. It achieves high toughness and chemical stability, meeting the needs of high-precision photolithography.

CN118567184BActive Publication Date: 2024-10-29SUNTIFIC MATERIALS WEIFANG LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411041212.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-10-29
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

Traditional positive photoresists have shortcomings in sensitivity and stability, making it difficult to meet the needs of high-precision photolithography.

Method used

Using an epoxy resin positive photoresist based on an alkali deactivation mechanism, through the use of high-toughness modified epoxy resin, solvent components, alkaline catalyst components and photoacid generator components, through specific preparation steps and composition ratios , forming a photoresist with high toughness and chemical stability.

Benefits of technology

Significantly improves the sensitivity and stability of the photoresist, enhances the interaction between molecular chains, improves impact resistance and chemical resistance, ensures the reliability and stability of the photoresist in high temperature environments, and can form high-temperature Quality positive images.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118567184B_ABST
    Figure CN118567184B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of photoresists, and in particular to an epoxy resin positive photoresist based on an alkali deactivation mechanism and a preparation method thereof. The high-toughness modified epoxy resin prepared by the invention has better toughness, and the modifier can react effectively with the epoxy resin to enhance the interaction between molecular chains, thereby significantly improving the mechanical properties of the material such as impact resistance and tensile strength, and can effectively protect the photoresist from scratching and chemical erosion during the manufacturing process; secondly, the epoxy resin positive photoresist based on the alkali deactivation mechanism provided by the invention, after being made into a photoresist film, the alkaline catalyst component in the non-exposed area can catalyze the epoxy resin to undergo a cross-linking reaction, thereby making it insoluble in a developer, and after the exposed area is exposed to ultraviolet light, a photoacid generator generates a compound that reacts with the alkaline catalyst to deactivate the epoxy resin and no longer catalyzes the cross-linking reaction, and the film can form a positive image after being developed with a developer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of photoresists, and in particular to an epoxy resin positive photoresist based on an alkali deactivation mechanism and a preparation method thereof. Background Art

[0002] Traditional photoresist materials mainly include two categories: negative photoresist and positive photoresist. After exposure, the negative photoresist undergoes a chemical reaction in the exposed area, reducing its solubility, while the non-exposed area remains intact. The desired pattern can be obtained through development. However, negative photoresists have disadvantages such as low resolution and poor contrast, and it is difficult to meet the needs of high-precision lithography. Negative photoresist is a negative chemically amplified photoresist with a wide thickness range that can achieve high aspect ratio and high sidewall verticality. It is now widely used in MEMS, microfluidics and other fields. However, this type of photoresist usually includes epoxy resin, photoacid generator, additives, solvents, etc. When exposed, the photoacid generator generates acid, and the acid catalyzes the epoxy resin to undergo a cross-linking reaction during baking. Due to the reaction mechanism, this type of photoresist can only be made negative, which limits its own application and cannot meet customers' needs for positive images.

[0003] Positive photoresist is the opposite. Its exposed area undergoes chemical reaction after exposure, and its solubility increases, while the non-exposed area remains unchanged. Positive photoresist has high resolution and contrast, so it has been widely used in the field of high-precision lithography. However, traditional positive photoresist still has shortcomings in sensitivity and stability. In order to solve the problems of traditional positive photoresist, researchers began to explore new positive photoresist materials based on alkali deactivation mechanism. Epoxy resin, as a polymer material with excellent chemical stability and physical properties, is widely used in the fields of coatings, adhesives, composite materials, etc. In recent years, with the continuous development of epoxy resin modification technology, its application in the field of photoresist has gradually attracted attention. Therefore, how to improve the preparation method of existing photoresist so that it can have better sensitivity and stability has become a technical problem to be solved by those skilled in the art. Summary of the invention

[0004] Technical issues solved

[0005] In view of the above-mentioned shortcomings of the prior art, the present invention provides an epoxy resin positive photoresist based on an alkali deactivation mechanism and a preparation method thereof, which can effectively solve the problems of poor sensitivity and stability of the photoresist in the prior art.

[0006] Technical Solution

[0007] To achieve the above objectives, the present invention is implemented through the following technical solutions:

[0008] An epoxy resin positive photoresist based on an alkali deactivation mechanism, the epoxy resin positive photoresist based on an alkali deactivation mechanism comprises: a high-toughness modified epoxy resin, a solvent component, an alkaline catalyst component and a photoacid generator component;

[0009] The high-toughness modified epoxy resin is prepared by modifying the epoxy resin with 2,2-bis[4-(3-carboxylphthalimide phenoxy)phenyl]propane.

[0010] Furthermore, the preparation steps of the 2,2-bis[4-(3-carboxyphthalimidophenoxy)phenyl]propane are:

[0011] Step 2.1, pour 2-3g of 2,2-bis[4-(4-aminophenoxy)phenyl]propane and 25-28g of N,N-dimethylacetamide into a flask, stir and dissolve at room temperature, then add 1-2g of trimellitic anhydride, stir evenly, and record the result as a mixed component;

[0012] Step 2.2, add 3 times the weight of toluene to the mixed components, heat and reflux to remove water, and react at a constant temperature of 48°C for 3-4 hours. After the reaction is completed, remove the toluene by rotary evaporation, and the result is recorded as a mixed system;

[0013] Step 2.3, pour the mixed system into ice water and let it stand and cool until solid precipitates. The obtained solid is filtered and then dried. The solid is ground through a 200-mesh sieve to obtain 2,2-bis[4-(3-carboxyphthalimidophenoxy)phenyl]propane.

[0014] Furthermore, in step 2.1, the stirring and dissolving method is stirring at a stirring speed of 500 r / min for 10 minutes, the stirring method is stirring at a stirring speed of 300 r / min for 30 minutes, the rotary evaporation temperature in step 2.2 is 52°C, and the drying method in step 2.3 is drying in an oven at 55°C for 5-6 hours.

[0015] Furthermore, the preparation steps of the high-toughness modified epoxy resin are:

[0016] Step 4.1, weigh 5-6 g of 2,2-bis[4-(3-carboxyphthalimidophenoxy)phenyl]propane and add it into a flask containing 15-18 g of N,N-dimethylacetamide, and heat and stir to obtain the first component;

[0017] Step 4.2, weigh 2-3g of carboxyl-terminated liquid nitrile rubber and 15-16g of epoxy resin, mix them, and evenly disperse them at a temperature of 100°C. The result is recorded as the second component;

[0018] Step 4.3, pour the first component into the second component at a weight ratio of 1:5, stir the reaction at 60°C for 20 minutes, then add 1-2g of 2-ethyl-4-methylimidazole, and stir at the original stirring speed for 30 minutes to obtain a high-toughness modified epoxy resin.

[0019] Furthermore, in step 4.1, the heating and stirring operation is to stir at a stirring speed of 500 r / min for 5 minutes under a 40°C water bath heating condition, in step 4.2, the method for uniform dispersion is to stir at a stirring speed of 500 r / min for 10 minutes, and in step 4.3, the stirring speed of the stirring reaction is 200 r / min.

[0020] Furthermore, the solvent component is one of ethylene glycol methyl ether, propylene glycol methyl ether, propylene glycol methyl ether acetate, ethyl acetate, ethyl lactate, γ-butyrolactone, N-methylpyrrolidone, dimethyl sulfoxide, N,N-dimethylformamide or N,N-dimethylacetamide.

[0021] Furthermore, the alkaline catalyst component is one of tetraethylammonium chloride, tetrabutylammonium chloride, tetraethylammonium tetrafluoroborate, triethanolamine, tetramethylammonium hydroxide, tetrabutylammonium hydroxide, N,N-dimethylcyclohexylamine or trioctylamine.

[0022] Furthermore, the photoacid generator component is prepared by mixing 2-methyl-4,6-bis(trichloromethyl)-1,3,5-triazine and N-hydroxynaphthaleneimide trifluoromethanesulfonate in an equal weight ratio.

[0023] A method for preparing an epoxy resin positive photoresist based on an alkali deactivation mechanism, the preparation method comprising: weighing 10-70 parts of a high-toughness modified epoxy resin, 30-90 parts of a solvent component, 0.5-10 parts of an alkaline catalyst component and 0.5-10 parts of a photoacid generator component in parts by weight, mixing the mixture, stirring the mixture at a stirring speed of 400-500 r / min for 10 minutes, and then filtering the mixture to obtain the epoxy resin positive photoresist based on the alkali deactivation mechanism.

[0024] Furthermore, the filtration treatment method is to filter with a filter membrane with a pore size of 0.2 μm.

[0025] Beneficial Effects

[0026] The present invention provides an epoxy resin positive photoresist based on an alkali deactivation mechanism and a preparation method thereof. Compared with the prior art, the present invention has the following beneficial effects:

[0027] The invention uses 2,2-bis[4-(3-carboxyphthalimidophenoxy)phenyl]propane prepared by using 2,2-bis[4-(4-aminophenoxy)phenyl]propane and N,N-dimethylacetamide as raw materials to modify epoxy resin, so that the prepared high-toughness modified epoxy resin has better toughness. The modifier can react effectively with the epoxy resin to enhance the interaction between molecular chains, thereby significantly improving the mechanical properties of the material such as impact resistance and tensile strength. The modified epoxy resin has good wear resistance and chemical resistance, thereby effectively protecting the photoresist from scratching and chemical erosion during the manufacturing process. Secondly, the modified epoxy resin has good thermal stability and chemical stability, can withstand high-temperature processing and use environment, and can make the prepared photoresist have higher reliability and stability during the microelectronic manufacturing process.

[0028] The epoxy resin positive photoresist based on the alkali deactivation mechanism provided by the present invention has the following characteristics: after being made into a photoresist film, the alkaline catalyst component in the non-exposed area can catalyze the epoxy resin to undergo a cross-linking reaction, thereby making it insoluble in a developer; after the exposed area is exposed to ultraviolet light, a photoacid generator generates a compound that reacts with the alkaline catalyst to deactivate it and no longer catalyzes the cross-linking reaction; and after the film is developed with a developer, a positive image can be formed. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the prior art descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0030] Figure 1 This is an experimental diagram of the SEM test results of Example 1 in the performance test of the present invention;

[0031] Figure 2 This is an experimental diagram of the SEM test results of Example 2 in the performance test of the present invention;

[0032] Figure 3 This is an experimental diagram of the SEM test results of Example 3 in the performance test of the present invention;

[0033] Figure 4 This is an experimental diagram of the SEM test results of Example 4 in the performance test of the present invention;

[0034] Figure 5 This is an experimental diagram of the SEM test results of the comparative example in the performance test of the present invention; DETAILED DESCRIPTION

[0035] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] The present invention will be further described below in conjunction with the embodiments.

[0037] Example 1

[0038] The present embodiment provides an epoxy resin positive photoresist based on an alkali deactivation mechanism, wherein the epoxy resin positive photoresist based on an alkali deactivation mechanism comprises: a high-toughness modified epoxy resin, a solvent component, an alkaline catalyst component, and a photoacid generator component;

[0039] The high-toughness modified epoxy resin is prepared by modifying the epoxy resin with 2,2-bis[4-(3-carboxyphthalimide phenoxy)phenyl]propane.

[0040] Wherein, the preparation steps of 2,2-bis[4-(3-carboxyphthalimidophenoxy)phenyl]propane are:

[0041] Step 2.1, pour 2 g of 2,2-bis[4-(4-aminophenoxy)phenyl]propane and 25 g of N,N-dimethylacetamide into a flask, stir at room temperature at a stirring speed of 500 r / min for 10 min, then add 1 g of trimellitic anhydride, stir at a stirring speed of 300 r / min for 30 min, and the result is recorded as a mixed component;

[0042] Step 2.2, add 3 times the weight of toluene to the mixed components, heat and reflux to remove water, and react at a constant temperature of 48°C for 3 hours. After the reaction, remove the toluene by rotary evaporation at 52°C, and the result is recorded as a mixed system;

[0043] Step 2.3, pour the mixed system into ice water and let it stand and cool until solid precipitates. The obtained solid is filtered and dried in an oven at 55°C for 5 hours. The solid is ground through a 200-mesh sieve to obtain 2,2-bis[4-(3-carboxyphthalimidophenoxy)phenyl]propane.

[0044] The preparation steps of high toughness modified epoxy resin are:

[0045] Step 4.1, weigh 5 g of 2,2-bis[4-(3-carboxyphthalimidophenoxy)phenyl]propane and add it into a flask containing 15 g of N,N-dimethylacetamide, and stir it at a stirring speed of 500 r / min for 5 min in a water bath at 40°C to obtain the first component;

[0046] Step 4.2, weigh 2 g of carboxyl-terminated liquid nitrile rubber and 15 g of epoxy resin, mix them, stir them at a temperature of 100° C. and a stirring speed of 500 r / min for 10 min, and the resultant is recorded as the second component;

[0047] Step 4.3, pour the first component into the second component at a weight ratio of 1:5, stir the mixture at 60°C and 200 r / min for 20 min, then add 1 g of 2-ethyl-4-methylimidazole, and stir at the original stirring speed for 30 min to obtain a high-toughness modified epoxy resin.

[0048] The solvent component is propylene glycol methyl ether acetate.

[0049] The alkaline catalyst component is tetrabutylammonium chloride.

[0050] The photoacid generator component is prepared by mixing 2-methyl-4,6-bis(trichloromethyl)-1,3,5-triazine and N-hydroxynaphthaleneimide trifluoromethanesulfonate in an equal weight ratio.

[0051] A method for preparing an epoxy resin positive photoresist based on an alkali deactivation mechanism, the preparation method comprising: weighing 10 parts of a high-toughness modified epoxy resin, 90 parts of a solvent component, 0.5 parts of an alkaline catalyst component and 10 parts of a photoacid generator component in parts by weight, mixing the mixture, stirring the mixture at a stirring speed of 400 r / min for 10 minutes, and filtering the mixture with a filter membrane having a pore size of 0.2 μm to obtain the epoxy resin positive photoresist based on the alkali deactivation mechanism.

[0052] Example 2

[0053] The present embodiment provides an epoxy resin positive photoresist based on an alkali deactivation mechanism, wherein the epoxy resin positive photoresist based on an alkali deactivation mechanism comprises: a high-toughness modified epoxy resin, a solvent component, an alkaline catalyst component, and a photoacid generator component;

[0054] The high-toughness modified epoxy resin is prepared by modifying the epoxy resin with 2,2-bis[4-(3-carboxyphthalimide phenoxy)phenyl]propane.

[0055] Wherein, the preparation steps of 2,2-bis[4-(3-carboxyphthalimidophenoxy)phenyl]propane are:

[0056] Step 2.1, pour 3 g of 2,2-bis[4-(4-aminophenoxy)phenyl]propane and 28 g of N,N-dimethylacetamide into a flask, stir at room temperature at a stirring speed of 500 r / min for 10 min, then add 2 g of trimellitic anhydride, stir at a stirring speed of 300 r / min for 30 min, and the result is recorded as a mixed component;

[0057] Step 2.2, add 3 times the weight of toluene to the mixed components, heat and reflux to remove water, and react at a constant temperature of 48°C for 4 hours. After the reaction, remove the toluene by rotary evaporation at 52°C. The result is recorded as a mixed system;

[0058] Step 2.3, pour the mixed system into ice water and let it stand and cool until solid precipitates. The obtained solid is filtered and dried in an oven at 55°C for 6 hours. The solid is ground through a 200-mesh sieve to obtain 2,2-bis[4-(3-carboxyphthalimidophenoxy)phenyl]propane.

[0059] The preparation steps of high toughness modified epoxy resin are:

[0060] Step 4.1, weigh 6 g of 2,2-bis[4-(3-carboxyphthalimidophenoxy)phenyl]propane and add it into a flask containing 18 g of N,N-dimethylacetamide, and stir it at a stirring speed of 500 r / min for 5 min in a water bath at 40°C to obtain the first component;

[0061] Step 4.2, weigh 3 g of carboxyl-terminated liquid nitrile rubber and 16 g of epoxy resin, mix them, stir them at a temperature of 100° C. and a stirring speed of 500 r / min for 10 min, and the resultant is recorded as the second component;

[0062] Step 4.3, pour the first component into the second component at a weight ratio of 1:5, stir the mixture at 60°C and 200 r / min for 20 min, then add 2 g of 2-ethyl-4-methylimidazole, and stir at the original stirring speed for 30 min to obtain a high-toughness modified epoxy resin.

[0063] The solvent component is propylene glycol methyl ether.

[0064] The alkaline catalyst component is tetramethylammonium hydroxide.

[0065] The photoacid generator component is prepared by mixing 2-methyl-4,6-bis(trichloromethyl)-1,3,5-triazine and N-hydroxynaphthaleneimide trifluoromethanesulfonate in an equal weight ratio.

[0066] A preparation method of an epoxy resin positive photoresist based on an alkali deactivation mechanism, the preparation method comprising: weighing 70 parts of a high-toughness modified epoxy resin, 30 parts of a solvent component, 10 parts of an alkaline catalyst component and 0.5 parts of a photoacid generator component in parts by weight, mixing the mixture, stirring the mixture at a stirring speed of 500 r / min for 10 minutes, and filtering the mixture with a filter membrane having a pore size of 0.2 μm to obtain the epoxy resin positive photoresist based on the alkali deactivation mechanism.

[0067] Example 3

[0068] The present embodiment provides an epoxy resin positive photoresist based on an alkali deactivation mechanism, wherein the epoxy resin positive photoresist based on an alkali deactivation mechanism comprises: a high-toughness modified epoxy resin, a solvent component, an alkaline catalyst component, and a photoacid generator component;

[0069] The high-toughness modified epoxy resin is prepared by modifying the epoxy resin with 2,2-bis[4-(3-carboxyphthalimide phenoxy)phenyl]propane.

[0070] Wherein, the preparation steps of 2,2-bis[4-(3-carboxyphthalimidophenoxy)phenyl]propane are:

[0071] Step 2.1, pour 3 g of 2,2-bis[4-(4-aminophenoxy)phenyl]propane and 27 g of N,N-dimethylacetamide into a flask, stir at room temperature at a stirring speed of 500 r / min for 10 min, then add 2 g of trimellitic anhydride, stir at a stirring speed of 300 r / min for 30 min, and the result is recorded as a mixed component;

[0072] Step 2.2, add 3 times the weight of toluene to the mixed components, heat and reflux to remove water, and react at a constant temperature of 48°C for 4 hours. After the reaction, remove the toluene by rotary evaporation at 52°C. The result is recorded as a mixed system;

[0073] Step 2.3, pour the mixed system into ice water and let it stand and cool until solid precipitates. The obtained solid is filtered and dried in an oven at 55°C for 5 hours. The solid is ground through a 200-mesh sieve to obtain 2,2-bis[4-(3-carboxyphthalimidophenoxy)phenyl]propane.

[0074] The preparation steps of high toughness modified epoxy resin are:

[0075] Step 4.1, weigh 5 g of 2,2-bis[4-(3-carboxyphthalimidophenoxy)phenyl]propane and add it into a flask containing 17 g of N,N-dimethylacetamide, and stir it at a stirring speed of 500 r / min for 5 min in a water bath at 40°C to obtain the first component;

[0076] Step 4.2, weigh 3 g of carboxyl-terminated liquid nitrile rubber and 16 g of epoxy resin, mix them, stir them at a temperature of 100° C. and a stirring speed of 500 r / min for 10 min, and the resultant is recorded as the second component;

[0077] Step 4.3, pour the first component into the second component at a weight ratio of 1:5, stir the mixture at 60°C and 200 r / min for 20 min, then add 2 g of 2-ethyl-4-methylimidazole, and stir at the original stirring speed for 30 min to obtain a high-toughness modified epoxy resin.

[0078] The solvent component is ethyl acetate.

[0079] The alkaline catalyst component is tetraethylammonium tetrafluoroborate.

[0080] The photoacid generator component is prepared by mixing 2-methyl-4,6-bis(trichloromethyl)-1,3,5-triazine and N-hydroxynaphthaleneimide trifluoromethanesulfonate in an equal weight ratio.

[0081] A method for preparing an epoxy resin positive photoresist based on an alkali deactivation mechanism, the preparation method comprising: weighing 30 parts of a high-toughness modified epoxy resin, 70 parts of a solvent component, 3 parts of an alkaline catalyst component and 7 parts of a photoacid generator component in parts by weight, mixing the mixture, stirring the mixture at a stirring speed of 500 r / min for 10 minutes, and filtering the mixture with a filter membrane having a pore size of 0.2 μm to obtain the epoxy resin positive photoresist based on the alkali deactivation mechanism.

[0082] Example 4

[0083] The present embodiment provides an epoxy resin positive photoresist based on an alkali deactivation mechanism, wherein the epoxy resin positive photoresist based on an alkali deactivation mechanism comprises: a high-toughness modified epoxy resin, a solvent component, an alkaline catalyst component, and a photoacid generator component;

[0084] The high-toughness modified epoxy resin is prepared by modifying the epoxy resin with 2,2-bis[4-(3-carboxyphthalimide phenoxy)phenyl]propane.

[0085] Wherein, the preparation steps of 2,2-bis[4-(3-carboxyphthalimidophenoxy)phenyl]propane are:

[0086] Step 2.1, pour 2 g of 2,2-bis[4-(4-aminophenoxy)phenyl]propane and 26 g of N,N-dimethylacetamide into a flask, stir at room temperature at a stirring speed of 500 r / min for 10 min, then add 2 g of trimellitic anhydride, stir at a stirring speed of 300 r / min for 30 min, and the result is recorded as a mixed component;

[0087] Step 2.2, add 3 times the weight of toluene to the mixed components, heat and reflux to remove water, and react at a constant temperature of 48°C for 3 hours. After the reaction, remove the toluene by rotary evaporation at 52°C, and the result is recorded as a mixed system;

[0088] Step 2.3, pour the mixed system into ice water and let it stand and cool until solid precipitates. The obtained solid is filtered and dried in an oven at 55°C for 6 hours. The solid is ground through a 200-mesh sieve to obtain 2,2-bis[4-(3-carboxyphthalimidophenoxy)phenyl]propane.

[0089] The preparation steps of high toughness modified epoxy resin are:

[0090] Step 4.1, weigh 6 g of 2,2-bis[4-(3-carboxyphthalimidophenoxy)phenyl]propane and add it into a flask containing 16 g of N,N-dimethylacetamide, and stir it at a stirring speed of 500 r / min for 5 min in a water bath at 40°C to obtain the first component;

[0091] Step 4.2, weigh 2 g of carboxyl-terminated liquid nitrile rubber and 15 g of epoxy resin, mix them, stir them at a temperature of 100° C. and a stirring speed of 500 r / min for 10 min, and the resultant is recorded as the second component;

[0092] Step 4.3, pour the first component into the second component at a weight ratio of 1:5, stir the mixture at 60°C and 200 r / min for 20 min, then add 2 g of 2-ethyl-4-methylimidazole, and stir at the original stirring speed for 30 min to obtain a high-toughness modified epoxy resin.

[0093] The solvent component is N,N-dimethylformamide.

[0094] The alkaline catalyst component is tetrabutylammonium hydroxide.

[0095] The photoacid generator component is prepared by mixing 2-methyl-4,6-bis(trichloromethyl)-1,3,5-triazine and N-hydroxynaphthaleneimide trifluoromethanesulfonate in an equal weight ratio.

[0096] A method for preparing an epoxy resin positive photoresist based on an alkali deactivation mechanism, the preparation method comprising: weighing 50 parts of a high-toughness modified epoxy resin, 40 parts of a solvent component, 6 parts of an alkaline catalyst component and 4 parts of a photoacid generator component in parts by weight, mixing the mixture, stirring the mixture at a stirring speed of 500 r / min for 10 minutes, and filtering the mixture with a filter membrane having a pore size of 0.2 μm to obtain the epoxy resin positive photoresist based on the alkali deactivation mechanism.

[0097] Comparative Example

[0098] The epoxy resin positive photoresist based on the alkali deactivation mechanism and the preparation method provided in this comparative example are substantially the same as those in Example 1, with the main difference being that the high-toughness modified epoxy resin in Example 1 is replaced with an unmodified epoxy resin in this comparative example.

[0099] Performance Testing

[0100] The epoxy resin positive photoresists based on the alkali deactivation mechanism in Examples 1-4 and the comparative example were spin-coated on the treated substrates respectively, and then pre-baked at 100°C for 60s on a hot plate, and the rotation speed was adjusted so that the film thickness after drying was 0.75μm. The standard L / S=1:1 detection mask was passed through an exposure machine at 365nm, and then baked at 130°C for 60s on a hot plate, and then immersed in propylene glycol methyl ether acetate for development for 60s. After washing with isopropyl alcohol and deionized water respectively, the photolithography process was completed, and positive photoresist images were obtained.

[0101] In the performance test, the minimum exposure amount to obtain 0.5μm1:1 equal-spaced graphics is used to represent photosensitivity; the minimum line width is found, sliced ​​for SEM testing, and its size, which is the resolution; observation is made with an electron microscope according to the following criteria: good means that the line edge is a straight line with a narrow edge; bad means that the line edge is not a line, has a width, and a wide edge, which represents the line edge roughness, and the obtained data is recorded in the table below.

[0102]

[0103] It can be seen from the data in the above table that the photosensitivity and resolution of the epoxy resin positive photoresist based on the alkali deactivation mechanism in Examples 1-4 are better than those in the comparative example, indicating that the modified high-toughness modified epoxy resin added in the present invention can better improve the performance of the photoresist than the unmodified epoxy resin.

[0104] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.

[0105] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. An epoxy resin positive photoresist based on an alkali deactivation mechanism, characterized in that: The epoxy resin positive photoresist based on the alkali deactivation mechanism comprises: a high-toughness modified epoxy resin, a solvent component, an alkaline catalyst component and a photoacid generator component; The high-toughness modified epoxy resin is prepared by modifying the epoxy resin with 2,2-bis[4-(3-carboxyphthalimide phenoxy)phenyl]propane; The preparation steps of the 2,2-bis[4-(3-carboxyphthalimidophenoxy)phenyl]propane are as follows: Step 2.1, pour 2-3g of 2,2-bis[4-(4-aminophenoxy)phenyl]propane and 25-28g of N,N-dimethylacetamide into a flask, stir and dissolve at room temperature, then add 1-2g of trimellitic anhydride, stir evenly, and record the result as a mixed component; Step 2.2, add 3 times the weight of toluene to the mixed components, heat and reflux to remove water, and react at a constant temperature of 48°C for 3-4 hours. After the reaction is completed, remove the toluene by rotary evaporation, and the result is recorded as a mixed system; Step 2.3, pour the mixed system into ice water and let it stand and cool until solid precipitates, filter the obtained solid and dry it, grind it through a 200-mesh sieve to obtain 2,2-bis[4-(3-carboxyphthalimidophenoxy)phenyl]propane; In step 2.1, the stirring method for dissolving is 500 r / min for 10 min, and the stirring method for uniform stirring is 300 r / min for 30 min. The rotary evaporation temperature in step 2.2 is 52° C., and the drying method in step 2.3 is drying in an oven at 55° C. for 5-6 h. The preparation steps of the high-toughness modified epoxy resin are: Step 4.1, weigh 5-6 g of 2,2-bis[4-(3-carboxyphthalimidophenoxy)phenyl]propane and add it into a flask containing 15-18 g of N,N-dimethylacetamide, and heat and stir to obtain the first component; Step 4.2, weigh 2-3g of carboxyl-terminated liquid nitrile rubber and 15-16g of epoxy resin, mix them, and disperse them evenly at a temperature of 100°C. The result is recorded as the second component; Step 4.3, pour the first component into the second component at a weight ratio of 1:5, stir and react at 60°C for 20 minutes, then add 1-2g of 2-ethyl-4-methylimidazole, and stir at the original stirring speed for 30 minutes to obtain a high-toughness modified epoxy resin; The alkaline catalyst component is one of tetraethylammonium chloride, tetrabutylammonium chloride, tetraethylammonium tetrafluoroborate, triethanolamine, tetramethylammonium hydroxide, tetrabutylammonium hydroxide, N,N-dimethylcyclohexylamine or trioctylamine; The photoacid generator component is prepared by mixing 2-methyl-4,6-bis(trichloromethyl)-1,3,5-triazine and N-hydroxynaphthalimide trifluoromethanesulfonate in an equal weight ratio.

2. The epoxy resin positive photoresist based on the alkali deactivation mechanism according to claim 1, characterized in that: In step 4.1, the heating and stirring operation is to stir at a stirring speed of 500 r / min for 5 minutes under a 40°C water bath heating condition. In step 4.2, the method for uniform dispersion is to stir at a stirring speed of 500 r / min for 10 minutes. In step 4.3, the stirring speed of the stirring reaction is 200 r / min.

3. The epoxy resin positive photoresist based on the alkali deactivation mechanism according to claim 1, characterized in that: The solvent component is one of ethylene glycol methyl ether, propylene glycol methyl ether, propylene glycol methyl ether acetate, ethyl acetate, ethyl lactate, gamma-butyrolactone, N-methylpyrrolidone, dimethyl sulfoxide, N,N-dimethylformamide or N,N-dimethylacetamide.

4. A method for preparing an epoxy resin positive photoresist based on an alkali deactivation mechanism according to any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: weighing 10-70 parts of a high-toughness modified epoxy resin, 30-90 parts of a solvent component, 0.5-10 parts of an alkaline catalyst component and 0.5-10 parts of a photoacid generator component, mixing the mixture, stirring the mixture at a stirring speed of 400-500 r / min for 10 minutes, and filtering the mixture to obtain an epoxy resin positive photoresist based on an alkali deactivation mechanism.

5. The method for preparing an epoxy resin positive photoresist based on an alkali deactivation mechanism according to claim 4, characterized in that: The filtering treatment method is to filter with a filter membrane with a pore size of 0.2 μm.

Citation Information

Patent Citations

  • High-thermal-conductivity electrical insulation packaging material and preparation method thereof

    CN111234752A

  • Polyimide positive photoresist based on alkali deactivation mechanism

    CN116449651A

  • Radiation sensitive resin composition, spacer and protective film of liquid crystal display device, and method for forming the same

    KR1020090064322A