Low-temperature fast-charging negative electrode composite material for power batteries, preparation method and application thereof
By using a combination of porous graphite and metal silver in the negative electrode material of lithium-ion battery and combining the lithium salt composite shell, the problem of poor low temperature performance in the existing technology is solved, and the high electronic conductivity and energy density are improved, and the The low-temperature performance and rate performance of lithium-ion batteries.
Patent Information
- Application Number
- CN202411060603.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-05
AI Technical Summary
The existing lithium-ion battery anode materials have poor electronic conductivity, low energy density, low first-time efficiency and poor low-temperature performance under low temperature conditions, which cannot meet the market's requirements for fast charging and low-temperature energy.
Porous graphite is used as the core material, doped with conductive agent and covered with metal silver, and lithium salt composites are used as the shell material to improve the electron conductivity and lithium ion diffusion rate through specific mass ratios and preparation methods to form a stable solid electrolyte interface.
It significantly improves the electronic conductivity, energy density and first charge and discharge efficiency of lithium-ion batteries, improves low-temperature performance, and enhances rate performance and cycle stability.
Smart Images

Figure CN118572095B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium-ion batteries, and in particular to a low-temperature fast-charging negative electrode composite material for a power battery, a preparation method and an application thereof. Background Art
[0002] As the market demands for fast charging and low-temperature performance of lithium-ion batteries increase, the negative electrode materials used in lithium-ion batteries are required to have excellent charging and discharging capabilities under low-temperature conditions in order to enhance the power capacity of the battery under low-temperature conditions.
[0003] At present, the negative electrode materials used in the market mainly use artificial graphite and natural graphite as the core materials. Hard carbon or soft carbon is coated on the surface of graphite to improve the lithium ion diffusion ability of the material, but it has the following disadvantages: 1) The electronic conductivity of the core material graphite is poor; 2) The amorphous carbon coating amount (2~5wt%) of the graphite surface coating is too high, which will reduce the energy density of the negative electrode material and its initial efficiency; 3) The lithium ion diffusion rate of the negative electrode material is low at low temperature, and the low temperature performance is poor. Summary of the invention
[0004] The main purpose of the present invention is to propose a low-temperature fast-charging negative electrode composite material for power batteries, a preparation method and its application, a negative electrode material and its preparation method and application, aiming to solve the problems of poor electronic conductivity, energy density, initial efficiency and low-temperature performance of graphite in the prior art.
[0005] To achieve the above object, the present invention provides a low-temperature fast-charging negative electrode composite material for a power battery, comprising a core material and a shell material coated on the surface of the core material;
[0006] The core material includes porous graphite, a conductive agent doped in the porous graphite, and metallic silver covering the surface of the porous graphite; the average pore size of the porous graphite is 1-5 nm;
[0007] The shell material includes a lithium salt complex.
[0008] In one embodiment, the lithium salt complex includes an organic lithium salt, an inorganic lithium salt and a film-forming agent.
[0009] In one embodiment, the lithium salt complex further includes a lithium capping agent, and the lithium capping agent includes a polymer, single lithium and a conductive agent.
[0010] In one embodiment, in the low-temperature fast-charging negative electrode composite material used in the power battery, the mass ratio of the core material to the shell material is 100:(5-15); and / or,
[0011] In the core material, the mass ratio of the porous graphite, the conductive agent and the metallic silver is (90-98): (1-5): (1-5); and / or,
[0012] The mass ratio of the organic lithium salt, the inorganic lithium salt, the film-forming agent and the lithium coating agent in the lithium salt composite is (1-10): (1-10): (0.5-2): (1-3); and / or,
[0013] The mass ratio of the polymer, the elemental lithium and the conductive agent in the lithium coating agent is (10-50):10:(1-5); and / or,
[0014] The conductive agent includes at least one of carbon nanotubes and graphene; and / or,
[0015] The organic lithium salt comprises at least one of lithium difluorooxalate, lithium difluoroborate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluoroacetate, and lithium difluorooxalatoborate; and / or,
[0016] The inorganic lithium salt includes at least one of LiPF6, LiAsF6, and LiBF4; and / or,
[0017] The film-forming agent includes at least one of vinylene carbonate, vinyl sulfite, propylene sulfite, and 1,4-butyrolactone sulfonate; and / or,
[0018] The polymer includes at least one of polyalkylene carbonate, polyalkylene oxide, polyalkylsiloxane, polyalkyl acrylate, and polyalkyl methacrylate.
[0019] The present invention also provides a method for preparing a low-temperature fast-charging negative electrode composite material for a power battery, comprising the following steps:
[0020] S10, mixing a carbon source, a conductive agent, metal particles and a peroxide cross-linking agent, and performing a heat treatment under an inert gas to obtain a first porous graphite;
[0021] S20, mixing the first porous graphite with a silver ammonia solution, a surfactant and a reducing agent to perform a silver mirror reaction to obtain a second porous graphite;
[0022] S30, mixing the second porous graphite with the lithium salt complex, and drying, to obtain the low-temperature fast-charging negative electrode composite material for the power battery.
[0023] In one embodiment, in step S10:
[0024] The mass ratio of the carbon source, the conductive agent, the metal particles and the peroxide cross-linking agent is 100: (1-5): (1-5): (1-5); and / or,
[0025] The carbon source includes at least one of petroleum coke, needle coke and pitch coke; and / or,
[0026] The conductive agent includes at least one of carbon nanotubes and graphene; and / or,
[0027] The metal particles include at least one of metal nano-sodium, metal nano-potassium, and metal nano-zinc, and the particle size of the metal particles is 500-2000 nm; and / or,
[0028] The peroxidation crosslinking agent includes at least one of dibenzoyl peroxide, benzoyl peroxide, cyclohexanone peroxide, cyclohexanone peroxide paste, and lauroyl peroxide.
[0029] In one embodiment, in step S20:
[0030] The silver ammonia solution contains Ag + and OH - The molar ratio is 1:(2-3); and / or,
[0031] The mass ratio of the silver salt, the first porous graphite, the surfactant and the reducing agent in the silver ammonia solution is (5-15):100:(1-5):(25-50); and / or,
[0032] The surfactant includes at least one of sodium butylnaphthalene sulfonate, sodium aminobenzene sulfonate, sodium fatty alcohol polyoxyethylene ether sulfate, and sodium fatty amine polyoxyethylene sulfate; and / or,
[0033] The reducing agent includes at least one of formaldehyde, acetaldehyde, benzaldehyde, cinnamaldehyde and acrolein.
[0034] In one embodiment, step S30 includes: mixing the second porous graphite with an organic lithium salt, an inorganic lithium salt, a film-forming agent and a lithium coating agent, and drying to obtain the low-temperature fast-charging negative electrode composite material for the power battery;
[0035] Wherein, the preparation of the lithium coating agent comprises the following steps:
[0036] A polymer solution is obtained, and the polymer solution is mixed with single-substance lithium and a conductive agent, filtered, and the filter residue is dried to obtain a lithium coating agent.
[0037] In one embodiment, the mass ratio of the second porous graphite, the organic lithium salt, the inorganic lithium salt, the film-forming agent and the lithium coating agent is 100: (1-10): (1-10): (0.5-2): (1-3); and / or,
[0038] The mass ratio of the polymer, the elemental lithium and the conductive agent in the polymer solution is (10-50):10:(1-5).
[0039] The present invention also provides an application, in which the aforementioned low-temperature fast-charging negative electrode composite material for a power battery or the low-temperature fast-charging negative electrode composite material for a power battery prepared by the aforementioned preparation method of the low-temperature fast-charging negative electrode composite material for a power battery is applied to a lithium-ion battery.
[0040] The present invention provides a low-temperature fast-charging negative electrode composite material for a power battery, a preparation method and an application thereof. The average pore size of the porous graphite is 1-5 nm, the porous graphite has a high specific surface area and a high porosity, provides more active sites and transmission paths, and provides more attachment points for the conductive agent and the metallic silver. The conductive agent is doped in the porous graphite to enhance the connection between the porous graphites, thereby improving the conductivity and mechanical stability of the negative electrode material. The metallic silver covers the surface of the porous graphite (including the pores), the contact area between the two is large, and the silver bridges the discontinuous pore structure in the porous graphite to form an additional electron transmission channel, thereby significantly improving the overall electronic conductivity. In addition, the high conductivity of silver helps to reduce The ohmic resistance inside the low negative electrode material is reduced, and the energy loss during the charge and discharge process is reduced, thereby improving the rate performance; the lithium salt complex is a complex composed of at least one organic lithium salt and at least one inorganic lithium salt, with the lithium salt complex as the shell. The lithium salt complex can reduce the freezing point of the electrolyte, so that it maintains a low viscosity at low temperatures, and improves the diffusion coefficient of lithium ions at low temperatures, thereby reducing the internal resistance of the battery, and improving the energy density and the first charge and discharge efficiency of the negative electrode material; at the same time, the lithium salt complex can form a more stable solid electrolyte interface on the surface of the negative electrode material, improve and reduce the transmission resistance of lithium ions at the interface, and reduce the loss of lithium ions caused by defects, thereby improving the rate performance and its first efficiency. The low-temperature fast-charging negative electrode composite material used in the power battery of the present invention has high electronic conductivity, energy density and first charge and discharge efficiency, and also has good low-temperature performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0042] Figure 1 This is a scanning electron microscope image (SEM) of the low-temperature fast-charging negative electrode composite material used in the power battery in Example 4 provided by the present invention.
[0043] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0044] To make the purpose, technical scheme and advantages of the embodiment of the present invention clearer, the technical scheme in the embodiment of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiment, it is carried out according to the normal conditions or the conditions recommended by the manufacturer. If the reagents or instruments used do not specify the manufacturer, they are all conventional products that can be purchased commercially. In addition, the meaning of "and / or" appearing in the full text includes three parallel schemes, taking "A and / or B" as an example, including scheme A, or scheme B, or schemes that A and B meet at the same time. In addition, the technical schemes between the various embodiments can be combined with each other, but must be based on the ability of ordinary technicians in the field to achieve. When the combination of technical solutions is contradictory or cannot be achieved, it should be considered that the combination of such technical solutions does not exist, and is not within the scope of protection required by the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the scope of protection of the present invention.
[0045] As the market demands for fast charging and low-temperature performance of lithium-ion batteries increase, the negative electrode materials used in lithium-ion batteries are required to have excellent charging and discharging capabilities under low-temperature conditions in order to enhance the power capacity of the battery under low-temperature conditions.
[0046] At present, the negative electrode materials used in the market mainly use artificial graphite and natural graphite as the core materials. Hard carbon or soft carbon is coated on the surface of graphite to improve the lithium ion diffusion ability of the material, but it has the following disadvantages: 1) The electronic conductivity of the core material graphite is poor; 2) The coating amount of the graphite surface coating layer is too high, which will reduce the energy density of the negative electrode material and its initial efficiency; 3) The lithium ion diffusion rate of the negative electrode material is low at low temperature, and the low temperature performance is poor.
[0047] In view of this, the present invention provides a low-temperature fast-charging negative electrode composite material for a power battery, comprising a core material, and a shell material coated on the surface of the core material;
[0048] The core material includes porous graphite, a conductive agent doped in the porous graphite, and metallic silver covering the surface of the porous graphite; the average pore size of the porous graphite is 1-5 nm;
[0049] The shell material includes a lithium salt complex.
[0050] In the technical solution of the present invention, the average pore size of the porous graphite is 1-5 nm, it has a high specific surface area and a high porosity, provides more active sites and transmission paths, and provides more attachment points for the conductive agent and the metallic silver; the conductive agent is doped in the porous graphite, which enhances the connection between the porous graphites and improves the conductivity and mechanical stability of the negative electrode material; the metallic silver covers the surface of the porous graphite (including the pores), the contact area between the two is large, and the silver bridges the discontinuous pore structure in the porous graphite to form an additional electron transmission channel, which significantly improves the overall electronic conductivity; in addition, the high conductivity of silver helps to reduce the ohmic resistance inside the negative electrode material. Resistance, reducing energy loss during charging and discharging, thereby improving rate performance; the lithium salt complex is a complex composed of at least one organic lithium salt and at least one inorganic lithium salt, with the lithium salt complex as the outer shell. The lithium salt complex can reduce the freezing point of the electrolyte, so that it maintains a low viscosity at low temperatures, and improves the diffusion coefficient of lithium ions at low temperatures, thereby reducing the internal resistance of the battery and improving the energy density and initial charge and discharge efficiency of the negative electrode material; at the same time, the lithium salt complex can form a more stable solid electrolyte interface on the surface of the negative electrode material, improve and reduce the transmission resistance of lithium ions at the interface, and reduce the loss of lithium ions caused by defects, thereby improving rate performance and its initial efficiency. Therefore, the low-temperature fast-charging negative electrode composite material used in the power battery of the present invention has high electronic conductivity, energy density and initial charge and discharge efficiency, and also has good low-temperature performance.
[0051] In the technical solution of the present invention, the organic lithium salt in the lithium salt complex has high compatibility with the electrolyte and can maintain a high lithium ion diffusion coefficient under low temperature conditions; the inorganic lithium salt can maintain good electrochemical stability under high temperature and room temperature conditions, and can provide the necessary lithium ion concentration to maintain the conductivity and energy output of the battery under high temperature environment. In addition, the inorganic lithium salt can also help form a more stable solid electrolyte interface film (SEI film), reduce the side reaction between the electrolyte and the electrode material at high temperature, and thus improve the high temperature performance of the battery. Therefore, the lithium salt complex shell in the present invention has the high and low temperature performance advantages of both organic lithium salts and inorganic lithium salts.
[0052] The metallic silver includes silver particles or silver nanowires, and the silver particles are preferably silver nanoparticles.
[0053] In some embodiments of the present invention, the lithium salt complex includes an organic lithium salt, an inorganic lithium salt and a film-forming agent.
[0054] In the technical solution of the present invention, the network structure of the film-forming agent in the lithium salt complex increases the contact area between the organic lithium salt and the inorganic lithium salt, which is conducive to more efficient migration of lithium ions between the two, thereby improving the conductivity and kinetic properties of the electrolyte; at the same time, during the first charge and discharge process, the film-forming agent can promote the formation of a SEI film with higher density and stronger structural stability, thereby improving the cycle performance of the negative electrode material.
[0055] In some embodiments of the present invention, the lithium salt complex further includes a lithium coating agent, and the lithium coating agent includes a polymer, single lithium and a conductive agent.
[0056] In the technical solution of the present invention, the polymer in the lithium coating agent can act as a physical barrier to isolate the elemental lithium from direct contact with the electrolyte, and prevent the lithium metal from forming lithium dendrites during the charge and discharge process, thereby improving the safety of the battery; the elemental lithium provides an additional lithium source, which helps to achieve a higher battery capacity. The elemental lithium releases lithium ions during the injection or battery formation stage, which improves the first efficiency of the negative electrode material and the diffusion rate of lithium ions during the charge and discharge process, thereby improving the rate performance; the conductive agent significantly improves the electronic conductivity of the lithium coating agent, ensuring the rapid transmission of lithium ions in the electrode material, thereby improving the rate performance of the battery and shortening the charge and discharge time of the battery. The first efficiency refers to the ratio of the actual available electrical energy to the theoretical maximum electrical energy during the first charge and discharge process of the battery; the rate performance refers to the ratio of the battery discharge or charge rate to the rated capacity of the battery.
[0057] In some embodiments of the present invention, in the negative electrode material, the mass ratio of the core material to the shell material is 100:(5~15). The mass ratio of the core material to the shell material can be 100:15, 100:10 or 100:5. The mass ratio can ensure that the material has a large energy density while providing sufficient volume expansion buffer space within a suitable range, relieve the stress caused by the volume change of the core material during charging and discharging, and improve the cycle life of the battery; at the same time, it is ensured that the shell material forms an effective conductive network without sacrificing too much energy density, promotes the rapid transmission of lithium ions, reduces internal resistance, and improves the rate performance of the battery. The energy density is an indicator of how much energy a battery can store per unit volume or per unit mass.
[0058] In some embodiments of the present invention, in the core material, the mass ratio of the porous graphite, the conductive agent and the metallic silver is (90-98): (1-5): (1-5). The mass ratio of the porous graphite, the conductive agent and the metallic silver can be 95:2.5:2.5, 90:5:5 or 98:1:1. The mass ratio within a suitable range can improve the electronic conductivity of the core material, provide more electron transmission paths, and reduce the internal resistance, thereby improving the energy density, rate performance and cycle stability of the battery.
[0059] In some embodiments of the present invention, the mass ratio of the organic lithium salt, the inorganic lithium salt, the film-forming agent and the lithium coating agent in the lithium salt complex is (1-10): (1-10): (0.5-2): (1-3). The mass ratio of the organic lithium salt, the inorganic lithium salt, the film-forming agent and the lithium coating agent in the lithium salt complex can be 5:5:1:1, 1:1:0.5:1 or 10:10:2:3. The mass ratio within a suitable range can enable the battery to maintain good electrochemical performance in a wider temperature range, form a more stable SEI film, increase the capacity and improve the initial efficiency and rate performance of the battery.
[0060] In some embodiments of the present invention, the mass ratio of the polymer, the elemental lithium and the conductive agent in the lithium coating agent is (10-50):10:(1-5). The mass ratio of the polymer, the elemental lithium and the conductive agent in the lithium coating agent can be 30:10:3, 10:10:1 or 50:10:5. The mass ratio within a suitable range can ensure that the battery has a high energy density and first efficiency; at the same time, it helps to build a more efficient electron transmission network, reduce internal resistance, and improve rate performance.
[0061] In some embodiments of the present invention, the conductive agent includes at least one of carbon nanotubes and graphene. Among the above conductive agents, carbon nanotubes are preferred because carbon nanotubes have a large aspect ratio and high mechanical strength, can act as an efficient electron channel, and can significantly improve the conductivity of the negative electrode material at a relatively low addition amount.
[0062] In some embodiments of the present invention, the organic lithium salt includes at least one of lithium difluorooxalate, lithium difluoroborate, lithium difluorooxalate borate, lithium dioxalate borate, lithium difluoroacetate, and lithium difluorooxalate borate. That is, the organic lithium salt may contain any one of lithium difluorooxalate, lithium difluoroborate, lithium difluorooxalate borate, lithium dioxalate borate, lithium difluoroacetate, and lithium difluorooxalate borate, or may contain two or more of lithium difluorooxalate, lithium difluoroborate, lithium difluorooxalate borate, lithium dioxalate borate, lithium difluoroacetate, and lithium difluorooxalate borate, all of which belong to the protection scope of the present invention. By selecting the above-mentioned organic lithium salt, it can be ensured that the battery has good low temperature performance.
[0063] In some embodiments of the present invention, the inorganic lithium salt includes at least one of LiPF6, LiAsF6, and LiBF4. That is, the inorganic lithium salt may contain any one of LiPF6, LiAsF6, and LiBF4, or may contain two or more of LiPF6, LiAsF6, and LiBF4 at the same time, all of which fall within the protection scope of the present invention. By selecting the above inorganic lithium salt, the battery can be guaranteed to have good high temperature performance.
[0064] In some embodiments of the present invention, the film-forming agent includes at least one of vinylene carbonate, vinyl sulfite, propylene sulfite, and 1,4-butyrolactone sulfonate. That is, the film-forming agent may contain any one of vinylene carbonate, vinyl sulfite, propylene sulfite, and 1,4-butyrolactone sulfonate, or may contain two or more of vinylene carbonate, vinyl sulfite, propylene sulfite, and 1,4-butyrolactone sulfonate at the same time, all of which belong to the protection scope of the present invention. By selecting the above-mentioned film-forming agent, it can be ensured that the SEI film with higher density and stronger structural stability is formed during the first charge and discharge process, thereby improving the cycle performance of the battery.
[0065] In some embodiments of the present invention, the polymer includes at least one of polyalkylene carbonate, polyalkylene oxide, polyalkylsiloxane, polyalkyl acrylate, and polyalkyl methacrylate. That is, the polymer may contain any one of polyalkylene carbonate, polyalkylene oxide, polyalkylsiloxane, polyalkyl acrylate, and polyalkyl methacrylate, or may contain two or more of polyalkylene carbonate, polyalkylene oxide, polyalkylsiloxane, polyalkyl acrylate, and polyalkyl methacrylate at the same time, all of which belong to the protection scope of the present invention. By selecting the above polymer, it is possible to better avoid direct contact between elemental lithium and the electrolyte.
[0066] The present invention also provides a method for preparing a low-temperature fast-charging negative electrode composite material for a power battery, comprising the following steps:
[0067] S10, mixing a carbon source, a conductive agent, metal particles and a peroxide cross-linking agent, and performing a heat treatment under an inert gas to obtain a first porous graphite;
[0068] S20, mixing the first porous graphite with a silver ammonia solution, a surfactant and a reducing agent to perform a silver mirror reaction to obtain a second porous graphite;
[0069] S30, mixing the second porous graphite with the lithium salt complex, and drying, to obtain the low-temperature fast-charging negative electrode composite material for the power battery.
[0070] In the technical solution of the present invention, in step S10: first, a carbon source, a conductive agent, metal particles and a peroxide crosslinking agent are mixed into a mixture to increase the contact surface of each component; during the heat treatment process, the metal particles are gasified, and their original positions in the mixture are vacated to form the first type of pores; at the same time, the peroxide crosslinking agent in the mixture is decomposed during the heat treatment process to produce oxygen free radicals, and the carbon source also produces carbon free radicals due to the breakage of carbon-carbon bonds during the heat treatment process. The oxygen free radicals and the carbon free radicals on the surface of the carbon source are crosslinked by forming covalent bonds at multiple crosslinking points on the surface of the carbon source. Due to the irregularity of the carbon source and the peroxide crosslinking agent, the carbon source is subjected to the first type of pores. Due to the random distribution of the physical cross-linking agent, the cross-linking points are not evenly distributed, leaving unfilled spaces in the material, forming nanoscale holes, i.e., the second type of holes. The formation of the first type of holes and the second type of holes makes the first porous graphite have a higher specific surface area and porosity; the conductive agent may form physical or chemical bonds with the surrounding carbon sources during the heat treatment process. This interaction can enhance the overall conductive network of the material, so that the current can be more efficiently transmitted within the material. At the same time, the conductive agent plays a supporting role in the first porous graphite, which helps to maintain the porous structure and prevent the carbon source from excessively shrinking or collapsing during the thermal process. In step S20: the first porous graphite is mixed with a silver ammonia solution, a surfactant and a reducing agent to increase the contact area of each component, so that the silver ammonia solution, the surfactant and the reducing agent are dispersed on the outer surface of the first porous graphite and the inner surface of the pores. Through the silver mirror reaction, the silver ions in the silver ammonia solution are reduced to metallic silver by the reducing agent, and the metallic silver is deposited on the outer surface of the first porous graphite and the inner surface of the pores, so that a continuous silver conductive network is formed on the first porous graphite, thereby improving the electronic conductivity of the final negative electrode material and improving its rate performance. In this step, the second porous graphite is obtained after silver deposition. In step S30: the second porous graphite is mixed and dried with a lithium salt complex to obtain a negative electrode material, the lithium salt complex is a complex composed of at least one organic lithium salt and at least one inorganic lithium salt, so that the shell of the lithium salt complex is formed on the surface of the second porous graphite. Since the lithium salt complex has both the high temperature performance of the inorganic lithium salt and the low temperature performance of the organic lithium salt, the high temperature performance and low temperature performance of the negative electrode material are good.
[0071] The negative electrode material prepared by the above method has all the beneficial effects of the above negative electrode materials, which will not be described one by one here.
[0072] In step S10, the conductive agent may be a conductive agent solution, the mass concentration of the conductive agent in the conductive agent solution is 1-5%, and the solvent in the conductive agent solution includes N-methylpyrrolidone.
[0073] In some embodiments of the present invention, in step S10, the heat treatment includes heating the carbon source to a first temperature T1 for a first heat treatment, then heating it to a second temperature T2 for a second heat treatment, and then heating it to a third temperature T3 for a third pretreatment, wherein the first temperature T1 is less than the second temperature T2 and less than the third temperature T3.
[0074] In the technical solution of the present invention, the purpose of the first heat treatment is to remove impurities in the material, preliminarily decompose and reconstruct the carbon source material, exclude non-carbon elements in the material, and begin to form a carbon structure. The purpose of the second heat treatment is to further reconstruct the carbon structure, so that the bonds between carbon atoms become tighter, so that it develops in a more ordered and more stable graphitization direction. The purpose of the third heat treatment is to deeply graphitize the material, so that the carbon structure reaches the maximum degree of ordered arrangement, and forms highly crystalline porous graphite.
[0075] In some embodiments of the present invention, the value range of T1 is 1000-1500° C. T1 can be 1000° C., 1300° C. or 1500° C. The value range of T1 within a suitable range can ensure that non-carbon elements in the material are discharged and the carbon structure is initially formed.
[0076] In some embodiments of the present invention, the first heat treatment time is 1 to 3 hours. The first heat treatment time can be 1 hour, 2 hours or 3 hours. The first heat treatment time within a suitable range can ensure that there is enough time to remove non-carbon elements in the material as much as possible.
[0077] In some embodiments of the present invention, the value range of T2 is 2000-2200° C. The value range of T2 can be 2000° C., 2100° C. or 2300° C. The value range of T2 within a suitable range can ensure that the carbon structure can be reconstructed and the bonding between carbon atoms becomes tighter.
[0078] In some embodiments of the present invention, the second heat treatment time is 1 to 3 hours. The second heat treatment time can be 1 hour, 2 hours or 3 hours. The second heat treatment time within a suitable range can ensure that the carbon structure has sufficient time to be reconstructed and the graphitization is relatively stable and orderly.
[0079] In some embodiments of the present invention, the value range of T3 is 2800-3200° C. The value range of T3 can be 2800° C., 3000° C. or 3200° C. The value range of T3 within a suitable range can ensure that the carbon structure reaches the maximum degree of orderly arrangement.
[0080] In some embodiments of the present invention, the third heat treatment lasts for 12 to 36 hours. The third heat treatment may last for 12 hours, 24 hours or 36 hours. The third heat treatment time within a suitable range can ensure that the carbon structure is arranged in the most orderly manner.
[0081] In some embodiments of the present invention, step S10 further includes: cooling down the heat treatment to obtain the first porous graphite. Cooling down refers to cooling down to room temperature under an inert gas.
[0082] In some embodiments of the present invention, in step S10: the mass ratio of the carbon source, the conductive agent, the metal particles and the peroxide cross-linking agent is 100: (1-5) ~ (1-5): (1-5). The mass ratio of the carbon source, the conductive agent, the metal particles and the peroxide cross-linking agent can be 100: 1: 1: 1, 100: 5: 5: 5 or 100: 3: 3: 3. The mass ratio within a suitable range can ensure that the first porous graphite has a higher specific surface area and porosity, and the overall conductive network and mechanical properties of the material are good.
[0083] In some embodiments of the present invention, in step S10: the carbon source includes at least one of petroleum coke, needle coke, and asphalt coke. That is, the carbon source may contain any one of petroleum coke, needle coke, and asphalt coke, or may contain two or more of them at the same time, all of which fall within the scope of protection of the present invention. By selecting the above carbon source, a porous graphite material with a higher degree of order and a more stable structure can be obtained.
[0084] In some embodiments of the present invention, in step S10: the conductive agent includes at least one of carbon nanotubes and graphene. Selecting the above conductive agent can better improve the mechanical properties of the negative electrode material, maintain the porous structure of the negative electrode material, and enhance the conductive properties of the negative electrode material.
[0085] In some embodiments of the present invention, in step S10: the metal particles include at least one of metal nano-sodium, metal nano-potassium, and metal nano-zinc, and the particle size of the metal particles is 500-2000 nm.
[0086] That is, the metal particles may contain any one of metal nano sodium, metal nano potassium, and metal nano zinc, or may contain two or more of metal nano sodium, metal nano potassium, and metal nano zinc at the same time, all of which belong to the protection scope of the present invention. The particle size of the metal particles may be 500nm, 700nm, 1500nm, or 2000nm. When two or more metal particles are contained at the same time, the particle sizes may be different. The above metal particles are selected to ensure that holes of 500 to 2000nm are formed in the original position after the metal particles are gasified during the heat treatment process.
[0087] In some embodiments of the present invention, in step S10: the peroxidation crosslinking agent includes at least one of dibenzoyl peroxide, benzoyl peroxide, cyclohexanone peroxide, cyclohexanone peroxide paste, and lauroyl peroxide. That is, the peroxidation crosslinking agent may contain any one of dibenzoyl peroxide, benzoyl peroxide, cyclohexanone peroxide, cyclohexanone peroxide paste, and lauroyl peroxide, or may contain two or more of dibenzoyl peroxide, benzoyl peroxide, cyclohexanone peroxide, cyclohexanone peroxide paste, and lauroyl peroxide at the same time, all of which belong to the protection scope of the present invention. The above-mentioned peroxidation crosslinking agent is selected to ensure that the particle size of the second type of pores formed is between 1 and 100 nm.
[0088] In some embodiments of the present invention, in step S20, the step of obtaining the silver ammonia solution is as follows: mixing the silver salt solution with ammonia water and adjusting the pH of the system to an alkaline range to obtain the silver ammonia solution. The silver salt includes at least one of silver chloride, silver nitrate, silver phosphate, silver sulfate, and silver bromide. The concentration of the ammonia water is 25%.
[0089] In some embodiments of the present invention, in step S20: the silver ammonia solution contains Ag + and OH - The molar ratio of Ag in the silver ammonia solution is 1:(2-3). + and OH - The molar ratio of may be 1:3, 1:2.5 or 1:2, and the molar ratio within a suitable range helps to maintain the stability of the solution and promote its reaction with the reducing agent.
[0090] In some embodiments of the present invention, in step S20: the mass ratio of the silver salt, the first porous graphite, the surfactant, and the reducing agent in the silver ammonia solution is (5-15):100:(1-5):(25-50). The mass ratio of the silver salt, the first porous graphite, the surfactant, and the reducing agent in the silver ammonia solution can be 5:100:5:50, 10:100:3:43, or 15:100:1:25. The mass ratio within a suitable range can ensure that a continuous and good silver conductive network is formed on the first porous graphite, so that the electronic conductivity of the material is higher.
[0091] In some embodiments of the present invention, in step S20, the temperature of the silver mirror reaction is 25-100° C. The temperature of the silver mirror reaction can be 25° C., 55° C., 75° C. or 100° C. The temperature of the silver mirror reaction within a suitable range can ensure a high efficiency of the silver mirror reaction.
[0092] In some embodiments of the present invention, in step S20: the surfactant includes at least one of sodium butylnaphthalene sulfonate, sodium aminobenzene sulfonate, sodium fatty alcohol polyoxyethylene ether sulfate, and sodium fatty amine polyoxyethylene sulfate. That is, the surfactant may contain any one of sodium butylnaphthalene sulfonate, sodium aminobenzene sulfonate, sodium fatty alcohol polyoxyethylene ether sulfate, and sodium fatty amine polyoxyethylene sulfate, or may contain two or more of sodium butylnaphthalene sulfonate, sodium aminobenzene sulfonate, sodium fatty alcohol polyoxyethylene ether sulfate, and sodium fatty amine polyoxyethylene sulfate at the same time, all of which belong to the protection scope of the present invention. The common feature of these surfactants is that they contain a hydrophilic sulfonate or sulfate group in their molecular structure, and a hydrophobic carbon chain or aromatic ring, so that they can form a monolayer in the reaction system, reduce the interfacial energy, and thus promote the silver mirror reaction. By selecting the above-mentioned surfactants, the efficiency of the silver mirror reaction can be guaranteed to be high.
[0093] In some embodiments of the present invention, in step S20: the reducing agent includes at least one of formaldehyde, acetaldehyde, benzaldehyde, cinnamaldehyde, and acrolein. That is, the reducing agent may contain any one of formaldehyde, acetaldehyde, benzaldehyde, cinnamaldehyde, and acrolein, or may contain two or more of formaldehyde, acetaldehyde, benzaldehyde, cinnamaldehyde, and acrolein at the same time, all of which belong to the protection scope of the present invention. The above reducing agent has strong reducing properties, can effectively reduce silver ions, and ensures that the efficiency of the silver mirror reaction is high.
[0094] In some embodiments of the present invention, step S20 includes: mixing the first porous graphite with a silver ammonia solution, a surfactant and a reducing agent, performing a silver mirror reaction, and carbonizing to obtain a second porous graphite.
[0095] Among them, the purpose of carbonization treatment is to further remove impurities, carbonize organic polymers to generate amorphous carbon, and enhance the conductivity of the material.
[0096] In some embodiments of the present invention, step S30 includes: mixing the second porous graphite with an organic lithium salt, an inorganic lithium salt, a film-forming agent and a lithium coating agent, and drying to obtain the low-temperature fast-charging negative electrode composite material for the power battery;
[0097] The preparation of the lithium coating agent comprises the following steps: obtaining a polymer solution, mixing the polymer solution with elemental lithium and a conductive agent, filtering, and drying the filter residue to obtain the lithium coating agent.
[0098] The drying method includes spray drying.
[0099] The polymer solution has a solute of a polymer and a solvent of a carbonate solvent, and the mass concentration of the polymer in the polymer solution is 1-10%. The mass concentration can be 1%, 5% or 10%. The mass concentration within a suitable range can ensure that the single lithium is well coated and is not easily in direct contact with the electrolyte.
[0100] In some embodiments of the present invention, the mass ratio of the second porous graphite, the organic lithium salt, the inorganic lithium salt, the film-forming agent and the lithium coating agent is 100: (1-10): (1-10): (0.5-2): (1-3). The mass ratio of the second porous graphite, the organic lithium salt, the inorganic lithium salt, the film-forming agent and the lithium coating agent can be 100: 10: 10: 2: 3, 100: 5: 7: 1: 2 or 100: 1: 1: 0.5: 1. The mass ratio can ensure sufficient lithium source supply within a suitable range to achieve a larger battery capacity; form an effective protective layer shell to reduce side reactions without excessively hindering the diffusion of lithium ions; the final prepared negative electrode material has good electrochemical properties, including higher energy density, rate performance and short charge and discharge time.
[0101] In some embodiments of the present invention, the mass ratio of the polymer, elemental lithium and conductive agent in the polymer solution is (10-50):10:(1-5). The mass ratio of the polymer, elemental lithium and conductive agent can be 50:10:1, 30:10:3 or 10:10:5. The mass ratio within a suitable range can ensure that the polymer in the prepared lithium coating agent can form a sufficient protective layer to prevent the elemental lithium from directly contacting the electrolyte, while not affecting the normal transmission of lithium ions; and at the same time, it contains an appropriate amount of conductive agent to improve the conductivity of the material without occupying too much space and affecting the lithium storage capacity of the lithium coating agent.
[0102] The present invention also provides an application, in which the aforementioned low-temperature fast-charging negative electrode composite material for power batteries or the low-temperature fast-charging negative electrode composite material for power batteries prepared by the aforementioned preparation method of the low-temperature fast-charging negative electrode composite material for power batteries is applied to lithium-ion batteries. The low-temperature fast-charging negative electrode composite material for power batteries has all the above-mentioned beneficial effects, which will not be described one by one here.
[0103] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments and drawings. It should be understood that the following embodiments are only used to explain the present invention and are not used to limit the present invention.
[0104] Example 1
[0105] A low-temperature fast-charging negative electrode composite material for a power battery, comprising a core material and a shell material coated on the surface of the core material;
[0106] Wherein, the core material comprises porous graphite, a conductive agent doped in the porous graphite, and metallic silver covering the surface of the porous graphite; the shell material comprises a lithium salt complex;
[0107] The average pore size of the porous graphite is 3.2 nm; the mass ratio of the porous graphite, the conductive agent and the metallic silver is 94:3:3; and the mass ratio of the core material to the shell material is 100:15.
[0108] Example 2
[0109] Example 2 is similar to Example 1, except that:
[0110] The average pore size of the porous graphite is 1 nm; the mass ratio of the porous graphite, the conductive agent and the metallic silver is 98:1:1; and the mass ratio of the core material to the shell material is 100:5.
[0111] Example 3
[0112] Example 2 is similar to Example 1, except that:
[0113] The average pore size of the porous graphite is 5 nm; the mass ratio of the porous graphite, the conductive agent and the metallic silver is 90:5:5; and the mass ratio of the core material to the shell material is 100:10.
[0114] Example 4
[0115] A method for preparing a low-temperature fast-charging negative electrode composite material for a power battery comprises the following steps:
[0116] S10, 100g of petroleum coke, 100g of carbon nanotube conductive liquid solution (concentration of 3wt%), 3g of metal potassium powder particles (particle size of 1000nm) and 3g of dibenzoyl peroxide are mixed evenly, and then in an argon inert atmosphere, the temperature is first raised to 1300°C for 2h, then raised to 2100°C for 2h, and finally raised to 3000°C for graphitization and maintained for 24h, and finally cooled to room temperature in an argon inert atmosphere to obtain a first porous graphite;
[0117] S20, dissolving 10g of silver chloride (0.07mol) in 100g of deionized water, adding 6.125g of ammonia water (0.175mol) to mix and adjust the pH of the system to obtain a silver ammonia solution, then adding 100g of the first porous graphite to disperse evenly, adding 3g of sodium butylnaphthalenesulfonate and 35g of formaldehyde to the silver ammonia solution in sequence at a temperature of 60°C for reduction reaction for 2h, filtering, and carbonizing the obtained filter residue at 1100°C for 6h to obtain a second porous graphite;
[0118] S30, dissolving 30g of polyalkylene carbonate in 600g of carbonate solvent to form a polymer solution with a mass concentration of 5wt%, then adding 10g of single lithium powder, stirring evenly, then adding 3g of carbon nanotube conductive agent to disperse evenly, filtering, taking the filter residue, and vacuum drying the filter residue at a temperature of 80°C for 24h under the protection of argon inert gas to obtain a lithium coating agent;
[0119] Add 5g of lithium difluorooxalate and 5g of LiPF6 to 110g of ethylene carbonate solvent and disperse them evenly, and add 1g of vinylene carbonate to obtain a 10wt% uniform mixed solution, then add 100g of the second porous graphite, 2g of the lithium coating agent solution and disperse them evenly, spray dry (inlet temperature 200℃, outlet temperature 80℃, flow rate 0.5kg / h, 2h) to obtain a low-temperature fast-charging negative electrode composite material for power batteries.
[0120] Example 5
[0121] A method for preparing a low-temperature fast-charging negative electrode composite material for a power battery comprises the following steps:
[0122] S10, 100 g of needle coke, 100 g of carbon nanotube conductive liquid solution (concentration of 1 wt%), 1 g of metal sodium particles (particle size of 500 nm) and 1 g of benzoyl peroxide are mixed evenly, and then heated to 1000° C. and kept for 3 h under an argon inert atmosphere, then heated to 2000° C. and kept for 3 h, and finally heated to 2800° C. and kept for 36 h under a graphitization process, and finally cooled to room temperature under an argon inert atmosphere to obtain a first porous graphite;
[0123] S20, dissolving 5g of silver nitrate (0.03mol) in 100g of deionized water, then adding 2.1g of ammonia water (0.06mol) to mix and adjust the pH of the system to obtain a silver ammonia solution, then adding 100g of the first porous graphite to disperse evenly, and then adding 1g of sodium aminobenzenesulfonate and 25g of acetaldehyde to the silver ammonia solution in sequence at a temperature of 25°C for a reduction reaction for 3h, filtering, and carbonizing the obtained filter residue at 1100°C for 6h to obtain a second porous graphite;
[0124] S30, dissolving 10g of polyalkylene oxide in 1000g of carbonate solvent to form a polymer solution with a mass concentration of 1wt%, then adding 10g of single lithium powder, stirring evenly, then adding 1g of carbon nanotube conductive agent to disperse evenly, filtering, taking the filter residue, and vacuum drying the filter residue at a temperature of 50°C for 36h under the protection of argon inert gas to obtain a lithium coating agent;
[0125] 1g of lithium difluoroborate and 1g of LiAsF6 were added to 75g of ethylene carbonate solvent and dispersed evenly, and 0.5g of vinyl sulfite was added to obtain a 30wt% uniform mixed solution, and then 100g of the second porous graphite was added, 1g of the lithium coating agent solution was dispersed evenly, and spray dried (inlet temperature 200°C, outlet temperature 80°C, flow rate 0.5kg / h, 2h) to obtain a low-temperature fast-charging negative electrode composite material for a power battery.
[0126] Example 6
[0127] A method for preparing a low-temperature fast-charging negative electrode composite material for a power battery comprises the following steps:
[0128] S10, 100g of pitch coke, 100g of carbon nanotube conductive liquid solution (concentration of 5wt%), 5g of metal zinc particles (particle size of 2000nm) and 5g of cyclohexanone peroxide are mixed evenly, and then heated to 1500°C for 1h, then heated to 2200°C for 1h, and finally heated to 3200°C for graphitization for 12h under an argon inert atmosphere, and then cooled to room temperature under an argon inert atmosphere to obtain a first porous graphite;
[0129] S20, dissolving 15g of silver sulfate (0.048mol) in 100g of deionized water, then adding 5.04g of ammonia water (0.144mol) to mix and adjust the pH of the system to obtain a silver ammonia solution, then adding 100g of the first porous graphite to disperse evenly, and then adding 5g of fatty alcohol polyoxyethylene ether sodium sulfate and 50g of benzaldehyde reducing agent to the silver ammonia solution at a temperature of 100°C for reduction reaction for 1h, filtering, and carbonizing the obtained filter residue at 1100°C for 6h to obtain a second porous graphite;
[0130] S30, dissolving 50g of polyalkylsiloxane in 5000g of carbonate solvent to form a polymer solution with a mass concentration of 10wt%, then adding 10g of single lithium powder, stirring evenly, then adding 5g of carbon nanotube conductive agent to disperse evenly, filtering, taking the filter residue, and vacuum drying the filter residue at a temperature of 100°C for 12h under the protection of argon inert gas to obtain a lithium coating agent;
[0131] 10g of lithium difluorooxalatoborate and 10g of LiBF4 were added to 440g of ethylene carbonate solvent and dispersed evenly, and 2g of propylene sulfite was added to obtain a 5wt% uniform mixed solution, and then 100g of the second porous graphite was added, 3g of the lithium coating agent solution was dispersed evenly, and spray dried (inlet temperature 200°C, outlet temperature 80°C, flow rate 0.5kg / h, 2h) to obtain a low-temperature fast-charging negative electrode composite material for power batteries.
[0132] Comparative Example 1
[0133] Compared with Example 4, Comparative Example 1 is the same as Example 4 except that metallic potassium powder particles and dibenzoyl peroxide are not added in step S10.
[0134] Comparative Example 2
[0135] Compared with Example 4, Comparative Example 2 is the same as Example 4 except that step S20 is not performed.
[0136] Comparative Example 3
[0137] Compared with Example 4, Comparative Example 3 is the same as Example 4 except that step S30 is not performed.
[0138] Performance Testing
[0139] The negative electrode material prepared in Example 4 was subjected to SEM testing, and the results were as follows: Figure 1 shown.
[0140] Depend on Figure 1 It can be seen that the material presents a secondary particle structure, the particle size is between 10 and 15 μm, and the particle size distribution is uniform.
[0141] The performance of the negative electrode materials in Examples 4 to 6 and Comparative Examples 1 to 3 was characterized in the following manner:
[0142] The powder resistivity and specific surface area of the negative electrode material are tested according to the test method in standard GB / T-24533-2019 "Graphite negative electrode materials for lithium-ion batteries";
[0143] The orientation index (OI value) of the negative electrode material was tested by X-ray diffraction (XRD);
[0144] The diffusion coefficient of the negative electrode material was tested by constant current intermittent titration technique (GITT);
[0145] The interlayer spacing D002 of the negative electrode material was tested by XRD;
[0146] The test results are shown in Table 1.
[0147] Table 1 Performance characteristics of negative electrode materials in Examples 4 to 6 and Comparative Examples 1 to 3
[0148]
[0149] It can be seen from Table 1 that the specific surface area and diffusion coefficient of the negative electrode materials prepared in Examples 4 to 6 are significantly higher than those in Comparative Examples 1 to 3. The reason may be that the surface of the negative electrode material prepared by the present invention is coated with organic lithium salts and inorganic lithium salts, which improves the lithium ion diffusion coefficient and the initial efficiency of the material. At the same time, the lithium coating agent releases lithium ions during the charge and discharge process, which improves the diffusion coefficient of the material.
[0150] The negative electrode materials prepared in Examples 4 to 6 and the negative electrode materials in Comparative Examples 1 to 3 were respectively assembled into button batteries according to the following methods:
[0151] The negative electrode materials prepared in Examples 4 to 6 and Comparative Examples 1 to 3 were used as negative electrodes and assembled into button cells with lithium sheets, electrolytes and separators in a glove box with argon and water content less than 0.1 ppm. The separator was celegard 2400; the electrolyte was a solution of LiPF6, in which the concentration of LiPF6 was 1 mol / L, and the solvent was a mixed solution of ethylene carbonate (EC) and diethyl carbonate (DMC) mixed in a weight ratio of 1:1.
[0152] The performance of the button batteries was tested by a blue battery tester on the six groups of button batteries prepared, and the test conditions were as follows:
[0153] First discharge capacity: Charge and discharge at a rate of 0.1C, with a voltage range of 0.005~2V. Stop after 3 cycles, and then test the discharge capacity under 1C conditions;
[0154] Low temperature capacity retention rate: Test its specific capacity at low temperature of -20℃ and 0.1C, and calculate the low temperature capacity retention rate, that is, the ratio of low temperature capacity to room temperature capacity (25℃, 0.1C);
[0155] Cycle performance: 25±3℃, 0.2C / 0.2C, 100 weeks;
[0156] Low temperature charging DCR: -20℃, 0.05C, 50%SOC;
[0157] The test results are shown in Table 2.
[0158] Table 2 Performance characteristics of button batteries corresponding to Examples 4 to 6 and Comparative Examples 1 to 3
[0159]
[0160] As can be seen from Table 2, the button cells prepared using the negative electrode materials of Examples 4 to 6 have significantly better discharge specific capacity, initial efficiency and low-temperature charging DCR than those of Comparative Examples 1 to 3. The reason is that the surface of graphite is coated with organic lithium salts and inorganic lithium salts to reduce the irreversible capacity of the material, and the lithium coating agent can release lithium ions during the first charge and discharge process, thereby improving the initial efficiency, improving the low-temperature capacity retention rate, reducing the low-temperature DCR, and improving the cycle performance.
[0161] The negative electrode materials of Examples 4 to 6 and Comparative Examples 1 to 3 are used as negative electrode active materials and the positive electrode active materials are ternary materials (LiNi 1 / 3 Co 1 / 3 Mn 1 / 3O2), electrolyte and diaphragm are assembled into a 5Ah soft pack battery. The diaphragm is celegard2400, and the electrolyte is LiPF6 solution (the solvent is a mixed solution of EC and DEC with a volume ratio of 1:1, and the concentration of LiPF6 is 1.3mol / L). The prepared soft pack battery is tested for its cycle and rate performance. The test results are detailed in Table 3.
[0162] Low temperature cycle performance: The battery cycle performance is tested at a temperature of -20±3℃ with a charge and discharge rate of 0.2C / 0.22C, a voltage range of 2.8V-4.2V, and a cycle number of 200 cycles;
[0163] Rate performance: Charge the battery to 100% SOC at a rate of 2C using constant current + constant voltage mode, and then calculate the constant current ratio = constant current capacity / (constant current capacity + constant voltage capacity).
[0164] Table 3 Performance characteristics of soft-pack batteries corresponding to Examples 4 to 6 and Comparative Examples 1 to 3
[0165]
[0166] It can be seen from Table 3 that the cycle performance and rate performance (i.e., fast charging performance) of the soft-pack batteries prepared from the negative electrode materials prepared in Examples 4 to 6 are significantly better than those in Comparative Examples 1 to 3. The reason is that the surface of the negative electrode material of the present invention is coated with organic lithium salts and inorganic lithium salts to reduce the consumption of lithium ions during the charge and discharge process and its large specific surface area, thereby improving its cycle performance; at the same time, the negative electrode material of the present invention has an excellent diffusion coefficient and a low OI value, thereby improving the fast charging performance of the material.
[0167] The above are only preferred embodiments of the present invention, and do not limit the patent scope of the present invention. For those skilled in the art, the present invention may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the patent protection scope of the present invention.
Claims
1. A low-temperature fast-charging negative electrode composite material for a power battery, characterized in that: It includes a core material and a shell material coated on the surface of the core material; The core material includes porous graphite, a conductive agent doped in the porous graphite, and metallic silver covering the surface of the porous graphite; the average pore size of the porous graphite is 1-5 nm; The shell material includes a lithium salt complex; The low-temperature fast-charging negative electrode composite material used in the power battery is prepared by the following steps: S10, mixing a carbon source, a conductive agent, metal particles and a peroxide cross-linking agent, and performing a heat treatment under an inert gas to obtain a first porous graphite; S20, mixing the first porous graphite with a silver ammonia solution, a surfactant and a reducing agent to perform a silver mirror reaction to obtain a second porous graphite; S30, mixing the second porous graphite with the lithium salt complex, and drying, to obtain the low-temperature fast-charging negative electrode composite material for the power battery.
2. The low-temperature fast-charging negative electrode composite material for a power battery according to claim 1, characterized in that: The lithium salt complex comprises an organic lithium salt, an inorganic lithium salt and a film-forming agent.
3. The low-temperature fast-charging negative electrode composite material for a power battery according to claim 2, characterized in that: The lithium salt composite further includes a lithium coating agent, wherein the lithium coating agent includes a polymer, single lithium and a conductive agent.
4. The low-temperature fast-charging negative electrode composite material for a power battery according to claim 3, characterized in that: In the low-temperature fast-charging negative electrode composite material used in the power battery, the mass ratio of the core material to the shell material is 100: (5-15); and / or, In the core material, the mass ratio of the porous graphite, the conductive agent and the metallic silver is (90-98): (1-5): (1-5); and / or, The mass ratio of the organic lithium salt, the inorganic lithium salt, the film-forming agent and the lithium coating agent in the lithium salt composite is (1-10): (1-10): (0.5-2): (1-3); and / or, The mass ratio of the polymer, the elemental lithium and the conductive agent in the lithium coating agent is (10-50):10:(1-5); and / or, The conductive agent includes at least one of carbon nanotubes and graphene; and / or, The organic lithium salt comprises at least one of lithium difluorooxalate, lithium difluoroborate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluoroacetate, and lithium difluorooxalatoborate; and / or, The inorganic lithium salt includes at least one of LiPF6, LiAsF6, and LiBF4; and / or, The film-forming agent includes at least one of vinylene carbonate, vinyl sulfite, propylene sulfite, and 1,4-butyrolactone sulfonate; and / or, The polymer includes at least one of polyalkylene carbonate, polyalkylene oxide, polyalkylsiloxane, polyalkyl acrylate, and polyalkyl methacrylate.
5. A method for preparing a low-temperature fast-charging negative electrode composite material for a power battery according to any one of claims 1 to 4, characterized in that: The following steps are involved: S10, mixing a carbon source, a conductive agent, metal particles and a peroxide cross-linking agent, and performing a heat treatment under an inert gas to obtain a first porous graphite; S20, mixing the first porous graphite with a silver ammonia solution, a surfactant and a reducing agent to perform a silver mirror reaction to obtain a second porous graphite; S30, mixing the second porous graphite with the lithium salt complex, and drying, to obtain the low-temperature fast-charging negative electrode composite material for the power battery.
6. The method for preparing the low-temperature fast-charging negative electrode composite material for a power battery according to claim 5, characterized in that: In step S10: The mass ratio of the carbon source, the conductive agent, the metal particles and the peroxide cross-linking agent is 100: (1-5): (1-5): (1-5); and / or, The carbon source includes at least one of petroleum coke, needle coke and pitch coke; and / or, The conductive agent includes at least one of carbon nanotubes and graphene; and / or, The metal particles include at least one of metal nano-sodium, metal nano-potassium, and metal nano-zinc, and the particle size of the metal particles is 500-2000 nm; and / or, The peroxidation crosslinking agent includes at least one of dibenzoyl peroxide, benzoyl peroxide, cyclohexanone peroxide, cyclohexanone peroxide paste, and lauroyl peroxide.
7. The method for preparing the low-temperature fast-charging negative electrode composite material for a power battery according to claim 5, characterized in that: In step S20: The silver ammonia solution contains Ag + and OH - The molar ratio is 1:(2-3); and / or, The mass ratio of the silver salt, the first porous graphite, the surfactant and the reducing agent in the silver ammonia solution is (5-15):100:(1-5):(25-50); and / or, The surfactant includes at least one of sodium butylnaphthalene sulfonate, sodium aminobenzene sulfonate, sodium fatty alcohol polyoxyethylene ether sulfate, and sodium fatty amine polyoxyethylene sulfate; and / or, The reducing agent includes at least one of formaldehyde, acetaldehyde, benzaldehyde, cinnamaldehyde and acrolein.
8. The method for preparing the low-temperature fast-charging negative electrode composite material for a power battery according to claim 5, characterized in that: Step S30 includes: mixing the second porous graphite with an organic lithium salt, an inorganic lithium salt, a film-forming agent and a lithium coating agent, and drying to obtain the low-temperature fast-charging negative electrode composite material for the power battery; Wherein, the preparation of the lithium coating agent comprises the following steps: A polymer solution is obtained, and the polymer solution is mixed with single-substance lithium and a conductive agent, filtered, and the filter residue is dried to obtain a lithium coating agent.
9. The method for preparing the low-temperature fast-charging negative electrode composite material for a power battery according to claim 8, characterized in that: The mass ratio of the second porous graphite, the organic lithium salt, the inorganic lithium salt, the film-forming agent and the lithium coating agent is 100: (1-10): (1-10): (0.5-2): (1-3); and / or, The mass ratio of the polymer, the elemental lithium and the conductive agent in the polymer solution is (10-50):10:(1-5).
10. An application, characterized in that: The low-temperature fast-charging negative electrode composite material for a power battery as described in any one of claims 1 to 4 or the low-temperature fast-charging negative electrode composite material for a power battery prepared by the preparation method of the low-temperature fast-charging negative electrode composite material for a power battery as described in any one of claims 5 to 9 is applied to a lithium-ion battery.