Preparation method and application of Mg-Cu / Al2O3 catalyst

Through the preparation and application of Mg-Cu/Al2O3 catalyst, the problems of low hydrogen sulfide removal efficiency and high deactivation treatment cost of catalysts in the existing technology are solved, the effects of efficient removal and low-temperature recovery of S are achieved, and the energy consumption is significantly reduced. and cost.

CN118577278BActive Publication Date: 2024-10-22CHINESE RES ACAD OF ENVIRONMENTAL SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411062561.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-10-22
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

Existing catalysts have low removal efficiency of hydrogen sulfide, and the processing cost of the deactivated catalyst is high, especially under low temperature conditions, it is difficult to achieve efficient removal and recovery.

Method used

Using the preparation method of Mg-Cu/Al2O3 catalyst, by combining Al2O3 particles with Cu(NO3)2 solution and Mg(NO3)2 solution, after ultrasonic treatment, drying and calcination, a catalyst containing 3-7.8% is prepared. Catalyst of Cu and Mg active components, and performs H2S removal and S recovery at 180-230°C.

Benefits of technology

Efficient removal of H2S is achieved. Each gram of catalyst can capture 506mg H2S. The catalytic efficiency is higher than that of cutting-edge technology. The deactivated catalyst can effectively recover S at low temperatures, reducing calcination costs and energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118577278B_ABST
    Figure CN118577278B_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a Mg-Cu / Al2O3 catalyst, belonging to the technical field of catalysts. The preparation method of the Mg-Cu / Al2O3 catalyst comprises the following steps: S1, placing Al2O3 particles in a Cu(NO3)2 solution to obtain a mixed solution, subjecting the mixed solution to ultrasonic treatment, standing, drying, and calcining, and obtaining a Cu(3.1wt%) / Al2O3 catalyst after the calcination is completed; S2, immersing the Cu(3.1wt%) / Al2O3 catalyst in a Mg(NO3)2 solution to obtain a mixture B; S3, subjecting the mixture B to ultrasonic treatment, drying, and calcining to obtain a Mg-Cu / Al2O3 catalyst; the Mg-Cu / Al2O3 catalyst prepared by the invention has high catalytic efficiency and reduces the cost of S recovery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalysts, and in particular to a preparation method and application of a Mg-Cu / Al2O3 catalyst. Background Art

[0002] Hydrogen sulfide (H2S) is a colorless, corrosive, highly toxic gas that is ubiquitous in many chemical processes, landfills, and shale gas formations, and permeates into various environments. H2S has the potential to corrode transportation pipelines and buildings, promote the formation of acid rain in the atmosphere, degrade the environment, and pose a threat to human health. The olfactory threshold of H2S is very low, only 0.0008 mg / m3, and it can cause discomfort even at low concentrations. Therefore, it is critical to reduce H2S emission levels below the olfactory threshold. Low-temperature catalytic oxidation technology can directly convert H2S into S without generating secondary pollution, but the treatment of deactivated catalysts remains a difficult problem.

[0003] The catalyst in the prior art has low efficiency in removing hydrogen sulfide. When recovering S, the catalyst temperature needs to be maintained at 500° C., which results in high heating costs. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a method for preparing a Mg-Cu / Al2O3 catalyst, comprising the following steps:

[0005] S1. Place Al2O3 particles in a Cu(NO3)2 solution to obtain a mixed solution, wherein the mass ratio of the Al2O3 particles to the Cu(NO3)2 solution is 1:4.75, and the mass percentage of the Cu(NO3)2 solution is 15.79%. The mixed solution is ultrasonically treated for 20-60 min, allowed to stand for 6-12 h, and then dried in a drying oven to obtain a mixture A. The temperature of the drying oven is 30-80°C, and the drying time is 30-100 min. Place the mixture A in a muffle furnace and calcine for 3-8 h. The calcination temperature of the muffle furnace is 300-600°C. After calcination, a Cu(3.1wt%) / Al2O3 catalyst is obtained;

[0006] S2, Mg(NO3)2 and distilled water are prepared into a Mg(NO3)2 solution in a mass ratio of 2.1:10, and the Cu(3.1wt%) / Al2O3 catalyst is immersed in the Mg(NO3)2 solution for 6-12h to obtain a mixture B, wherein the mass ratio of the Cu(3.1wt%) / Al2O3 catalyst to the Mg(NO3)2 solution is 5:24.2;

[0007] S3. Ultrasonic treatment of the mixture B for 20-30 min, drying in a drying oven, and calcining in a muffle furnace for 3-8 h. After calcination, a Mg-Cu / Al2O3 catalyst is obtained. The calcination temperature in the muffle furnace is 200-300°C.

[0008] It has been determined that the Mg-Cu / Al2O3 catalyst prepared in the present invention contains 3-7.8% of Cu and Mg active components, which can effectively achieve high-efficiency removal of H2S and greatly reduce the cost of H2S removal.

[0009] Furthermore, the Al2O3 particles are mixed by Al2O3 particles with a particle size of 0.88-2 mm, Al2O3 particles with a particle size of 425-880 μm, and Al2O3 particles with a particle size of 270-425 μm in a mass ratio of 0.5-3:95-99:0.5-2.

[0010] Description: Using three different sizes of Al2O3 particles as carriers, the formed catalyst can effectively load the active components, improve the contact efficiency between the active components and H2S, and improve the H2S removal effect.

[0011] On the other hand, the present invention also provides an application of a Mg-Cu / Al2O3 catalyst. The Mg-Cu / Al2O3 catalyst prepared by the above method is applied to H2S gas treatment to convert H2S gas into S, and the S is recovered.

[0012] Furthermore, the method of applying the Mg-Cu / Al2O3 catalyst to H2S gas treatment is as follows: H2S gas is mixed with water atomized gas to obtain a mixed gas, the humidity of the mixed gas is adjusted to 40-80%, the temperature of the mixed gas is adjusted to 30-60°C, the mixed gas is passed into a hammer reaction tower, and the mixed gas is passed through the Mg-Cu / Al2O3 catalyst to remove H2S, and then in a vertical tube furnace, the Mg-Cu / Al2O3 catalyst fully adsorbed with S is purged with N2 gas, and the S in the purged tail gas is captured and recovered through a condenser.

[0013] Furthermore, calculated based on the amount of H2S gas introduced, the amount of the Mg-Cu / Al2O3 catalyst used is 2.69 g / L.

[0014] Note: Each gram of this catalyst can capture 506 mg of H2S.

[0015] Furthermore, the N2 purge intensity is 120 mL / min.

[0016] Note: The above-mentioned purge intensity can ensure that the sublimated sulfur gas is effectively transported to the condenser.

[0017] Furthermore, the heating temperature of the Mg-Cu / Al2O3 catalyst is 180-230°C.

[0018] Note: The deactivated catalyst can effectively recover S at a temperature of 180-230°C, ensuring that the S adsorbed by the catalyst is sublimated into the purge gas, maintaining a recovery efficiency of no less than 83%, which can effectively reduce the calcination cost.

[0019] Furthermore, the tail gas captured by the condenser is passed into a NaOH solution with a mass concentration of 20% by microporous aeration to purify the SO2 gas in the tail gas.

[0020] Note: NaOH solution can effectively remove SO2 gas that may be contained in the exhaust gas.

[0021] The beneficial effects of the present invention are:

[0022] (1) The Mg-Cu / Al2O3 catalyst prepared by the present invention can achieve a capture performance of 506 mgH2S per gram of the catalyst, which is 1.26 to 1.51 times the catalytic performance of the previous catalyst and has high catalytic efficiency.

[0023] (2) The deactivated catalyst can achieve effective S recovery at a temperature of 180-230°C, with an S recovery efficiency of no less than 83%. The calcination cost is less than half of that of the existing technology, which can effectively reduce energy consumption and thus reduce the cost of S recovery. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is the N1s chart of the XPS sample of the Mg-Cu / Al2O3 catalyst prepared in Example 1 of the present invention.

[0025] Figure 2 It is the Cu2p diagram of the XPS sample of the Mg-Cu / Al2O3 catalyst prepared in Example 1 of the present invention.

[0026] Figure 3 It is the O1s chart of the XPS sample of the Mg-Cu / Al2O3 catalyst prepared in Example 1 of the present invention.

[0027] Figure 4 It is a thermogravimetric diagram of the sample of Mg-Cu / Al2O3 catalyst prepared in Example 1 of the present invention.

[0028] Figure 5 This is the XRD diagram of the composite calcination of the surface active components of the Mg-Cu / Al2O3 catalyst prepared in Example 3.

[0029] Figure 6It is a comparison chart of the amount of H2S gas that can be captured per gram of catalyst in Examples 1 to 3.

[0030] Figure 7 It is a bar chart comparing the capture performance of single gram Mg-Cu / Al2O3 catalyst in Examples 4 to 6.

[0031] Figure 8 This is a comparison chart of the amount of H2S gas that can be effectively treated per gram of catalyst at different humidity in Examples 6 to 9. DETAILED DESCRIPTION

[0032] Example 1: A method for preparing a Mg-Cu / Al2O3 catalyst, comprising the following steps:

[0033] S1. Al2O3 particles are placed in a Cu(NO3)2 solution to obtain a mixed solution, wherein the mass ratio of Al2O3 particles to Cu(NO3)2 solution is 1:4.75, and the mass percentage of Cu(NO3)2 solution is 15.79%. The mixed solution is ultrasonically treated for 20 minutes, and then allowed to stand for 6 hours. The wavelength of the ultrasonic treatment is 7.5 mm, and the frequency of the ultrasonic treatment is 30 kHz. The mixed solution is then dried in a drying oven to obtain a mixture A. The temperature of the drying oven is 30°C, and the drying time is 30 minutes. The mixture A is placed in a muffle furnace and calcined for 3 hours. The calcination temperature of the muffle furnace is 300°C. After calcination, a Cu(3.1wt%) / Al2O3 catalyst is obtained.

[0034] The Al2O3 particles are mixed with Al2O3 particles with a particle size of 0.88-2 mm, Al2O3 particles with a particle size of 425-880 μm, and Al2O3 particles with a mass ratio of 0.5:95:0.5;

[0035] S2, Mg(NO3)2 and distilled water are prepared into Mg(NO3)2 solution in a mass ratio of 2.1:10, and Cu(3.1wt%) / Al2O3 catalyst is immersed in the Mg(NO3)2 solution for 6h to obtain a mixture B, wherein the mass ratio of Cu(3.1wt%) / Al2O3 catalyst to Mg(NO3)2 solution is 5:24.2;

[0036] S3. Ultrasonic treatment of mixture B for 20-30 min, with a wavelength of 7.5 mm and a frequency of 30 kHz, followed by drying in a drying oven, and calcination in a muffle furnace for 3 h. After calcination, Mg-Cu / Al2O3 catalyst is obtained, and the calcination temperature in the muffle furnace is 200°C.

[0037] The chemical reactions involved are:

[0038] ① There is a dehydration oxidation reaction in the preparation process of Cu (3.1wt%) / Al2O3 catalyst:

[0039] Cu(NO3)2(s)→CuO(s)+2NO2(g)+1 / 2O2(g)(1)

[0040] There is also a complex vacancy oxygen formation mechanism, during which CuO(s) becomes Cu2O.

[0041] ②The preparation process of Mg-Cu / Al2O3 catalyst involves the replacement and compounding of Mg and Cu, and the formation of the internal pore structure of the catalyst caused by the desorption of bound water in Mg(NO3)2·6H2O.

[0042] The N1s graph, Cu2p graph, O1s graph and thermogravimetric graph of the XPS sample of the Mg-Cu / Al2O3 catalyst prepared in this example are shown in the figure below: Figure 1 , Figure 2 , Figure 3 , Figure 4 shown.

[0043] Example 2: A method for preparing a Mg-Cu / Al2O3 catalyst, comprising the following steps:

[0044] S1. Al2O3 particles are placed in a Cu(NO3)2 solution to obtain a mixed solution, wherein the mass ratio of Al2O3 particles to Cu(NO3)2 solution is 1:4.75, and the mass percentage of Cu(NO3)2 solution is 15.79%. The mixed solution is ultrasonically treated for 40 minutes, and then allowed to stand for 8 hours. The wavelength of the ultrasonic treatment is 8 mm, and the frequency of the ultrasonic treatment is 40 kHz. The mixed solution is then dried in a drying oven to obtain a mixture A. The temperature of the drying oven is 50°C, and the drying time is 50 minutes. The mixture A is placed in a muffle furnace and calcined for 4 hours. The calcination temperature of the muffle furnace is 400°C. After calcination, a Cu(3.1wt%) / Al2O3 catalyst is obtained.

[0045] The Al2O3 particles are mixed with Al2O3 particles with a particle size of 0.88-2 mm, Al2O3 particles with a particle size of 425-880 μm, and Al2O3 particles with a mass ratio of 1:98:1;

[0046] S2, Mg(NO3)2 and distilled water are prepared into Mg(NO3)2 solution in a mass ratio of 2.1:10, and Cu(3.1wt%) / Al2O3 catalyst is immersed in the Mg(NO3)2 solution for 10 hours to obtain a mixture B, wherein the mass ratio of Cu(3.1wt%) / Al2O3 catalyst to Mg(NO3)2 solution is 5:24.2;

[0047] S3. The mixture B was ultrasonically treated for 25 minutes, the wavelength of the ultrasonic treatment was 8 mm, the frequency of the ultrasonic treatment was 40 kHz, and then placed in a drying oven for drying, and then placed in a muffle furnace for calcination for 4 hours. After the calcination was completed, Mg-Cu / Al2O3 catalyst was obtained, and the muffle furnace calcination temperature was 250°C.

[0048] Embodiment 3: A method for preparing a Mg-Cu / Al2O3 catalyst comprises the following steps:

[0049] S1. Al2O3 particles are placed in a Cu(NO3)2 solution to obtain a mixed solution, wherein the mass ratio of Al2O3 particles to Cu(NO3)2 solution is 1:4.75, and the mass percentage of Cu(NO3)2 solution is 15.79%. The mixed solution is ultrasonically treated for 60 minutes, and then allowed to stand for 12 hours. The wavelength of the ultrasonic treatment is 10 mm, and the frequency of the ultrasonic treatment is 50 kHz. The mixed solution is then dried in a drying oven to obtain a mixture A. The temperature of the drying oven is 80°C, and the drying time is 100 minutes. The mixture A is placed in a muffle furnace and calcined for 8 hours. The calcination temperature of the muffle furnace is 600°C. After calcination, a Cu(3.1wt%) / Al2O3 catalyst is obtained.

[0050] The Al2O3 particles are mixed with Al2O3 particles with a particle size of 0.88-2 mm, Al2O3 particles with a particle size of 425-880 μm, and Al2O3 particles with a mass ratio of 3:99:2;

[0051] S2, Mg(NO3)2 and distilled water are prepared into Mg(NO3)2 solution in a mass ratio of 2.1:10, and Cu(3.1wt%) / Al2O3 catalyst is immersed in the Mg(NO3)2 solution for 12h to obtain a mixture B, wherein the mass ratio of Cu(3.1wt%) / Al2O3 catalyst to Mg(NO3)2 solution is 5:24.2;

[0052] S3. The mixture B was ultrasonically treated for 30 minutes, the wavelength of the ultrasonic treatment was 10 mm, the frequency of the ultrasonic treatment was 50 kHz, and then placed in a drying oven for drying, and then placed in a muffle furnace for calcination for 8 hours. After the calcination was completed, Mg-Cu / Al2O3 catalyst was obtained, and the muffle furnace calcination temperature was 300°C.

[0053] The XRD pattern of the composite calcined active components of the Mg-Cu / Al2O3 catalyst prepared in Example 3 is shown in Figure 5 As shown, the comparison of the amount of H2S gas that can be captured per gram of the catalyst prepared in Example 1 to Example 3 is shown in Figure 6 As shown, by comparison, it can be seen that the Mg-Cu / Al2O3 catalyst prepared in Example 3 has the best effect.

[0054] Example 4: Mg-Cu / Al2O3 catalyst is applied to H2S gas treatment to convert H2S gas into S, and the S is recovered.

[0055] The method of applying Mg-Cu / Al2O3 catalyst to H2S gas treatment is as follows: H2S gas is mixed with water atomized gas to obtain a mixed gas, the humidity of the mixed gas is adjusted to 40%, the temperature of the mixed gas is adjusted to 30°C, the mixed gas is passed into a hammer reaction tower, and the mixed gas is passed through the Mg-Cu / Al2O3 catalyst to remove H2S;

[0056] In this process, H2O not only acts as a catalytic oxidation intermediate, but also forms a surface water film on the catalyst surface through hydrogen-oxygen bonding. The water film can capture H2S and dissociate H2S into H + and HS - / S2 - (eq2-4); at the same time, Cu x VOs in O will catalyze part of H2O into OH (eq5-8); then, OH and adsorbed oxygen (*O2) will continue to oxidize HS - / S2 - Become S (eq9-12); the reactions involved are as follows:

[0057]

[0058] In the absence of Mg-coated materials, Cu compounds react with S anions, resulting in the deactivation of the catalyst. The chemical reaction equation is as follows:

[0059]

[0060] The Laves-like structure material of Mg-coated Cu (Cu2O and CuO are coated inside) formed by MgCu2O3 and Mg2Cu protects Cu ions from direct contact with S anions in this process. In this process, a water film is formed on the outer layer of the Mg coating layer, and part of the H2O enters the coating layer to complete the hydroxylation process of H2O. The alkaline sites of MgCu2O3 and Mg2Cu will enrich hydroxyl radicals in this process. The enriched hydroxyl radicals mainly have the following reactions: ① Catalyze HS - / S 2- Become S; ② Capture H in the reaction system + , buffering pH; the coating delays the deactivation of the catalyst, thereby greatly improving the desulfurization efficiency.

[0061] In addition, during this process, NO3 - With NO2 - With H in the system +Reacts with O2 to generate strong oxidizing nitric acid, which circulates to remove HS - / S 2- NH Group may also participate in HS - / S 2- removal.

[0062] The reactions involved are as follows:

[0063]

[0064] The reaction process does not produce any secondary polluting gas, and the tail gas can reach 0 pollutants.

[0065] The 20% concentration of NaOH solution is a protective measure to prevent gas pollution generated after the catalyst is deactivated.

[0066] Then, in a vertical tube furnace, N2 gas is used to purge the Mg-Cu / Al2O3 catalyst fully adsorbed with S, and the S in the purge tail gas is captured and recovered through the condenser; the amount of Mg-Cu / Al2O3 catalyst is 2.69g / L calculated by the amount of H2S gas introduced; the purge intensity of N2 is 120mL / min; the heating temperature of the Mg-Cu / Al2O3 catalyst is 180℃; the tail gas captured by the condenser is passed into a NaOH solution with a mass concentration of 20% by microporous aeration to purify the SO2 gas in the tail gas. This process is to sublimate the S element adsorbed on the catalyst at room temperature and then purge it to the condenser with N2 for recovery. In theory, there is no secondary pollutant gas, but there may be a small amount of sulfide and sulfate on the surface of the catalyst, and SO2 may be generated in the purge tail gas. Therefore, NaOH solution protection liquid is also required at the tail gas end to prevent secondary pollution. The gas after the NaOH solution does not need special treatment and can be discharged directly.

[0067] Example 5: This example is different from Example 4 in that the method for applying the Mg-Cu / Al2O3 catalyst to H2S gas treatment is as follows: H2S gas is mixed with water atomized gas to obtain a mixed gas, the humidity of the mixed gas is adjusted to 60%, the temperature of the mixed gas is adjusted to 40°C, the mixed gas is passed into a hammer reaction tower, and the mixed gas is passed through the Mg-Cu / Al2O3 catalyst to remove H2S;

[0068] The heating temperature of the Mg-Cu / Al2O3 catalyst was 200°C.

[0069] Example 6: This example is different from Example 4 in that the method for applying the Mg-Cu / Al2O3 catalyst to H2S gas treatment is as follows: H2S gas is mixed with water atomized gas to obtain a mixed gas, the humidity of the mixed gas is adjusted to 80%, the temperature of the mixed gas is adjusted to 60°C, the mixed gas is passed into a hammer reaction tower, and the mixed gas is passed through the Mg-Cu / Al2O3 catalyst to remove H2S;

[0070] The heating temperature of the Mg-Cu / Al2O3 catalyst was 230°C.

[0071] The comparative bar graph of the capture performance of a single gram of Mg-Cu / Al2O3 catalyst in Examples 4 to 6 is shown in FIG. Figure 7 As shown, by comparison, it can be seen that Example 6 has the best effect in treating H2S gas.

[0072] Example 7: Based on Example 6, Example 7 adjusts the humidity of the H2S gas to 60%.

[0073] Example 8: Based on Example 6, Example 8 adjusts the humidity of the H2S gas to 50%.

[0074] Example 9: Based on Example 6, Example 9 adjusts the humidity of the H2S gas to 70%.

[0075] The comparison of the amount of H2S gas that can be effectively treated per gram of catalyst at different humidity in Example 6-Example 9 is shown in the figure below. Figure 8 As shown, comparative examples 6 to 9, from Figure 8 It can be seen that when the humidity of H2S gas reaches 60%, the catalytic effect is the best, and the amount of H2S gas that can be effectively treated per gram of catalyst is the largest, so Example 7 is the best example.

Claims

1. An application of Mg-Cu / Al2O3 catalyst, characterized in that: The Mg-Cu / Al2O3 catalyst is applied to H2S gas treatment to convert H2S gas into S, and the S is recovered; The method of applying the Mg-Cu / Al2O3 catalyst to H2S gas treatment, converting H2S gas into S, and recovering S is as follows: mixing H2S gas with water atomized gas to obtain a mixed gas, adjusting the humidity of the mixed gas to 40-80%, adjusting the temperature of the mixed gas to 30-60°C, passing the mixed gas into a hammer reaction tower, allowing the mixed gas to pass through the Mg-Cu / Al2O3 catalyst to remove H2S, and then in a vertical tube furnace, purging the Mg-Cu / Al2O3 catalyst fully adsorbed with S with N2 gas, and capturing and recovering S in the purged tail gas through a condenser; The preparation method of the Mg-Cu / Al2O3 catalyst comprises the following steps: S1. Place Al2O3 particles in a Cu(NO3)2 solution to obtain a mixed solution, wherein the mass ratio of the Al2O3 particles to the Cu(NO3)2 solution is 1:4.75, and the mass percentage of the Cu(NO3)2 solution is 15.79%. The mixed solution is ultrasonically treated for 20-60 min, allowed to stand for 6-12 h, and then dried in a drying oven to obtain a mixture A. The temperature of the drying oven is 30-80°C, and the drying time is 30-100 min. Place the mixture A in a muffle furnace and calcine for 3-8 h. The calcination temperature of the muffle furnace is 300-600°C. After calcination, a Cu(3.1wt%) / Al2O3 catalyst is obtained; S2, Mg(NO3)2 and distilled water are prepared into a Mg(NO3)2 solution in a mass ratio of 2.1:10, and the Cu(3.1wt%) / Al2O3 catalyst is immersed in the Mg(NO3)2 solution for 6-12h to obtain a mixture B, wherein the mass ratio of the Cu(3.1wt%) / Al2O3 catalyst to the Mg(NO3)2 solution is 5:24.2; S3. Ultrasonic treatment of the mixture B for 20-30 min, drying in a drying oven, and calcining in a muffle furnace for 3-8 h. After calcination, a Mg-Cu / Al2O3 catalyst is obtained. The calcination temperature in the muffle furnace is 200-300°C.

2. The use of a Mg-Cu / Al2O3 catalyst as claimed in claim 1, characterized in that: The Al2O3 particles are mixed with Al2O3 particles with a particle size of 0.88-2 mm, Al2O3 particles with a particle size of 425-880 μm, and Al2O3 particles with a particle size of 270-425 μm in a mass ratio of 0.5-3:95-99:0.5-2.

3. The use of a Mg-Cu / Al2O3 catalyst as claimed in claim 1, characterized in that: Calculated based on the amount of H2S gas introduced, the amount of the Mg-Cu / Al2O3 catalyst used is 2.69 g / L.

4. The use of a Mg-Cu / Al2O3 catalyst as claimed in claim 1, characterized in that: The N2 purge intensity is 120 mL / min.

5. The use of a Mg-Cu / Al2O3 catalyst as claimed in claim 1, characterized in that: The heating temperature of the Mg-Cu / Al2O3 catalyst is 180-230°C.

6. The use of a Mg-Cu / Al2O3 catalyst as claimed in claim 1, characterized in that: The tail gas captured by the condenser is passed into a NaOH solution with a mass concentration of 20% by microporous aeration to purify the SO2 gas in the tail gas.