A forging method for high-performance difficult-to-deform titanium alloy
By adopting segmented heating and anti-oxidation coating treatment in titanium alloy forging, combined with multiple forging and straightening treatments, the problems of tissue unevenness and oxidation in titanium alloy forging are solved, and the strength and quality of titanium alloy rods are improved.
Patent Information
- Application Number
- CN202411067450.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-06
AI Technical Summary
The existing titanium alloy forging methods lead to uneven structure and performance during the plastic processing of titanium alloy, low strength, and easy oxidation and cracks during the heating process, affecting the quality of the finished product.
Using segmented heating and anti-oxidation coating treatment, pre-treated through laser cutting and electrostatic powder spraying technology, multiple forgings are performed using a fast forging machine and combined with water cooling and straightening treatment, controlling the forging ratio and temperature to avoid oxidation and cracks , improve uniformity and strength.
It effectively avoids oxidation and cracks of titanium alloy during forging, improves the structure and performance uniformity of titanium alloy rods, and enhances the strength and quality of the final product.
Smart Images

Figure CN118577734B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of titanium alloy forging, in particular to a forging method of a high-performance difficult-to-deform titanium alloy. Background Art
[0002] Forging is a processing method that uses a forging machine to apply pressure to a metal blank to cause it to undergo plastic deformation in order to obtain a forging with certain mechanical properties, shape, and size.
[0003] Titanium alloy is an alloy composed of titanium as the basis and other elements added. Titanium has two isomorphous crystals: titanium is an allotrope with a melting point of 1668°C. By utilizing the different characteristics of the above two structures of titanium and adding appropriate alloying elements, its phase transition temperature and component content are gradually changed to obtain titanium alloys with different structures; titanium alloy has the characteristics of heat resistance, strength, plasticity, toughness, formability, weldability, corrosion resistance and good biocompatibility, but due to the special properties of titanium alloy, its forging process is also relatively complicated and cumbersome.
[0004] The existing patent application number is CN202110234220.0, which is a forging method for titanium alloy bars. The method includes the following steps: blanking: select titanium alloy ingots that meet the standards, blank them into a baking furnace according to the process size, and remove the burrs on the end surface after blanking; forging heating: clean the ash in the furnace, place the titanium alloy ingot blanked into the baking furnace in an effective heating area and start heating, heat the temperature to 960±10°C, and the heating time does not exceed 90 minutes. Put the heated titanium alloy ingot into a warm charging furnace, keep it warm for 30 to 40 minutes, and then start forging;
[0005] The existing patent publication number is CN201510351434.0, which is a titanium alloy forging process, comprising the following steps: step 1: titanium alloy surface treatment, preheating at 110°C for 15 minutes, and applying a protective agent on the titanium alloy surface; step 2: charging the titanium alloy billet into a furnace and heating it at a temperature of 1000°C for 0.5 hours, then raising the furnace temperature to 1200°C and keeping it for 2 hours; step 3: forging the billet into shape; step 4: removing the surface protective agent after the billet is naturally cooled; step 5: inspecting the titanium alloy workpiece;
[0006] However, the existing titanium alloy forging methods still have some problems in practical use;
[0007] 1. The existing titanium alloy forging method and traditional process often cause the formation of texture during the plastic processing of titanium alloy, which leads to uneven organization and performance of bars or final parts, and cannot obtain high strength, affecting the final quality;
[0008] 2. The existing forging process is prone to oxidation of the titanium alloy ingot during the heating process. The existing anti-oxidation method is not ideal. At the same time, the existing heating method is prone to uneven heating, which can easily cause cracks in the titanium alloy billet during the forging process, affecting the cost quality of the overall workpiece.
[0009] Therefore, a forging method for a high-performance difficult-to-deform titanium alloy is needed to solve the above problems. Summary of the invention
[0010] The purpose of the present invention is to provide a forging method for a high-performance difficult-to-deform titanium alloy, so as to solve the problem that the existing titanium alloy forging process proposed in the above background technology is easy to cause the final product to have low strength and unsatisfactory mechanical properties, and at the same time cannot avoid the oxidation of the titanium alloy billet during the forging heating process and the occurrence of cracks during the forging process.
[0011] To achieve the above object, the present invention provides the following technical solution: a forging method for a high-performance difficult-to-deform titanium alloy, comprising the following steps:
[0012] S1. Pretreatment of titanium alloy materials: first, select titanium alloy materials with appropriate chemical composition and cut them into appropriate sizes according to requirements, then clean the dirt and oil on the surface of the ingot, preheat it and apply an anti-oxidation coating;
[0013] S2, heating the pretreated titanium alloy material; using a heating device to heat the cut ingot, and the subsequent heating of the ingot heater adopts a segmented heating method;
[0014] S3, forging of titanium alloy ingots: after heating the ingot, a fast forging machine is used to perform forging treatment, and the forging ratio of the forging to the titanium alloy ingot is controlled at 1.25-1.83, and water cooling is performed after forging is completed;
[0015] S4, intermediate forging; after further preheating and heat preservation of the billet obtained in the previous step for 3-4.5 hours, a fast forging machine is used for secondary forging, and the feed amount Lo is controlled at 0.7B-0.8B, and a total of 2-3 fires of forging are performed, and the billet is chamfered in the last fire;
[0016] S5, finished product forging; the blank obtained in the above step is subjected to rounding treatment, and the bar obtained by rounding is straightened by utilizing the residual heat.
[0017] Preferably, the titanium alloy ingot in S1 is cut by a laser cutting machine, and the anti-oxidation coating is mainly composed of 30% to 60% Si3N4 and 45% to 75% SiC, and 10% to 25% Fe, and the rest is one or more combinations of Al2O3, SiO2, MgO, and Cr2O3.
[0018] Preferably, the anti-oxidation coating in S1 is sprayed by powder electrostatic spraying at a spraying temperature of 300-800°C.
[0019] Preferably, the heating in S2 adopts three-stage heating. First, the heating equipment is heated to 800-850°C, and the ingot is placed inside the heating equipment for preheating. The preheating time is 1.5-2.5 hours, and then the temperature is increased for 2.5-3.5 hours. The heating temperature is 200°C to 300°C above the β phase transformation point. After the heating is completed, it is kept warm for 2-3.5 hours.
[0020] Preferably, the heating equipment adopts a natural gas furnace or a resistance furnace, and the distance between the ingot and the heat source is greater than 280 mm during heating to avoid uneven heating caused by local overheating.
[0021] Preferably, the stroke reduction of the blank forging in S3 is controlled at 70-90 mm, and when the temperature is 150°C lower than the β phase transformation point, the stroke reduction is gradually reduced to 40-60 mm, and the termination forging temperature is ≥850°C.
[0022] Preferably, the S4 further heats the forged billet in S3, and the heating adopts a three-stage heating method as above, the heating temperature is 100°C to 150°C above the β phase transformation point, the interruption temperature of each fire is 100-150°C below the β phase transformation point, the forging ratio of each fire is controlled between 3-6, and the chamfer of the billet in the last fire in S4 is one of octal or twelve.
[0023] Preferably, the feed amount Lo in S4 is B (hammer head width)×(0.7-0.8), and the forging downward force is ≤3 / 5Lo.
[0024] Preferably, in S5, the blank in the previous step is heated to 50-100°C below the β phase transformation point, and rounding forging is performed using a flat anvil and a V-shaped anvil on a fast forging machine. After rounding, the blank is straightened using the residual temperature, and the straightening temperature is not lower than 150-200°C below the β phase transformation point. After straightening, the curvature of the titanium alloy bar is not greater than 4mm / m.
[0025] Compared with the prior art, the beneficial effects of the present invention are: the forging method of the high-performance difficult-to-deform titanium alloy;
[0026] 1. By applying an anti-oxidation coating before heating, severe oxidation of the titanium alloy can be avoided during the heating process, thereby improving the forging quality at a low cost. The three-stage heating method is used to ensure the heating uniformity of the titanium alloy billet, avoid cracks in the titanium alloy billet during the forging process, and reasonably control the forging ratio at different stages to improve the overall forging quality.
[0027] 2. By reasonably controlling the initial forging temperature and the final forging temperature, increasing the forging deformation in the β phase region, improving the forging ratio, and reasonably controlling the feed amount and the downward pressure of the forging press at different forging stages, the large-sized cast grains at the edge and middle of the titanium alloy billet can be fully broken, the grain size in the core of the titanium alloy billet can be reduced, the uniformity of the overall organization and performance can be improved, and the overall strength and organizational performance of the final titanium alloy bar can be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The process flow chart of titanium alloy forging of the present invention is as follows;
[0029] Figure 2 It is a schematic diagram of the three-stage heating curve of the present invention. DETAILED DESCRIPTION
[0030] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] Example 1
[0032] The technical solution of the present invention is a forging method of a high-performance difficult-to-deform titanium alloy, comprising the following steps:
[0033] S1. Pretreatment of titanium alloy materials: first, select titanium alloy materials with appropriate chemical composition and cut them into appropriate sizes according to requirements, then clean the dirt and oil on the surface of the ingot, preheat it and apply an anti-oxidation coating;
[0034] The titanium alloy ingot in S1 is cut by a laser cutting machine. The main components of the anti-oxidation coating are 30% Si3N4 and 45% SiC, as well as 15% Fe, and the rest is a combination of 10% SiO2 and Cr2O3;
[0035] The anti-oxidation coating in S1 is sprayed by powder electrostatic spraying, and the spraying temperature is 300-800℃
[0036] S2, heating the pretreated titanium alloy material; using a heating device to heat the cut ingot, and the subsequent heating of the ingot heater adopts a segmented heating method;
[0037] The heating in S2 adopts three-stage heating. First, the heating equipment is heated to 800°C, and the ingot is placed inside the heating equipment for preheating. The preheating time is 2.5 hours, and then the temperature is increased for heating. The heating time is 2.5 hours. The heating temperature is 250°C above the β phase transformation point. After the heating is completed, the temperature is kept for 2.5 hours.
[0038] The heating equipment uses a natural gas furnace or a resistance furnace, and the distance between the ingot and the heat source is greater than 280mm during heating to avoid uneven heating caused by local overheating.
[0039] S3, forging of titanium alloy ingots: after heating the ingot, a fast forging machine is used to perform forging treatment, and the forging ratio of the forging to the titanium alloy ingot is controlled at 1.25-1.83, and water cooling is performed after forging is completed;
[0040] In S3, the stroke reduction of the forging process is controlled at 80mm, and when the temperature is 150℃ lower than the β phase transformation point, the stroke reduction is gradually reduced to 60mm, and the termination forging temperature is ≥850℃.
[0041] S4, intermediate forging; after further preheating and heat preservation of the billet obtained in the previous step for 3-4.5 hours, a fast forging machine is used for secondary forging, and the feed amount Lo is controlled at 0.8B, and a total of 2-3 fires of forging are performed, and the billet is chamfered in the last fire;
[0042] S4 further heats the forged billet in S3. The heating is the same as above, using a three-stage heating method. The heating temperature is 120°C above the β phase transformation point, the interruption temperature of each fire is 150°C below the β phase transformation point, and the forging ratio of each fire is controlled between 6. In S4, the chamfer of the billet in the last fire is octagonal.
[0043] In S4, the feed amount Lo is B (hammer head width) × 0.8, and the forging pressure amount is ≤ 3 / 5Lo.
[0044] S5, finished product forging; the blank obtained in the above step is subjected to rounding treatment, and the bar obtained by rounding is straightened by using the residual heat;
[0045] In S5, the blank in the previous step is heated to 80°C below the β phase transformation point, and rounding forging is performed using a flat anvil and a V-shaped anvil on a fast forging machine. After rounding, the blank is straightened using the residual heat. The straightening temperature is not lower than 180°C below the β phase transformation point. After straightening, the curvature of the titanium alloy bar is not greater than 4mm / m.
[0046] Example 2
[0047] The technical solution of the present invention is a forging method of a high-performance difficult-to-deform titanium alloy, comprising the following steps:
[0048] S1. Pretreatment of titanium alloy materials: first, select titanium alloy materials with appropriate chemical composition and cut them into appropriate sizes according to requirements, then clean the dirt and oil on the surface of the ingot, preheat it and apply an anti-oxidation coating;
[0049] The titanium alloy ingot in S1 is cut by a laser cutting machine. The main components of the anti-oxidation coating are 40% Si3N4 and 35% SiC, as well as 20% Fe, and the rest is a combination of 5% Al2O3, SiO2, and Cr2O3;
[0050] The anti-oxidation coating in S1 is sprayed by powder electrostatic spraying at a temperature of 400°C.
[0051] S2, heating the pretreated titanium alloy material; using a heating device to heat the cut ingot, and the subsequent heating of the ingot heater adopts a segmented heating method;
[0052] The heating in S2 adopts three-stage heating. First, the heating equipment is heated to 850°C, and the ingot is placed inside the heating equipment for preheating. The preheating time is 2 hours, and then the temperature is increased for 3 hours. The heating temperature is 250°C above the β phase transformation point. After the heating is completed, the temperature is kept for 3 hours.
[0053] The heating equipment uses a natural gas furnace or a resistance furnace, and the distance between the ingot and the heat source is greater than 280mm during heating to avoid uneven heating caused by local overheating.
[0054] S3, forging of titanium alloy ingots: after heating the ingot, a fast forging machine is used to perform forging treatment, and the forging ratio of the forging to the titanium alloy ingot is controlled at 1.25-1.83, and water cooling is performed after forging is completed;
[0055] In S3, the stroke reduction of the open forging process is controlled at 80mm, and when the temperature is 150℃ lower than the β phase transformation point, the stroke reduction is gradually reduced to 50mm, and the termination forging temperature is ≥850℃.
[0056] S4, intermediate forging; after further preheating and heat preservation of the billet obtained in the previous step for 3-4.5 hours, a fast forging machine is used for secondary forging, and the feed amount Lo is controlled at 0.75B. A total of 3 fires are performed, and the billet is chamfered in the last fire;
[0057] S4 further heats the forged billet in S3, and the heating adopts a three-stage heating method as above, the heating temperature is 150°C above the β phase transformation point, the interruption temperature of each fire is 100°C below the β phase transformation point, and the forging ratio of each fire is controlled between 5. The chamfer of the billet in the last fire in S4 is twelve squares;
[0058] In S4, the feed amount Lo is B (hammer head width) × (0.75), and the forging pressure amount is ≤3 / 5Lo.
[0059] S5, finished product forging; the blank obtained in the above step is subjected to rounding treatment, and the bar obtained by rounding is straightened by using the residual heat;
[0060] In S5, the blank in the previous step is heated to 80°C below the β phase transformation point, and is forged by using a flat anvil and a V-shaped anvil on a fast forging machine. After the rounding is completed, the blank is straightened by using the residual temperature. The straightening temperature is not less than 200°C below the β phase transformation point. After the straightening is completed, the curvature of the titanium alloy bar is not more than 4mm / m
[0061] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
[0062] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
[0063] In summary, the above description of the disclosed embodiments enables professionals and technicians in the field to implement or use the present invention. Various modifications to these embodiments will be apparent to professionals and technicians in the field, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but should conform to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A forging method for a high-performance hard-to-deform titanium alloy, characterized in that: The following steps are involved: S1. Pretreatment of titanium alloy materials: first, select titanium alloy materials with appropriate chemical composition and cut them into appropriate sizes according to requirements, then clean the dirt and oil on the surface of the ingot, preheat it and apply an anti-oxidation coating; S2, heating the pretreated titanium alloy material; using a heating device to heat the cut ingot, and the subsequent heating of the ingot heating machine adopts a segmented heating method. The heating in S2 adopts a three-stage heating method. First, the heating device is heated to 800-850°C, and the ingot is placed inside the heating device for preheating. The preheating time is 1.5-2.5 hours, and then the temperature is increased for heating. The heating time is 2.5-3.5 hours. The heating temperature is 200°C to 300°C above the β phase transformation point. After the heating is completed, it is kept warm for 2-3.5 hours; S3, open forging of titanium alloy ingot; after heating the ingot, the open forging process is performed by a fast forging machine, the forging ratio of the open forging to the titanium alloy ingot is controlled at 1.25-1.83, and water cooling is performed after the forging is completed. In S3, the stroke reduction of the open forging is controlled at 70-90 mm, and when the temperature is 150°C lower than the β phase transformation point, the stroke reduction is gradually reduced to 40-60 mm, and the termination forging temperature is ≥850°C; S4, intermediate forging; after further preheating and heat preservation of the billet obtained in the previous step for 3-4.5 hours, a fast forging machine is used for secondary forging, and the feed amount Lo is controlled at 0.7B-0.8B, and a total of 2-3 fires of forging are performed, and the billet is chamfered in the last fire; S5, finished product forging; the blank obtained in the above step is subjected to rounding treatment, and the bar obtained by rounding is straightened by using the residual heat; The S4 further heats the forged blank in S3, and the heating adopts a three-stage heating method as above, the heating temperature is 100°C to 150°C above the β phase transformation point, the interruption temperature of each fire is 100-150°C below the β phase transformation point, and the forging ratio of each fire is controlled between 3-6. The chamfer of the blank in the last fire in S4 is one of eight sides or twelve sides; The feed amount Lo in S4 is B (hammer head width) × (0.7-0.8), and the forging pressure amount is ≤3 / 5Lo.
2. A forging method for a high-performance difficult-to-deform titanium alloy according to claim 1, characterized in that: The titanium alloy ingot in S1 is cut by a laser cutting machine. The main components of the anti-oxidation coating are 30% to 60% Si3N4 and 45% to 75% SiC, as well as 10% to 25% Fe, and the rest are one or more combinations of Al2O3, SiO2, MgO, and Cr2O3.
3. A forging method for a high-performance difficult-to-deform titanium alloy according to claim 2, characterized in that: The anti-oxidation coating in S1 is sprayed by powder electrostatic spraying at a temperature of 300-800°C.
4. The forging method of a high-performance difficult-to-deform titanium alloy according to claim 1, characterized in that: The heating equipment adopts one of a natural gas furnace or a resistance furnace, and during heating, the distance between the ingot and the heat source is greater than 280 mm to avoid uneven heating caused by local overheating.
5. The forging method of a high-performance difficult-to-deform titanium alloy according to claim 1, characterized in that: In S5, the blank in the previous step is heated to 50-100° C. below the β phase transformation point, and rounding forging is performed using a flat anvil and a V-shaped anvil on a fast forging machine. After rounding, the blank is straightened using the residual temperature. The straightening temperature is not lower than 150-200° C. below the β phase transformation point. After straightening, the curvature of the titanium alloy bar is not greater than 4 mm / m.
Citation Information
Cited By
Titanium alloy cast ingot aluminum layer coating equipment and method based on electric arc spraying
CN122382501A