Method for preparing amorphous nano ferric oxide by taking manganese extraction slag as raw material and application of amorphous nano ferric oxide

Preparation of amorphous nanoferrous oxide by sulfuric acid calcination and microwave hydrothermal method has solved the problem of high cost of manganese slag waste utilization and amorphous nanoferrous oxide preparation, and achieved efficient and low-cost resource recycling and electricity Preparation of materials with excellent chemical properties.

CN118993157APending Publication Date: 2024-11-22NORTHEASTERN UNIV AT QINHUANGDAO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411078606.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The prior art is difficult to effectively utilize manganese slag-raising waste, and the method of preparing amorphous nano iron trioxide is expensive and complicated, so it cannot adapt to situations where the iron content changes greatly.

Method used

The manganese slag is calcined by sulfuric acid to obtain an iron sulfate solution, and amorphous nanoferric oxide is prepared by microwave hydrothermal method, simplifying the process and reducing costs, and is suitable for slag with high and low iron content.

Benefits of technology

It has achieved efficient secondary resource utilization for manganese slag extraction, and prepared amorphous nanoferrous oxide with excellent electrochemical performance, which is suitable for supercapacitors and other fields, reducing environmental pollution and energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993157A_ABST
    Figure CN118993157A_ABST
Patent Text Reader

Abstract

The invention provides a method for preparing amorphous nano ferric oxide by taking manganese extraction slag as a raw material and application of the amorphous nano ferric oxide, and belongs to the technical field of mineral processing and efficient utilization of wastes. The method comprises the following steps: (1) roasting a mixed material containing manganese extraction slag and acid to obtain roasted clinker; (2) dissolving out the roasted clinker to obtain a dissolved-out material; (3) mixing with a precipitant, and stirring at constant temperature in a water bath kettle to obtain a precursor; and (4) carrying out microwave heating on the precursor to obtain the amorphous nano ferric oxide. The method for preparing the amorphous nano ferric oxide by using the ferric sulfate solution obtained by roasting the manganese extraction residues with the sulfuric acid is simple, convenient and easy to implement and low in cost, not only realizes high value-added utilization of secondary resources of the manganese extraction residues, but also reduces discharge of wastes, and the amorphous nano Fe2O3 prepared by a microwave hydrothermal method has a good application prospect and is suitable for industrial production. The method can be used in the fields of supercapacitor materials and the like, and provides new technology and theoretical support for efficient utilization of secondary resources of the manganese extraction slag.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of mineral processing and waste efficient utilization, and in particular to a method for preparing amorphous nano-iron sesquioxide by using manganese extraction slag as raw material and application thereof. Background Art

[0002] Manganese slag is a solid waste generated in the process of extracting manganese from manganese-containing ores. For example, the manganese slag after extracting manganese from pyrolusite mainly contains SiO2 and Fe2O3, as well as a small amount of manganese, aluminum, barium and strontium, and has a high value of comprehensive utilization of secondary resources. The manganese slag is stored by damming or discharged into landfills, which not only occupies a large area of ​​arable land resources, but also pollutes the environment. Therefore, seeking efficient recycling methods for secondary resources and carrying out high value-added utilization of manganese slag waste can not only make effective use of resources, but also improve the economic benefits of enterprises and reduce pollution to the environment. It is of great significance to the optimal allocation of manganese ore resources and the sustainable development of enterprises.

[0003] In the prior art, the main methods used to extract iron from iron-containing slag are wet leaching, reduction roasting-magnetic separation, biomass pyrolysis, etc. Wet leaching requires a large amount of acid and has high requirements for equipment; reduction roasting requires the addition of reducing substances and the roasting temperature is relatively high; the reduction order of Fe2O3 in the biomass pyrolysis method is a step-by-step transformation of Fe2O3→Fe3O4→FeO→Fe. Although it is low-cost and environmentally friendly, the process is relatively complicated and the cycle is relatively long. In addition, the above methods are mainly aimed at the case where the iron content in the iron-containing slag is high, such as iron ore, red mud, and laterite nickel ore acid leaching slag. Therefore, it is also necessary to explore an economically reasonable method for extracting manganese slag and iron that can adapt to large changes in iron content.

[0004] Fe2O3 is widely used in many fields because of its abundant resources, low production cost, non-toxicity and environmental friendliness. Compared with conventional Fe2O3, nano-Fe2O3 shows better performance, better chemical reactivity, gas sensitivity, electrochemical performance and semiconductor characteristics, as well as stronger catalytic activity, and has broad application prospects. In some advanced applications, the amorphous nature and large surface area of ​​the Fe2O3 phase are necessary. Compared with the crystal structure, amorphous Fe2O3 has the advantages of small particle size, long-range disorder, good dispersibility and large specific surface area, which makes it have stronger catalytic activity, more superior optical, magnetic, electrochemical and adsorption properties, and shows great application potential in modern nanotechnology, such as solar energy conversion, electrochemistry, adsorption purification, catalysis and humidity sensors.

[0005] In recent years, the synthesis of amorphous Fe2O3 has made great progress, and researchers have successfully synthesized amorphous nano-Fe2O3 using different methods. At present, the main methods for preparing amorphous Fe2O3 are sol-gel method, precipitation method, microemulsion method, microwave irradiation method, thermal decomposition method, ultrasonic chemical synthesis method, etc. However, the preparation of these amorphous ferric oxides all uses analytical pure chemical reagents as raw materials, and some also add surfactants, templates, etc., which is relatively costly.

[0006] In the prior art, the raw materials of the microwave hydrothermal method are more commonly iron-containing chemical reagents such as FeCl3, Fe(NO3)3 and alkaline precipitants. The reaction principle is to first convert trivalent iron salt into α-FeOOH or Fe(OH)3, and then regenerate Fe2O3. The experimental method is to heat a beaker or a round-bottom flask in a microwave oven. However, different raw materials, methods, system pH value, concentration, temperature and other reaction conditions will affect the morphology and crystallinity of the product, and thus amorphous ferric oxide cannot be obtained. Therefore, the art is in urgent need of a method for preparing a novel amorphous ferric oxide nanomaterial. Summary of the invention

[0007] In view of the above problems existing in the prior art, the present invention provides a method and application for preparing amorphous nano-iron trioxide using manganese extraction slag as raw material. The present invention uses the ferric sulfate solution obtained by roasting the manganese extraction slag with sulfuric acid to prepare amorphous nano-iron trioxide, which is simple and easy to operate with low cost, not only realizing the high added value utilization of the secondary resources of manganese extraction slag, but also reducing the discharge of waste. The amorphous nano-Fe2O3 prepared by the microwave hydrothermal method has good application prospects and can be used in the fields of supercapacitor materials, etc., providing new technology and theoretical support for the efficient utilization of the secondary resources of manganese extraction slag.

[0008] The technical solution of the present invention is as follows:

[0009] A method for preparing amorphous nano-iron oxide using manganese extraction slag as raw material, the method comprising the following steps:

[0010] (1) Mixing: mixing the manganese extraction slag with concentrated sulfuric acid and deionized water to obtain a mixed material;

[0011] Preferably, the concentration of the concentrated sulfuric acid in step (1) is 98%; the mass ratio of the concentrated sulfuric acid to the manganese extraction slag is 2-5:1, and the volume ratio of the water to the concentrated sulfuric acid is 0.4-1.0:1.

[0012] More preferably, the mass ratio of the concentrated sulfuric acid to the manganese extraction slag in step (1) is 2.5:1, 3:1, 3.5, 4:1 or 4.5:1, etc.

[0013] More preferably, the volume ratio of water to acid in step (1) is 0.4:1, 0.5:1, 0.6:1, 0.7:1, 0.8:1 or 0.9:1, etc.

[0014] Furthermore, the volume ratio of water to concentrated sulfuric acid in step (1) of the present invention is most preferably 0.6:1. The use of water can increase the activity of the reaction between concentrated sulfuric acid and manganese extraction slag. If the volume ratio of water to concentrated sulfuric acid is greater than 0.6:1, the mixed material is easy to splash during the roasting process, and the sulfuric acid concentration is reduced, and the iron extraction rate is reduced; if the volume ratio is less than 0.6:1, the fluidity of the system is reduced, thereby reducing the reaction contact area, which is not conducive to the reaction.

[0015] (2) calcining: calcining the mixture at 250-600° C. for 0.5-4 h to obtain calcined material;

[0016] Preferably, the calcination temperature in step (2) is 250°C, 350°C, 450°C, 550°C, 565°C or 580°C, etc.

[0017] Preferably, the calcination time in step (2) is 0.5 h, 1 h, 1.5 h, 2 h, 3 h, or 3.5 h.

[0018] Furthermore, when sulfuric acid is used to roast iron, part of the sulfuric acid will decompose to produce SO2 and SO3 gases. The sulfur trioxide tail gas produced by the roasting in step (2) is absorbed by sulfuric acid with a mass fraction of 60-70% and used to replace the concentrated sulfuric acid in step (1).

[0019] More preferably, the sulfur trioxide tail gas generated after the roasting in step (2) is absorbed by sulfuric acid with a mass fraction of 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68% or 69%.

[0020] (3) dissolution: mixing the roasted clinker with deionized water and stirring to obtain a dissolution material;

[0021] Preferably, in step (3), the mass ratio of the roasted clinker to deionized water is 1:4-8; the stirring conditions are: stirring temperature is 85-95°C, stirring speed is 200-400r / min, and stirring time is 30-60min.

[0022] More preferably, the mass ratio of the roasted clinker to water in step (3) is 1:5, 1:6 or 1:7, etc.

[0023] More preferably, the temperature of the dissolution process in step (3) is 86°C, 87°C, 88°C, 89°C, 90°C, 91°C, 92°C, 93°C or 94°C, etc.

[0024] More preferably, the stirring speed of the dissolution process in step (3) is 220 r / min, 250 r / min, 300 r / min, 350 r / min or 380 r / min, etc.

[0025] More preferably, the dissolution process in step (3) takes 32 min, 35 min, 38 min, 40 min, 42 min, 45 min, 50 min or 55 min.

[0026] (4) separation: performing solid-liquid separation on the dissolved material to obtain a filtrate and a filter residue, washing the filter residue with water, and mixing the washing liquid obtained after washing with the filtrate to obtain a ferric sulfate solution;

[0027] Preferably, the solid-liquid separation in step (4) is a commonly used operation in the art, and a typical but non-limiting solid-liquid separation method may be filtration or the like.

[0028] (5) placing the ferric sulfate solution in a constant temperature water bath at 25-40° C., slowly adding the ammonia solution into the ferric sulfate solution, and stirring to obtain a precursor solution;

[0029] Preferably, the water bath temperature in step (5) is 25°C, 28°C, 30°C, 32°C or 35°C, etc.

[0030] Preferably, in step (5), the mass ratio of NH3·H2O in the aqueous ammonia solution to ferric sulfate in the ferric sulfate solution is 1.5-4:1; the stirring speed is 200-300 r / min, and the stirring time is 20-40 min.

[0031] Preferably, the ammonia solution in step (5) is prepared by mixing commercially available concentrated ammonia water and water in a ratio of 1:4, wherein the concentration of the commercially available concentrated ammonia water is 25% to 28%.

[0032] More preferably, the mass ratio of NH3·H2O in the ammonia solution to ferric sulfate in the ferric sulfate solution in step (5) is 1.8:1, 2.0:1, 2.5:1, 3.0:1, 3.2:1, 3.5:1 or 3.8:1, etc.

[0033] More preferably, the stirring speed in step (5) is 220 r / min, 240 r / min, 260 r / min or 280 r / min, etc.

[0034] More preferably, the water bath heating time, i.e. the stirring time, in step (5) is 25 min, 28 min, 30 min, 32 min, 35 min or 38 min, etc.

[0035] (6) subjecting the precursor solution to a microwave hydrothermal reaction at 120-180° C. for 15-45 min to obtain a reaction product;

[0036] Preferably, the container for the microwave hydrothermal reaction in step (6) is a closed transparent reaction kettle.

[0037] More preferably, the temperature of the microwave heating in step (6) is 130°C, 140°C, 150°C, 160°C or 170°C, etc.

[0038] More preferably, the heating time in step (6) is 20 min, 25 min, 30 min, 35 min or 40 min, etc.

[0039] (7) The reaction product is cooled and filtered, washed with deionized water and dried, and then calcined at 100-500° C. for 0.5-4 h to obtain amorphous nano-iron oxide.

[0040] Preferably, the drying temperature in step (7) is 80-120° C. and the drying time is 3-6 hours.

[0041] More preferably, the drying temperature in step (7) is 85°C, 90°C, 95°C, 100°C, 105°C, 110°C or 115°C, etc.

[0042] More preferably, the drying time in step (7) is 3.5 h, 4 h, 4.5 h, 5 h or 5.5 h, etc.

[0043] More preferably, the calcination temperature in step (7) is 200°C, 250°C, 300°C, 350°C, 400°C or 450°C, etc.

[0044] More preferably, the calcination time in step (7) is 1 h, 2 h, 2.5 h, 3 h, 3.5 h or 3.8 h.

[0045] The present invention also provides amorphous nano-iron oxide prepared by the method, wherein the iron oxide is an amorphous particle with a diameter of 10-100 nm. Further, the diameter of the iron oxide nanoparticles prepared in step (7) is 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm or 90 nm.

[0046] The present invention further provides the application of amorphous nano-iron sesquioxide prepared by the method, wherein the iron sesquioxide is applied to any one of new energy materials, catalytic materials, new magnetic materials, and adsorption purification materials, or a combination of at least two of them.

[0047] The present invention further provides a supercapacitor, wherein the electrode material of the supercapacitor is the amorphous nano-iron sesquioxide described above.

[0048] The manganese extraction slag in the above step (1) is a solid waste obtained after manganese is extracted from low-grade pyrolusite and / or high-grade pyrolusite. The pyrolusite of the present invention may also be high-grade pyrolusite, but high-grade pyrolusite is currently in short supply in China. In order to comprehensively utilize resources, low-grade pyrolusite is preferably used.

[0049] The main components of manganese extraction slag are silicon dioxide and ferric oxide. Since silicon dioxide does not react with sulfuric acid, the roasting temperature in the present invention is relatively low. The iron extraction rate reaches more than 80% at 250°C. Theoretically, the decomposition temperature of ferric sulfate is 480°C, and this raw material contains a large amount of silicon dioxide. Iron and silicon are associated together, resulting in a wider extraction temperature, up to 600°C.

[0050] In the present invention, the conversion process of iron is:

[0051] Fe2O3+2H2SO4+6H2O=Fe2(H2O)4[(SO4)2O](H2O)4

[0052] Fe2(H2O)4[(SO4)2O](H2O)4+H2SO4=Fe2(SO4)3+9H2O↑

[0053] The present invention adopts a method combining pyrometallurgy and wet method to extract iron element, with fast reaction rate and high extraction rate. Compared with the traditional wet reduction, the present invention has less acid usage, low equipment corrosion, simple operation, easy control, and less waste discharge; compared with the traditional pyrometallurgy reduction, the present invention has lower roasting temperature, reduced energy consumption, cost saving, and less environmental pollution. The iron extraction method of the present invention is suitable for slag with high and low iron content, and the concentration of iron ions in the prepared ferric sulfate solution does not have much effect on the performance of the subsequent preparation of ferric oxide, thus expanding the application scope of this method.

[0054] In the above step (5), ammonia water is a precipitant. Different precipitants will affect the morphology of the product ferric oxide. The inventors have used NaOH as a precipitant, but failed to prepare amorphous ferric oxide, but obtained α-Fe2O3. In addition, α-FeOOH was not detected in the intermediate product of the microwave hydrothermal method of the present invention, and only a very small amount of amorphous FeOOH was detected.

[0055] In the above step (6), the mixed solution is placed in a closed reactor, and then placed in a single-mode microwave synthesizer for reaction. A magnetron is placed in the reactor, accompanied by magnetic stirring. The reactor is a special reactor for equipment, with a maximum tolerance temperature of 240°C and a maximum tolerance pressure of 3MPa.

[0056] All parts of the reactor are made of microwave transparent materials to ensure that microwaves directly irradiate the reaction samples and the samples in the reactor fully absorb microwave energy and are heated. The reactor has good corrosion resistance and can meet the reaction conditions of most reactions. Its completely closed structure does not cause loss of samples and volatile components during the reaction process. High temperature and high pressure can accelerate the reaction process and promote the completion of certain reactions.

[0057] In addition, the single-mode microwave synthesizer uses advanced single-mode technology. Microwaves are emitted from the wave source at an oscillation frequency of 2450 MHz per second, transmitted through the waveguide, enter the reaction chamber in a single mode, and are transmitted in a certain direction in the reactor to form a microwave field with uniform energy, ensuring that the reaction system heats up quickly and is heated evenly.

[0058] The beneficial technical effects of the present invention are:

[0059] 1. The method for preparing amorphous nano-iron trioxide from manganese slag as raw material does not use any surfactant, template and iron-containing chemical reagent, and prepares amorphous nano-iron trioxide with excellent electrochemical performance by adjusting the experimental conditions. The preparation process is simple, easy to operate, less polluting, economically reasonable, and realizes the resource recycling and reuse of waste, reduces environmental pollution, and turns waste into treasure, providing new technology and theoretical support for the efficient and comprehensive utilization of secondary resources of manganese slag.

[0060] 2. The present invention uses the method to prepare ferric sulfate solution, and the iron extraction rate can reach more than 97%; the prepared ferric oxide product is amorphous nanoparticles, with good product performance and stable and controllable quality. The high added value utilization of manganese slag solid waste by the present invention can not only make effective use of resources, but also improve the economic benefits of enterprises, reduce pollution to the environment, and has important significance for the optimal allocation of manganese ore resources and the sustainable development of enterprises.

[0061] 3. The single-mode microwave synthesizer used in the present invention has the following advantages:

[0062] (1) Single-mode microwave technology: standing wave single-mode microwave output, microwave morphology is consistent and better coupled with the sample, with higher energy density, ensuring heating uniformity and experimental repeatability;

[0063] (2) Rapid cooling system: Reasonable cooling air duct design ensures that the cooling gas can quickly and comprehensively cool the reaction bottle, and the reaction temperature can be cooled to a safe temperature within a few minutes.

[0064] (3) Magnetic stirring system: The rotation speed is faster and more stable, making the stirring of various emulsions, suspensions, solid-liquid mixtures and some low-viscosity substances more uniform.

[0065] The above characteristics are conducive to the preparation of amorphous nanoparticles. Since amorphous Fe2O3 has the advantages of small particle size, long-range disorder, good dispersibility and large specific surface area, it exhibits many unique characteristics and has great application prospects. This patent uses manganese slag as raw material, and cleverly combines hydrothermal conditions with microwave heating. It has excellent characteristics such as high reaction efficiency, fast speed, uniform heating, high recovery rate, high sample purity, more uniform morphology, energy saving and environmental protection, and simple operation. It is simple and easy, low cost, and the prepared amorphous Fe2O3 can be applied to multiple high-tech fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0066] Figure 1 The XRD and SEM images of the iron oxide prepared in Example 1;

[0067] Figure 2 The XRD and SEM images of the iron oxide prepared in Example 2;

[0068] Figure 3 This is the infrared spectrum of the ferric oxide prepared in Example 2;

[0069] Figure 4 The nitrogen adsorption-desorption isotherm diagram of the ferric oxide prepared in Example 2;

[0070] Figure 5 This is the SEM image of the ferric oxide prepared in Example 7;

[0071] Figure 6 This is the SEM image of the ferric oxide prepared in Comparative Example 1;

[0072] Figure 7 The XRD and SEM images of the iron oxide prepared in Comparative Example 2;

[0073] Figure 8 XRD diagrams of Comparative Examples 3, 4, and 5;

[0074] Fig. 9 These are the SEM images of Comparative Examples 3, 4, and 5. DETAILED DESCRIPTION

[0075] The present invention is described in detail below in conjunction with the accompanying drawings and embodiments. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0076] The performance testing methods used in the following embodiments are:

[0077] 1. Calculation of iron extraction rate: The calculation formula is:

[0078]

[0079] Wherein: η(Fe) is the extraction rate of iron, %; m(Fe, liquid) is the mass of iron in the dissolution solution, g; m(Fe, solid) is the mass of iron in the manganese extraction slag, g.

[0080] 2. Crystal phase analysis: Use X-ray diffractometer (XRD) to perform phase analysis to determine the physical form of ferric oxide.

[0081] 3. Morphology analysis: Scanning electron microscopy (SEM) was used to analyze the morphology of the ferric oxide material.

[0082] 4. Specific surface area analysis: Use a specific surface area tester (BET) to test the specific surface area of ​​ferric oxide material.

[0083] 5. Assembly and capacity test of supercapacitor: The prepared Fe2O3 powder, acetylene black and the prepared 5% PVDF (polyvinylidene fluoride) solution were mixed evenly in a solid mass ratio of 8:1:1, and then an appropriate amount of NMP (N-methylpyrrolidone) was added to the mixture and ground into a flowing slurry. The mixed slurry was evenly coated on the dried nickel foam to make a working electrode, a platinum sheet was used as a counter electrode, a saturated calomel electrode was used as a reference electrode, and 3M KOH was used as an electrolyte to assemble a three-stage supercapacitor. The constant current charge and discharge curve of the manganese dioxide sample was tested at a current density of 0.5A / g using a Solartron 1260+1287 electrochemical workstation, and its specific capacitance was calculated.

[0084] Embodiment 1:

[0085] This embodiment provides a method for preparing amorphous nano-iron sesquioxide, comprising the following steps:

[0086] (1) Weigh 10 g of manganese extraction slag; the manganese extraction slag is a solid waste obtained after manganese extraction from low-grade pyrolusite, and the specific composition is shown in Table 1 below:

[0087] Table 1

[0088] Element <![CDATA[SiO2]]> <![CDATA[Fe2O3]]> MnO <![CDATA[Al2O3]]> SrO BaO CaO Content (100%) 81.33 12.73 1.46 1.11 0.60 0.23 0.09

[0089] The manganese extraction slag, deionized water and 98% concentrated sulfuric acid are mixed, wherein the mass ratio of the concentrated sulfuric acid to the manganese extraction slag is 3:1, and the volume ratio of the water to the concentrated sulfuric acid is 1.0:1, to obtain a mixed material.

[0090] (2) roasting the mixed material at 550° C. for 0.5 hours to obtain roasted clinker; and absorbing the sulfur trioxide tail gas generated by the roasting with sulfuric acid having a mass fraction of 60% to replace the concentrated sulfuric acid in step (1).

[0091] (3) The roasted clinker was mixed with deionized water in a mass ratio of 1:4, and dissolved at 95° C. and a stirring speed of 300 r / min for 30 min to obtain a dissolved material.

[0092] (4) filtering the dissolved material to separate the solid from the liquid to obtain a filtrate and a filter residue, washing the filter residue with deionized water, and mixing the washing liquid obtained after washing with the filtrate to obtain a ferric sulfate solution.

[0093] (5) The ferric sulfate solution is placed in a constant temperature water bath at 40° C., 25% commercially available concentrated ammonia water and water are mixed in a ratio of 1:4 to prepare an ammonia solution, which is slowly added to the ferric sulfate solution and stirred at a speed of 300 r / min for 40 min. The mass ratio of NH3·H2O in the ammonia solution to ferric sulfate in the ferric sulfate solution is 4:1.

[0094] (6) The mixed solution was placed in a sealed transparent reaction vessel in a single-mode microwave synthesizer, and subjected to microwave hydrothermal reaction at 120° C. for 45 min to obtain a reaction product.

[0095] (7) The reaction product is cooled and filtered, the filtered material is washed with deionized water and then dried at 120° C. for 3 h, and then calcined at 400° C. for 2 h to obtain a ferric oxide sample.

[0096] Figure 1 The XRD and SEM images of the prepared ferric oxide are shown in Figure 1. Figure 1 It can be seen from the figure that the ferric oxide is amorphous nanoparticles.

[0097] Embodiment 2:

[0098] This embodiment provides a method for preparing amorphous nano-iron sesquioxide, comprising the following steps:

[0099] (1) Weigh 10 g of manganese extraction slag; the composition of the manganese extraction slag is the same as that of Example 1.

[0100] The manganese extraction slag, deionized water and 98% concentrated sulfuric acid are mixed, wherein the mass ratio of the concentrated sulfuric acid to the manganese extraction slag is 5:1, and the volume ratio of the water to the concentrated sulfuric acid is 0.6:1, to obtain a mixed material.

[0101] (2) roasting the mixed material at 565° C. for 2 hours to obtain roasted clinker; and absorbing the sulfur trioxide tail gas generated by the roasting with sulfuric acid having a mass fraction of 65% and then using it to replace the concentrated sulfuric acid in step (1).

[0102] (3) The roasted clinker was mixed with deionized water in a mass ratio of 1:6, and dissolved at 90° C. and a stirring speed of 250 r / min for 45 min to obtain a dissolved material.

[0103] (4) filtering the dissolved material to separate the solid from the liquid to obtain a filtrate and a filter residue, washing the filter residue with water, and mixing the washing liquid obtained after washing with the filtrate to obtain a ferric sulfate solution.

[0104] (5) The ferric sulfate solution is placed in a constant temperature water bath at 30° C., 28% commercially available concentrated ammonia water and water are mixed in a ratio of 1:4 to prepare an ammonia solution, which is slowly added to the ferric sulfate solution and stirred at a speed of 200 r / min for 20 min. The mass ratio of NH 3 ·H 2 O in the ammonia solution to the ferric sulfate in the ferric sulfate solution is 3:1.

[0105] (6) The mixed solution was placed in a sealed transparent reaction vessel in a single-mode microwave synthesizer, and subjected to microwave hydrothermal reaction at 180° C. for 30 min to obtain a reaction product.

[0106] (7) The reaction product is cooled and filtered, the filtered material is washed with deionized water and then dried at 80° C. for 6 h, and then calcined at 400° C. for 4 h to obtain a ferric oxide sample.

[0107] Figure 2 The XRD and SEM images of the prepared ferric oxide are shown in Figure 1. Figure 2 It can be seen from the figure that the ferric oxide is an amorphous material and the particles are relatively uniform.

[0108] Figure 3 is the infrared spectrum of the sample. Figure 3 Medium 3421cm -1 The broad absorption peak at 1630 cm -1 The small absorption peak at 1049-1117 cm -1 The weak absorption peak in the range is caused by the vibration of the SO bond in the sulfate ion, indicating that there is a small amount of SO4 in the system during the formation of Fe2O3 2- Adsorbed on the surface of sample particles; at 1443cm -1 The small absorption peak at 592cm corresponds to the vibration of CO bond, which may be due to the adsorption of CO2 in the air by Fe2O3 sample; -1The significant absorption peak at can be attributed to the vibration of Fe-O bonds. The results show that there are Fe-O bonds and OH bonds in the Fe2O3 product, thus confirming the formation of Fe2O3 compounds.

[0109] Figure 4 The adsorption-desorption isotherm of the sample shows an obvious hysteresis loop, which belongs to the IV type isotherm. Its hysteresis loop is steep and narrow, and the closing point is near p / p0=0.2, which belongs to the H1 type hysteresis loop, indicating that the material is a cylindrical uniform mesoporous material with a narrow pore size distribution. Its specific surface area is 194.95m 2 ·g -1 .

[0110] Embodiment 3:

[0111] The difference from Example 2 is that the calcination temperature in step (2) is 250° C., and the obtained ferric oxide is an amorphous nanomaterial.

[0112] Embodiment 4:

[0113] The difference from Example 2 is that the mass ratio of the concentrated sulfuric acid to the manganese extraction slag in step (1) is 2:1, and the obtained ferric oxide is an amorphous nanomaterial.

[0114] Embodiment 5:

[0115] The difference from Example 2 is that the mass ratio of the ammonia water to the ferric sulfate in the ferric sulfate solution in step (5) is 2:1, and the obtained ferric oxide is an amorphous nanomaterial.

[0116] Embodiment 6:

[0117] The difference from Example 2 is that the microwave hydrothermal reaction time in step (6) is 15 minutes, and the reaction product obtained is an amorphous nanomaterial of ferric oxide.

[0118] Embodiment 7:

[0119] The difference from Example 2 is that the calcination temperature in step (7) is 100° C. and the calcination time is 0.5 h to obtain a reaction product. Figure 5 This is a SEM image of the prepared ferric oxide. It can be seen from the image that although the ferric oxide particles obtained are slightly irregular in shape and partially agglomerated, the obtained ferric oxide is still an amorphous nanomaterial.

[0120] Embodiment 8:

[0121] This embodiment provides a method for preparing amorphous nano-iron sesquioxide, comprising the following steps:

[0122] (1) Weigh 10 g of manganese extraction slag; the composition of the manganese extraction slag is the same as that of Example 1.

[0123] The manganese extraction slag, deionized water and 98% concentrated sulfuric acid are mixed, wherein the mass ratio of the concentrated sulfuric acid to the manganese extraction slag is 4:1, and the volume ratio of the water to the concentrated sulfuric acid is 0.4:1, to obtain a mixed material.

[0124] (2) roasting the mixed material at 600° C. for 4 hours to obtain roasted clinker, and absorbing the sulfur trioxide tail gas generated by the roasting with sulfuric acid having a mass fraction of 70% and then using it to replace the concentrated sulfuric acid in step (1).

[0125] (3) The roasted clinker was mixed with deionized water in a mass ratio of 1:8, and dissolved at 85° C. and a stirring speed of 200 r / min for 60 min to obtain a dissolved material.

[0126] (4) filtering the dissolved material to separate the solid from the liquid to obtain a filtrate and a filter residue, washing the filter residue with water, and mixing the washing liquid obtained after washing with the filtrate to obtain a ferric sulfate solution.

[0127] (5) The ferric sulfate solution is placed in a constant temperature water bath at 25° C., 25% commercially available concentrated ammonia water and water are mixed in a ratio of 1:4 to prepare an ammonia solution, which is slowly added to the ferric sulfate solution and stirred at a speed of 250 r / min for 30 min. The mass ratio of NH 3 ·H 2 O in the ammonia solution to ferric sulfate in the ferric sulfate solution is 1.5:1.

[0128] (6) The mixed solution was placed in a sealed transparent reaction vessel in a single-mode microwave synthesizer, and subjected to microwave hydrothermal reaction at 150° C. for 45 min to obtain a reaction product.

[0129] (7) The reaction product is cooled and filtered, the filtered material is washed with deionized water and then dried at 100° C. for 4 h, and then calcined at 500° C. for 2 h to obtain an amorphous nano-iron oxide material.

[0130] Comparative Example 1:

[0131] The difference from Example 2 is that the ferric sulfate solution in step (5) is placed in a constant temperature water bath at 60°C. Figure 6 This is a SEM image of the prepared ferric oxide. It can be seen from the image that the obtained ferric oxide particles are seriously agglomerated.

[0132] Comparative Example 2:

[0133] The difference from Example 2 is that the calcination temperature in step (7) is 750°C. Figure 7The XRD and SEM images of the prepared ferric oxide show that the calcination temperature of the obtained ferric oxide is too high, and it changes from an amorphous state to α-Fe2O3 (JCPDS No.33-0664). The sample morphology has changed significantly, the particles are spherical, the surface is firm and smooth, the boundaries are clear, and the particle size increases.

[0134] Comparative Example 3:

[0135] The difference from Example 2 is that the precipitant in step (5) is a NaOH solution, and the mass ratio of NaOH in the NaOH solution to ferric sulfate in the ferric sulfate solution is 4:1.

[0136] Comparative Example 4:

[0137] The difference from Comparative Example 3 is that in step (5), in addition to adding the precipitant NaOH solution during the preparation of ferric oxide, a small amount of PVP (polyvinyl pyrrolidone) surfactant is also added.

[0138] Comparative Example 5:

[0139] The difference from Comparative Example 3 is that in step (5), in addition to adding the precipitant NaOH solution, a small amount of PEG (polyethylene glycol)-2000 surfactant is also added during the preparation of ferric oxide.

[0140] The XRD patterns and SEM images of Comparative Examples 3, 4 and 5 are shown in Table 1. Figure 8 and Fig. 9 As shown in the figure, it can be seen that the ferric oxide sample prepared using NaOH solution as a precipitant is α-Fe2O3, which corresponds to the standard card PDF#89-0597 of hematite (syn). After adding a surfactant, the particle agglomeration phenomenon is slightly improved, but agglomeration still exists.

[0141] Test example:

[0142] In the above embodiments and comparative examples, the iron extraction rate from manganese extraction slag and the specific surface area and specific capacitance of the obtained ferric oxide are shown in Table 2.

[0143] Table 2

[0144] Iron extraction rate (%) Specific capacitance (F / g) <![CDATA[Specific surface area (m 2 / g)]]> Example 1 90.25 375 125.65 Example 2 97.45 500 194.95 Example 3 84.52 438 167.32 Example 4 86.53 465 185.52 Example 5 96.87 447 188 Example 6 97.15 395 134 Example 7 97.36 405 137.14 Example 8 90.12 390 158.72 Comparative Example 1 97.32 270 100.17 Comparative Example 2 97.10 54 8.72 Comparative Example 3 97.50 103 19.46 Comparative Example 4 97.86 189 40.51 Comparative Example 5 97.33 206 46.01

[0145] It can be seen from Table 2 that the iron extraction roasting temperature and the mass ratio of concentrated sulfuric acid to pyrolusite have a great influence on the iron extraction rate. The water bath temperature for preparing the ferric oxide precursor and the calcination temperature of the product have a significant influence on its specific surface area and electrochemical properties. The mass ratio of ammonia water to ferric sulfate and the microwave hydrothermal reaction time also have a great influence on the specific surface area and electrochemical properties of the ferric oxide product.

[0146] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and implementation modes, and can be fully applicable to various fields suitable for the present invention. For those familiar with the art, for those of ordinary skill in the art, various changes, modifications, substitutions and variations can be made to these embodiments without departing from the principle and spirit of the present invention. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to specific details.

Claims

1. A method for preparing amorphous nano-iron oxide using manganese extraction slag as raw material, characterized in that: The method comprises the following steps: (1) Mixing: mixing the manganese extraction slag with concentrated sulfuric acid and deionized water to obtain a mixed material; (2) calcining: calcining the mixture at 250-600° C. for 0.5-4 h to obtain calcined material; (3) dissolution: mixing the roasted clinker with deionized water and stirring to obtain a dissolution material; (4) separation: performing solid-liquid separation on the dissolved material to obtain a filtrate and a filter residue, washing the filter residue with water, and mixing the washing liquid obtained after washing with the filtrate to obtain a ferric sulfate solution; (5) placing the ferric sulfate solution in a constant temperature water bath at 25-40° C., slowly adding the ammonia solution into the ferric sulfate solution, and stirring to obtain a precursor solution; (6) subjecting the precursor solution to a microwave hydrothermal reaction at 120-180° C. for 15-45 min to obtain a reaction product; (7) The reaction product is cooled and filtered, washed with deionized water and dried, and then calcined at 100-500° C. for 0.5-4 h to obtain amorphous nano-iron oxide.

2. The method according to claim 1, characterized in that The concentration of the concentrated sulfuric acid in step (1) is 98%; the mass ratio of the concentrated sulfuric acid to the manganese extraction slag is 2-5:1, and the volume ratio of the water to the concentrated sulfuric acid is 0.4-1.0:

1.

3. The method according to claim 1, characterized in that: The sulfur trioxide tail gas generated by the roasting in step (2) is absorbed by sulfuric acid with a mass fraction of 60-70% and then used to replace the concentrated sulfuric acid in step (1).

4. The method according to claim 1, characterized in that: In step (3), the mass ratio of the roasted clinker to deionized water is 1:4-8; the stirring conditions are: stirring temperature is 85-95°C, stirring speed is 200-400r / min, and stirring time is 30-60min.

5. The method according to claim 1, characterized in that In step (5), the mass ratio of NH3·H2O in the ammonia solution to ferric sulfate in the ferric sulfate solution is 1.5-4:1; the stirring speed is 200-300 r / min, and the stirring time is 20-40 min.

6. The method according to claim 1, characterized in that The container for the microwave hydrothermal reaction in step (6) is a closed transparent reaction kettle.

7. The method according to claim 1, characterized in that The drying temperature in step (7) is 80-120° C. and the drying time is 3-6 hours.

8. Amorphous nano-iron oxide prepared by the method according to any one of claims 1 to 7, characterized in that: The ferric oxide is amorphous particles with a diameter of 10-100 nm.

9. The use of amorphous nano-iron oxide prepared by the method according to any one of claims 1 to 7, characterized in that: The ferric oxide is applied to any one of new energy materials, catalytic materials, new magnetic materials, and adsorption purification materials, or a combination of at least two of them.

10. A supercapacitor, characterized in that: The electrode material of the supercapacitor comprises the iron oxide as claimed in claim 9.