A novel release film and preparation method thereof

By using fluorine-containing functional polymer release agents and hexagonal boron nitride in the release film, the problem of easy disengagement of release films in the existing technology in the high temperature and high humidity environment is solved, and a higher membrane base is achieved Combined strength and comprehensive performance.

CN118578736BActive Publication Date: 2024-11-26ZHEJIANG JUMAY SPECIAL MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411062594.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-26
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

The existing release films are prone to disengage in high temperature and high humidity environments, and the poor interface compatibility and additive migration problems caused by the application method affect their binding strength and durability.

Method used

Using fluorine-containing functional polymer release agents and hexagonal boron nitride and other materials, the release layer is prepared by uniform stirring and extrusion granulation technology, and high-temperature molten film is combined with the substrate to enhance the film-based bonding strength and high-temperature resistance. .

Benefits of technology

The stability, bonding strength and comprehensive performance of the release film are improved, ensuring that it is not easy to detach under high temperature environments, and has excellent thermal shrinkage and mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118578736B_ABST
    Figure CN118578736B_ABST
Patent Text Reader

Abstract

The present invention discloses a novel release film, comprising a substrate, on which a release layer is provided. The hexagonal boron nitride in the release layer of the present invention has the function of strengthening the high temperature resistance of the film, and the use of a fluorine-containing functional polymer release agent not only has a positive reinforcing effect of interface bonding in the release layer itself, but also has better adhesion and bonding with the substrate during lamination and compounding, so that the overall stability and bonding strength of the release film are higher. For the substrate, a mixed coupling agent additive system is used to make it have better high temperature resistance and heat insulation effect, and the polyester surface of the substrate forms an easy-to-combine surface layer with active groups, which can be better compounded with the release layer, thereby making it have better film-base bonding strength and peeling strength as a whole.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of release film preparation, and more particularly to a novel release film and a preparation method thereof. Background Art

[0002] Release film, also known as peeling film, isolation film, separation film, etc., refers to a film with a separable surface. Usually, in order to increase the release force of plastic film, the plastic film will be plasma treated, fluorine treated, or coated with a silicone release agent on the surface of the film material, such as PET, PE, OPP, etc.; so that it can show extremely light and stable release force for various organic pressure-sensitive adhesives, such as hot melt adhesives, acrylic adhesives and rubber-based pressure-sensitive adhesives. According to the different release forces required for the release film, the viscosity of the isolation product adhesive is different, and the release force is adjusted accordingly to achieve an extremely light and stable release force when peeling. The release film has no stickiness or slight stickiness after contact with specific materials under limited conditions. Release films are widely used in packaging, printing, silk screen, pad printing, nameplates, membrane switches, flexible circuits, insulation products, circuit boards, laser anti-counterfeiting, lamination, electronics, sealing material films, reflective materials, waterproof materials, medicine (plaster paper), sanitary paper, adhesive products, die-cutting and punching processing and other industries.

[0003] The patent document with the patent number CN111423609A discloses an intrinsic antistatic release film base film and its application. The antistatic release film base film is made of modified HDPE, and the modified HDPE includes the following raw materials: olefinic compounds and quaternary ammonium salts containing double bonds. The prior art prepares an intrinsic antistatic release film base film by doping polymerizable quaternary ammonium salts in high-density polyethylene polymerization monomers. Quaternary ammonium salts are excellent cationic antistatic agents, which are uniformly dispersed in the resin to form a path to leak static charge. The groups with antistatic function will not migrate and will not be stuck away, thus playing the role of intrinsic antistatic. In the prior art, a small amount of quaternary ammonium salts containing two or more carbon-carbon double bonds are added to the comonomer of the modified HDPE, which not only has the effect of improving the antistatic performance of the modified HDPE, but also unexpectedly finds that it has the effect of improving the antistatic property of the release film under high temperature and high humidity environment.

[0004] Patent document with patent number CN110028853 A discloses a release agent, a non-silicone release film containing the release agent, and a method for manufacturing the same. The main component of the release agent is a polyvinyl ester compound to avoid the silicon migration problem in silicone release agents. However, the main component of the release agent is a polyvinyl ester compound, and its specific preparation method has not been published. Patent document with patent number CN111393699A discloses a flame retardant release film and a method for preparing the same. The release agent is added with an alcohol hydroxyl flame retardant, and the alcohol hydroxyl reacts with the isocyanate in the bridging agent under heating to successfully graft the flame retardant onto the silicone polymer with a certain binding force with the base film, which can greatly reduce the migration and precipitation of the flame retardant, thereby achieving a long-lasting flame retardant effect. The release agent has a flame retardant effect, but does not improve the base material of the release film.

[0005] The release film of the prior art is obtained by applying a release agent on the surface of a substrate. For granular fillers or additives with poor interface compatibility, the application method will result in obvious protruding particles, which can easily cause the release agent to be loosely bonded to the substrate and easily detached. It will also cause part of the release agent to remain on the surface of the product when the release film is removed, causing changes in the working performance of the product surface. In view of this, we disclose a method for preparing a novel release film. On the basis of meeting various functional requirements of the release film, the substrate and the release layer are improved to prepare a release film with strong functionality, high film-base bonding strength, and high comprehensive performance. Summary of the invention

[0006] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a new type of release film, including a substrate and a release layer. Under the premise that the substrate itself or the release layer itself is stable, the release layer is firmly bonded to the substrate and is not easy to separate, and it has excellent comprehensive properties such as high temperature resistance, heat shrinkage performance and mechanical properties.

[0007] To achieve the above object, the present invention proposes the following technical solutions:

[0008] A novel release film comprises a substrate, a release layer is provided on the substrate, and the release layer comprises the following raw material components by weight:

[0009] 100-130 parts of mixed resin;

[0010] 10-15 parts of hexagonal boron nitride;

[0011] 5.5-10 parts of fluorine-containing functional polymer release agent;

[0012] 0.5-0.8 parts of polyquaternium salt;

[0013] Wherein, the mixed resin comprises the following raw materials in parts by weight:

[0014] Polypropylene 56-70 parts;

[0015] 13-15 parts of glycidyl methacrylate grafted polypropylene;

[0016] Polyethylene 24-30 parts;

[0017] Ethylene-methyl methacrylate copolymer 7-15 parts.

[0018] On the basis of the above solution and as a preferred solution of the above solution, the thickness of the release layer is 0.1-1 mm.

[0019] On the basis of the above scheme and as a preferred scheme of the above scheme, the substrate includes the following raw materials in parts by weight: 85-95 parts of PET polyester particles, 10-15 parts of polypropylene grafted maleic anhydride, and 5-10 parts of a mixture of phosphate coupling agent, silica aerogel and (2,4-difluorophenyl)trimethylsilane.

[0020] On the basis of the above scheme and as a preferred scheme of the above scheme, the mass ratio of phosphate coupling agent, silica aerogel and (2,4-difluorophenyl)trimethylsilane in the mixture of phosphate coupling agent, silica aerogel and (2,4-difluorophenyl)trimethylsilane is (0.7-0.9): (0.5-0.8):1.

[0021] On the basis of the above scheme and as a preferred scheme of the above scheme, the preparation method of the novel release film comprises the following steps:

[0022] A. Preparation of substrate: a mixture of phosphate coupling agent and (2,4-difluorophenyl)trimethylsilane is prepared into a 0.5wt% coupling agent aqueous solution, and then the PET polyester particles in the substrate are immersed in the coupling agent aqueous solution, continuously stirred for 1-4 hours, and vacuum dried; then the dried PET polyester particles and polypropylene grafted maleic anhydride are mixed and stirred, and then conveyed to a screw extruder, and clamped by a cooling roller and a pressure roller to obtain a dry substrate;

[0023] B. Substrate surface treatment: clean the impurities on the substrate surface, and perform anti-static treatment on the substrate, then evenly spray the coupling agent aqueous solution on the dry substrate surface, and obtain the pre-treated base paper after natural drying;

[0024] C. Prepare a mixed masterbatch of the release layer, mix the mixed resin, hexagonal boron nitride, fluorine-containing functional polymer release agent, and polyquaternary ammonium salt in proportion using a blender, and send them into a twin-screw extruder for extrusion granulation, cooling, and drying to obtain a mixed masterbatch;

[0025] D. Put the mixed masterbatch into the screw again. The molten material from the extrusion section of the screw passes through the filter plate of the die head to turn the original vortex-shaped material into a flat flow, and then enters the laminating machine mold to be split to both ends and become flakes. After the uniform flakes flow out, they enter the process of compounding with the substrate.

[0026] E. The high-temperature molten film of the sheet passes through the clamping of the cooling roller and the pressure roller, so that it adheres to the substrate and cools rapidly to obtain the initial product of the release film;

[0027] F. The initial release film product is subjected to corona pretreatment, super calendering and drying treatments in sequence, and then pulled into the finished product winding machine to obtain the release film.

[0028] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:

[0029] The present invention discloses a novel release film, comprising a substrate, on which a release layer is provided. The hexagonal boron nitride in the release layer of the present invention has the function of strengthening the high temperature resistance of the film, and the use of a fluorine-containing functional polymer release agent not only has a positive reinforcing effect of interface bonding in the release layer itself, but also has better adhesion and bonding with the substrate during lamination and compounding, so that the overall stability and bonding strength of the release film are higher. For the substrate, a mixed coupling agent additive system is used to make it have better high temperature resistance and heat insulation effect, and the polyester surface of the substrate forms an easy-to-combine surface layer with active groups, which can be better compounded with the release layer, thereby making it have better film-base bonding strength and peeling strength as a whole. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0031] Figure 1 It is a schematic diagram of the synthesis reaction of the fluorine-containing functional polymer release agent of the present invention. DETAILED DESCRIPTION

[0032] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the described embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Unless otherwise defined, the technical terms or scientific terms used herein should be the common meanings understood by people with general skills in the field to which the present invention belongs.

[0033] The words "first", "second" and similar words used in the patent application specification and claims of the present invention do not indicate any order, quantity or importance, but are only used to distinguish different components. Similarly, unless the context clearly indicates otherwise, the singular form of "a", "an" or "the" and other similar words do not indicate a quantitative limitation, but indicate the existence of at least one. "Include" or "comprise" and other similar words mean that the elements or objects appearing before "include" or "comprise" cover the features, wholes, steps, operations, elements and / or components listed after "include" or "comprise", and do not exclude the existence or addition of one or more other features, wholes, steps, operations, elements, components and / or their collections. "Up", "down", "left", "right" and the like are only used to indicate relative positional relationships. When the absolute position of the described object changes, the relative positional relationship may also change accordingly.

[0034] Generally, release film is obtained by applying release agent on the surface of substrate. Release agent mainly includes silicon-containing release agent, non-silicone release agent and emerging fluorine-containing release agent. Silicone release agent has low cost and is suitable for most application fields, but silicon-containing release agent has the problem of silicon migration, which easily leads to the mismatch between film-base bonding strength, peeling strength and use requirements. Therefore, the use of fluorine-containing release agent is the current mainstream choice. In order to solve the problems of traditional release agent, we use fluorine-containing functional polymer for modification. Fluorine-containing functional polymer release agent is a new functional structure with symmetrical effect formed by a connecting group connecting two or four traditional molecules through chemical bonds. In this way, it can meet the normal use of fluorine-containing release agent while also having strong film-base bonding strength, and the usage amount is lower than that of traditional fluorine-containing release agent.

[0035] The synthesis of the fluorine-containing functional polymer release agent of the present invention comprises two stages: intermediate synthesis and synthesis of the fluorine-containing functional polymer release agent.

[0036] Phase I: Intermediate synthesis.

[0037] Using ethylenediamine and epifluoropropane as raw materials and anhydrous ethanol as solvent, epifluoropropane replaces four active hydrogen atoms on the nitrogen atom of ethylenediamine during the reaction, and epifluoropropane undergoes a ring-opening reaction. The specific reaction process is: weigh ethylenediamine and epifluoropropane according to the molar mass ratio, place ethylenediamine and anhydrous ethanol with a mass ratio of 2:5 in a three-necked flask, and then use a dropping funnel containing epifluoropropane to drop epifluoropropane into the three-necked flask at a dropping speed of 0.5mL / min; at the same time, control the speed of the constant speed stirrer at 300r / min, gradually increase the temperature to the reaction temperature of 80℃ at a heating rate of 5℃ / min, start timing and maintain the reaction temperature, and react for at least 6h; after the reaction, remove excess raw materials and solvents with a rotary evaporator to obtain an intermediate.

[0038] Phase II: Synthesis of fluorine-containing functional polymer release agent.

[0039] The cycloheptyl tertiary amine reacts with the prepared intermediate under the condition of anhydrous ethanol and deionized water as solvents, and the F atom on the intermediate is attacked and replaced by the N atom in the cycloheptyl tertiary amine to generate a fluorine-containing polyquaternary ammonium salt release agent. The specific reaction process is as follows: a certain amount of the intermediate of the first stage is put into a three-necked flask, anhydrous ethanol is added into the three-necked flask at a mass ratio of the intermediate to anhydrous ethanol of 1:2, and the mixture is stirred at a stirring speed of 300 r / min; then, cycloheptyl tertiary amine is put into a dropping funnel at a molar ratio of the intermediate to cycloheptyl tertiary amine of 1:3, the dropping speed is adjusted, and the dropping speed is 0.5 mL / min, and the stirring speed is 300 r / min; a segmented heating method is adopted, firstly, the temperature is gradually increased to 80°C at a heating rate of 10°C / min, and after keeping the temperature for 10 minutes, the temperature is gradually increased to 120°C at a heating rate of 5°C / min, and the reaction is completed after 20 minutes, and the excess raw materials and solvents are removed by a rotary evaporator, and the fluorine-containing functional polymer release agent is obtained by vacuum drying.

[0040] After calculation, the yield of the above fluorine-containing functional polymer release agent synthesis reaction is 89.1%. The dried fluorine-containing functional polymer release agent is placed in a vacuum drying oven for standby use. The use of the fluorine-containing functional polymer release agent in the release layer is beneficial to its high temperature resistance and heat insulation performance by utilizing its larger steric hindrance and multi-quaternary ammonium salt structure. Compared with the fluorine-containing release agent of the prior art, the fluorine-containing functional polymer release agent of the present invention has a higher film-based bonding strength with the substrate.

[0041] Further, in the present invention, the hexagonal boron nitride used is the simplest boron-nitrogen polymer. Hexagonal boron nitride is similar to the hexagonal carbon network in graphite. Nitrogen and boron in hexagonal boron nitride also form hexagonal mesh layers, overlapping each other to form crystals. Boron nitride is resistant to high temperatures, has extremely stable chemical properties, and is resistant to strong acid corrosion. It is mainly used for refractory materials, semiconductor solid-phase doping sources, structural materials for atomic piles, packaging materials for neutron radiation protection, rocket engine components, high-temperature lubricants and release agents. During use, the hexagonal boron nitride is dried after being impregnated with a 0.5wt%-2.5wt% siloxane coupling agent alcohol solution. Preferably, the hexagonal boron nitride of the present invention is obtained by treating with a 0.75wt% 3-aminopropyltriethoxysilane coupling agent alcohol solution, and the dried hexagonal boron nitride is ground into 1000 mesh particles through a quartz mortar for standby use. In the alcohol solution, the hexagonal boron nitride powder settles downwards. During the treatment with the alcohol solution of 3-aminopropyltriethoxysilane coupling agent, there will be a short-term flocculent emulsion state of the solution. Such treatment not only helps its surface activation, but also helps the uniform dispersion of the hexagonal boron nitride in other matrices. Untreated hexagonal boron nitride and the hexagonal boron nitride treated by the present invention are blended with PP and then injection molded into dumbbell-shaped strips. After liquid nitrogen brittle fracture, the cross section is observed by field emission scanning electron microscopy. The untreated hexagonal boron nitride is obviously separated from the PP matrix interface.

[0042] Performance testing and requirements

[0043] Surface performance

[0044] The apparent performance test includes two aspects: instrument detection or human sensory (such as hand pressing) test. The hardness of the film roll can be uniform by instrument detection or hand pressing. The film roll is visually flat, the end surface is neat and burr-free, and clean. A single film is visually flat under normal light, and there are no defects, scratches, foreign matter, etc. that affect use under strong light.

[0045] Performance requirements

[0046] The release film performance test is carried out according to different test standards. The test reference standards and performance requirements are shown in Table 1.

[0047] Table 1 Performance test requirements of release film

[0048]

[0049] Example 1

[0050] A novel release film comprises a substrate, a release layer is provided on the substrate, and the release layer comprises the following raw material components by weight:

[0051] Mixed resin 116 parts;

[0052] 13 parts of hexagonal boron nitride;

[0053] 7 parts of fluorine-containing functional polymer release agent;

[0054] 0.6 part of polyquaternium salt;

[0055] Wherein, the mixed resin comprises the following raw materials in parts by weight:

[0056] Polypropylene 70 parts;

[0057] 15 parts of glycidyl methacrylate grafted polypropylene;

[0058] 24 parts of polyethylene;

[0059] Ethylene-methyl methacrylate copolymer 7 parts.

[0060] Further, the substrate comprises the following raw materials in parts by weight: 90 parts of PET polyester particles, 13 parts of polypropylene grafted maleic anhydride, and 7 parts of a mixture of a phosphate coupling agent, a silica aerogel and (2,4-difluorophenyl)trimethylsilane. Preferably, the mass ratio of the phosphate coupling agent, the silica aerogel and (2,4-difluorophenyl)trimethylsilane in the mixture of the phosphate coupling agent, the silica aerogel and (2,4-difluorophenyl)trimethylsilane is 0.7:0.8:1.

[0061] In this embodiment, a method for preparing a novel release film comprises the following steps:

[0062] A. Preparation of substrate: a mixture of phosphate coupling agent and (2,4-difluorophenyl)trimethylsilane is prepared into a 0.5wt% coupling agent aqueous solution, and then the PET polyester particles in the substrate are immersed in the coupling agent aqueous solution, stirred continuously for 3 hours, and vacuum dried; then the dried PET polyester particles and polypropylene grafted maleic anhydride are mixed and stirred, and then conveyed to a screw extruder, and clamped by a cooling roller and a pressure roller to obtain a dry substrate;

[0063] B. Substrate surface treatment: clean the impurities on the substrate surface, and perform anti-static treatment on the substrate, then evenly spray the coupling agent aqueous solution on the dry substrate surface, and obtain the pre-treated base paper after natural drying;

[0064] C. Prepare a mixed masterbatch of the release layer, mix the mixed resin, hexagonal boron nitride, fluorine-containing functional polymer release agent, and polyquaternary ammonium salt in proportion using a blender, and send them into a twin-screw extruder for extrusion granulation, cooling, and drying to obtain a mixed masterbatch;

[0065] D. Put the mixed masterbatch into the screw again. The molten material from the extrusion section of the screw passes through the filter plate of the die head to turn the original vortex-shaped material into a flat flow, and then enters the laminating machine mold to be split to both ends and become flakes. After the uniform flakes flow out, they enter the process of compounding with the substrate.

[0066] E. The high-temperature molten film of the sheet passes through the clamping of the cooling roller and the pressure roller, so that it adheres to the substrate and cools rapidly to obtain the initial product of the release film;

[0067] F. The initial release film product is subjected to corona pretreatment, super calendering and drying treatments in sequence, and then pulled into the finished product winding machine to obtain the release film.

[0068] Example 2

[0069] Different from the above-mentioned embodiment 1, a novel release film comprises a substrate, a release layer is provided on the substrate, and the release layer comprises the following raw material components in parts by weight:

[0070] 100 parts of mixed resin;

[0071] 10 parts of hexagonal boron nitride;

[0072] 5.5 parts of fluorine-containing functional polymer release agent;

[0073] 0.5 part of polyquaternium salt;

[0074] Wherein, the mixed resin comprises the following raw materials in parts by weight:

[0075] Polypropylene 56 parts;

[0076] 13 parts of glycidyl methacrylate grafted polypropylene;

[0077] 24 parts of polyethylene;

[0078] Ethylene-methyl methacrylate copolymer 7 parts.

[0079] Further, the substrate comprises the following raw materials in parts by weight: 85 parts of PET polyester particles, 10 parts of polypropylene grafted maleic anhydride, and 5 parts of a mixture of a phosphate coupling agent, a silica aerogel and (2,4-difluorophenyl)trimethylsilane. Preferably, the mass ratio of the phosphate coupling agent, the silica aerogel and (2,4-difluorophenyl)trimethylsilane in the mixture of the phosphate coupling agent, the silica aerogel and (2,4-difluorophenyl)trimethylsilane is 0.9:0.5:1.

[0080] Example 3

[0081] Different from the above-mentioned embodiment 1, a novel release film comprises a substrate, a release layer is provided on the substrate, and the release layer comprises the following raw material components in parts by weight:

[0082] 130 parts of mixed resin;

[0083] 15 parts of hexagonal boron nitride;

[0084] 10 parts of fluorine-containing functional polymer release agent;

[0085] 0.8 part of polyquaternium salt;

[0086] Wherein, the mixed resin comprises the following raw materials in parts by weight:

[0087] Polypropylene 70 parts;

[0088] 15 parts of glycidyl methacrylate grafted polypropylene;

[0089] 30 parts of polyethylene;

[0090] 15 parts of ethylene-methyl methacrylate copolymer.

[0091] Further, the substrate comprises the following raw materials in parts by weight: 95 parts of PET polyester particles, 15 parts of polypropylene grafted maleic anhydride, and 10 parts of a mixture of a phosphate coupling agent, a silica aerogel and (2,4-difluorophenyl)trimethylsilane. Preferably, the mass ratio of the phosphate coupling agent, the silica aerogel and (2,4-difluorophenyl)trimethylsilane in the mixture of the phosphate coupling agent, the silica aerogel and (2,4-difluorophenyl)trimethylsilane is 0.9: 0.8:1.

[0092] Comparative Example 1

[0093] Different from Example 1, the substrate includes the following raw materials in parts by weight: 90 parts of PET polyester particles, 13 parts of polypropylene grafted maleic anhydride, and 7 parts of a mixture of silica aerogel and (2,4-difluorophenyl)trimethylsilane. Preferably, the mass ratio of silica aerogel to (2,4-difluorophenyl)trimethylsilane in the mixture of silica aerogel and (2,4-difluorophenyl)trimethylsilane is 0.8:1.

[0094] Other processes and materials used refer to Example 1.

[0095] Comparative Example 2

[0096] Different from Example 1, the substrate includes the following raw materials in parts by weight: 90 parts of PET polyester particles, 13 parts of polypropylene grafted maleic anhydride, and 7 parts of a mixture of a phosphate coupling agent and (2,4-difluorophenyl)trimethylsilane. Preferably, the mass ratio of the phosphate coupling agent to (2,4-difluorophenyl)trimethylsilane in the mixture of the phosphate coupling agent and (2,4-difluorophenyl)trimethylsilane is 0.7:1.

[0097] Other processes and materials used refer to Example 1.

[0098] Comparative Example 3

[0099] Different from Example 1, a novel release film includes a substrate, a release layer is provided on the substrate, and the release layer includes the following raw material components by weight:

[0100] Mixed resin 116 parts;

[0101] 7 parts of fluorine-containing functional polymer release agent;

[0102] 0.6 part of polyquaternium salt;

[0103] Wherein, the mixed resin comprises the following raw materials in parts by weight:

[0104] Polypropylene 70 parts;

[0105] 15 parts of glycidyl methacrylate grafted polypropylene;

[0106] 24 parts of polyethylene;

[0107] Ethylene-methyl methacrylate copolymer 7 parts.

[0108] Other processes and materials used refer to Example 1.

[0109] Comparative Example 4

[0110] Different from Example 1, a novel release film includes a substrate, a release layer is provided on the substrate, and the release layer includes the following raw material components by weight:

[0111] Mixed resin 116 parts;

[0112] 13 parts of hexagonal boron nitride;

[0113] 0.6 part of polyquaternium salt;

[0114] Wherein, the mixed resin comprises the following raw materials in parts by weight:

[0115] Polypropylene 70 parts;

[0116] 15 parts of glycidyl methacrylate grafted polypropylene;

[0117] 24 parts of polyethylene;

[0118] Ethylene-methyl methacrylate copolymer 7 parts.

[0119] Other processes and materials used refer to Example 1.

[0120] Comparative Example 5

[0121] Different from Example 1, a novel release film includes a substrate, a release layer is provided on the substrate, and the release layer includes the following raw material components by weight:

[0122] Mixed resin 116 parts;

[0123] 13 parts of hexagonal boron nitride;

[0124] 7 parts of fluorine-containing functional polymer release agent;

[0125] 0.6 part of polyquaternium salt;

[0126] Wherein, the mixed resin comprises the following raw materials in parts by weight:

[0127] Polypropylene 70 parts;

[0128] 24 parts of polyethylene.

[0129] The following is a performance test of Examples 1 to 4 of the present invention, Comparative Examples 1 to 5, and a common release film. The comparison of relevant test results is shown in Table 2.

[0130] Table 2 Test comparison analysis table

[0131]

[0132] The samples to be tested were prepared according to the test standard, and then randomly sampled. The apparent performance of Examples 1 to 3 was first evaluated. The release films of Examples 1 to 3 were smooth and flat, without obvious scratches, bubbles, impurities and other defects. The release films of Comparative Examples 1, 4 and 5 were pressed, and had a granular and rough feeling.

[0133] From the comparative results in Table 2 above, it can be seen that the comprehensive properties of the new release film of the present invention, such as peel strength, high temperature resistance, heat shrinkage performance and mechanical properties, are better, and the bonding strength between the release layer and the substrate film base is high, which is due to the improvements in both the substrate and the release layer:

[0134] From Comparative Example 1 to Comparative Example 2, the use of a mixture such as a phosphate coupling agent not only solves the problem of dispersion and high temperature insulation, but also utilizes the most basic function of the coupling agent to firmly bond the substrate to each additive, and also makes it easier for the surface to form a stable hydrogen bond with the release coating layer, thereby strengthening the bonding strength of the composite membrane substrate. In terms of mechanical properties, the silica aerogel in the substrate is an additive with a porous, disordered, nanoscale continuous network structure. Compared with ordinary silica, it has a large specific surface area and good dispersibility; and the silica aerogel can solve the problem of low density, easy floating, and inability to disperse into the polyester of the phosphate coupling agent. The combined use of silica aerogel and phosphate coupling agent avoids agglomeration.

[0135] From Comparative Example 3 to Comparative Example 5, the use of mixed resin with glycidyl methacrylate grafted polypropylene and ethylene-methyl methacrylate copolymer in the release layer is to strengthen the melt blending between polypropylene and polyethylene and strengthen the interface strength between the two in terms of mechanical properties. Similarly, the fluorine-containing functional polymer release agent also has an auxiliary effect on the stability of the interface. Siloxane coupling agent is also used in hexagonal boron nitride to enhance the interface bonding ability. Figure 1 According to the structural formula of the fluorine-containing functional polymer release agent, it not only has an effect on the interface bonding of the release layer itself, but also, during the lamination and composite process, its own active functional groups such as hydroxyl and amino groups can form hydrogen bonds with the active agent functional groups on the surface of the substrate. Hydrogen bonds can form a strong attraction between molecules, promoting adhesion between hydroxyl and amino groups.

[0136] In terms of high temperature resistance, the phosphate coupling agent in the substrate uses the flame retardant and heat insulation properties of the material itself to help with high temperature resistance and heat insulation effects, but it is not as strong as hexagonal boron nitride in high temperature resistance and heat insulation. Figure 1 In the release layer, the fluorine-containing functional polymer release agent takes advantage of its large steric hindrance and many flame retardant and heat-insulating elements, and also has a good high-temperature resistant and heat-insulating effect.

[0137] In terms of light transmittance, due to the difference in the interface bonding performance between the material itself or the substrate and the release layer, the uneven dispersion of the filler will lead to lumps or agglomeration, which in turn leads to poor light transmittance. In addition, according to tests, the release film of the present invention also has good solvent resistance and can be reused 65-70 times.

[0138] In summary, the release film of the present invention has excellent comprehensive properties such as film-base bonding strength, peel strength, high temperature resistance, heat shrinkage performance and mechanical properties, so that the release paper of the present invention has the characteristics of long service life and can be further promoted for use.

[0139] Although the present invention has been disclosed as above with preferred embodiments, it is not intended to limit the present invention. A person with ordinary knowledge in the technical field to which the present invention belongs may make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be determined by the definition of the claims.

Claims

1. A novel release film, comprising a substrate, characterized in that: A release layer is provided on the substrate, and the release layer comprises the following raw material components by weight: 100-130 parts of mixed resin; 10-15 parts of hexagonal boron nitride; 5.5-10 parts of fluorine-containing functional polymer release agent; 0.5-0.8 parts of polyquaternium salt; The substrate comprises the following raw materials in parts by weight: 85-95 parts of PET polyester particles; 10-15 parts of polypropylene grafted maleic anhydride, and 5-10 parts of a mixture of a phosphate coupling agent, a silica aerogel and (2,4-difluorophenyl)trimethylsilane; The preparation of the fluorine-containing functional polymer release agent comprises the following steps: Phase I: Intermediate Synthesis Put epifluoropropane in a dropping funnel, and place ethylenediamine and anhydrous ethanol in a mass ratio of 2:5 in a three-necked flask, and then drop epifluoropropane into the three-necked flask; gradually increase the temperature to a reaction temperature of 80°C at a heating rate of 5°C / min, start timing and maintain the reaction temperature, and react for at least 6 hours; after the reaction is completed, remove excess raw materials and solvents with a rotary evaporator to obtain an intermediate; Phase II: Synthesis of fluorinated functional polymer release agent The intermediate is placed in a three-necked flask, and anhydrous ethanol is added to the three-necked flask in a mass ratio of 1:2 between the intermediate and anhydrous ethanol. After stirring, cycloheptyl tertiary amine is placed in a dropping funnel and added dropwise to the three-necked flask. The temperature is gradually increased to 80°C at a heating rate of 10°C / min by a staged heating method. After keeping the temperature for 10 minutes, the temperature is gradually increased to 120°C at a heating rate of 5°C / min. After 20 minutes, the reaction is completed, and the excess raw materials and solvent are removed by a rotary evaporator. The fluorine-containing functional polymer release agent is obtained by vacuum drying. The mixed resin comprises the following raw materials in parts by weight: Polypropylene 56-70 parts; 13-15 parts of glycidyl methacrylate grafted polypropylene; Polyethylene 24-30 parts; 7-15 parts of ethylene-methyl methacrylate copolymer; The hexagonal boron nitride is prepared by impregnation with 0.5wt%-2.5wt% of a siloxane coupling agent alcohol solution and then drying.

2. A novel release film according to claim 1, characterized in that: The thickness of the release layer is 0.1-1 mm.

3. A novel release film according to claim 1, characterized in that: The mass ratio of the phosphate coupling agent, the silica aerogel and (2,4-difluorophenyl)trimethylsilane in the mixture of the phosphate coupling agent, the silica aerogel and (2,4-difluorophenyl)trimethylsilane is (0.7-0.9): (0.5-0.8):

1.

4. A novel release film according to claim 1, wherein the hexagonal boron nitride is treated with a 0.75wt% 3-aminopropyltriethoxysilane coupling agent alcohol solution, and the dried hexagonal boron nitride is ground into 1000 mesh particles in a quartz mortar.

5. A method for preparing the novel release film according to any one of claims 1 to 4, characterized in that: The following steps are involved: A. Preparation of substrate: a mixture of phosphate coupling agent and (2,4-difluorophenyl)trimethylsilane is prepared into a 0.5wt% coupling agent aqueous solution, and then the PET polyester particles in the substrate are immersed in the coupling agent aqueous solution, continuously stirred for 1-4 hours, and vacuum dried; then the dried PET polyester particles and polypropylene grafted maleic anhydride are mixed and stirred, and then conveyed to a screw extruder, and clamped by a cooling roller and a pressure roller to obtain a dry substrate; B. Substrate surface treatment: clean the impurities on the substrate surface, and perform anti-static treatment on the substrate, then evenly spray the coupling agent aqueous solution on the dry substrate surface, and obtain the pre-treated base paper after natural drying; C. Prepare a mixed masterbatch of the release layer, mix the mixed resin, hexagonal boron nitride, fluorine-containing functional polymer release agent, and polyquaternary ammonium salt in proportion using a blender, and send them into a twin-screw extruder for extrusion granulation, cooling, and drying to obtain a mixed masterbatch; D. Put the mixed masterbatch into the screw again. The molten material from the extrusion section of the screw passes through the filter plate of the die head to turn the original vortex-shaped material into a flat flow, and then enters the laminating machine mold to be split to both ends and become flakes. After the uniform flakes flow out, they enter the process of compounding with the substrate. E. The high-temperature molten film of the sheet passes through the clamping of the cooling roller and the pressure roller, so that it adheres to the substrate and cools rapidly to obtain the initial product of the release film; F. The initial release film product is subjected to corona pretreatment, super calendering and drying treatment in sequence, and then pulled into the finished product winding to obtain the release film.