A hydrogen storage material for a two-stage metal hydride hydrogen compressor and a preparation method thereof

CN118581353BActive Publication Date: 2024-11-15JIANGSU FEIYUE PUMP GRP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411075509.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-15
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

但是,目前市面上,专门针对氢压缩机用二级储氢合金的较少,现有储氢合金对于二级储氢合金适配性较低,仍需进一步提高吸、放氢性能和使用寿命,从而提高实际应用性

Benefits of technology

[0023] 1. In the scheme, a single CaCu is obtained through optimized preparation 5 Rare earth hydrogen storage alloy with type hexagonal crystal, suitable for hydrogen storage alloy in the second stage of dual-stage metal hydride hydrogen compressor, which is La 1-a-b Y a Ce b Ni c M d . By defining and optimizing the chemical composition structure and stoichiometric ratio of the hydrogen storage alloy, the hydrogen storage alloy has the advantages of easy activation, good kinetic properties, and long cycle life. The hydrogen absorption equilibrium pressure of the hydrogen storage alloy at 25°C is up to about 3MPa, and it can easily accept the hydrogen supply from the first-stage compression working medium; and it only needs to be heated to about 190°C to output a hydrogen pressure of 45MPa, which is very suitable for hydrogenation. The reaction bed structure material has little impact on the mechanical properties, so it is very suitable for the second-stage hydrogen storage alloy of the two-stage metal hydride hydrogen compressor.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118581353B_ABST
    Figure CN118581353B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of hydrogen storage materials, and in particular to a hydrogen storage alloy for a two-stage metal hydride hydrogen compressor and a preparation method thereof. The hydrogen storage alloy is a single CaCu5-type hexagonal crystal structure. The hydrogen storage alloy is La 1‑a‑b Y a Ce b Ni c M d , wherein 0.1≤a≤0.7, 0≤b≤0.7, 4.6≤c≤4.9, 0.1≤d≤0.4, 0.6≤a+b≤0.8, c+d=5; M includes at least one of Mn and Al. In this scheme, the alloy has the advantages of easy activation, good kinetic properties and long cycle life, and is very suitable for the second stage hydrogen storage alloy of a two-stage metal hydride hydrogen compressor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of hydrogen storage materials, and in particular to a hydrogen storage material for a two-stage metal hydride hydrogen compressor and a preparation method thereof. Background Art

[0002] Hydrogen energy is a high-quality secondary energy with the greatest potential for sustainable development. It has the advantages of abundant reserves, wide sources, clean and efficient, and has great development potential. In the wide application field of hydrogen energy, the development of hydrogen-oxygen fuel cell vehicles is one of the solutions to the carbon emission problem in the transportation industry, and the construction of hydrogen refueling stations is the basic guarantee for the application of hydrogen fuel cell vehicles. Among them, the core component of the hydrogen refueling station is the hydrogen compressor. The moving parts of the traditional mechanical hydrogen compressor will wear out after long-term operation, thereby destroying the seal and reducing the compressor displacement and efficiency. In contrast, the hydrogen compressor with reversible metal hydride as the working medium has the advantages of no moving parts, no wear, a large boost range, and no pollution to the environment. At the same time, it can also work with low-grade heat sources to further save energy.

[0003] Metal hydride hydrogen compressors work by utilizing the property that the equilibrium hydrogen pressure of metal hydrides changes exponentially with temperature, that is, they absorb hydrogen at a relatively low temperature and release high-pressure hydrogen when heated. Generally, metal hydrides have a high thermal effect of absorbing and releasing hydrogen. Therefore, in order to ensure that the compression system absorbs and releases hydrogen quickly, in addition to strengthening the heat transfer performance of the reaction bed, the alloy composition design can be used to appropriately reduce the enthalpy change of hydrogen absorption and desorption of each stage of compression working medium. The strategy that matches this is multi-stage compression, that is, using low-pressure alloys to generate a higher transition hydrogen pressure, introducing high-pressure alloys to absorb hydrogen, and then heating them to produce ultra-high-pressure hydrogen.

[0004] In the prior art, selecting suitable hydride materials is one of the keys to achieving high-efficiency operation of metal hydride compressors. At present, hydrogen storage materials for hydrogen compressors generally include AB5 series, AB2 series and AB series. Among them, AB5 series alloys have excellent comprehensive properties and strong anti-poisoning ability, and can be used as purification and compression materials. The prototype LaNi5 alloy of the AB5 series hydrogen storage alloy has the characteristics of easy activation, moderate and flat equilibrium pressure, small equilibrium pressure difference between hydrogen absorption and desorption, and good kinetics and resistance to impurity gas poisoning. However, there are currently few secondary hydrogen storage alloys specifically for hydrogen compressors on the market, and the existing hydrogen storage alloys have low adaptability to secondary hydrogen storage alloys, and there is still a need to further improve the hydrogen absorption and desorption performance and service life, so as to improve practical applicability.

[0005] Therefore, it is of great significance to further optimize the hydrogen storage alloy material and prepare a hydrogen storage material for a two-stage metal hydride hydrogen compressor. Summary of the invention

[0006] The object of the present invention is to provide a hydrogen storage alloy for a two-stage metal hydride hydrogen compressor and a preparation method thereof, so as to solve the problems raised in the above-mentioned background technology.

[0007] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0008] A hydrogen storage alloy for a two-stage metal hydride hydrogen compressor, the hydrogen storage alloy is La 1-a-b Y a Ce b Ni c M d , among which, 0.1≤a≤0.7, 0≤b≤0.7, 4.6≤c≤4.9, 0.1≤d≤0.4, 0.6≤a+b≤0.8, c+d=5.

[0009] In a further proposal, La 1-a-b Y a Ce b Ni c M d Here, M includes at least one of Mn and Al.

[0010] In a further embodiment, the hydrogen storage alloy has a single CaCu5-type hexagonal crystal structure.

[0011] In a further proposal, La 1-a-b Y a Ce b Ni c M d , 0.5≤a≤0.55.

[0012] In a further embodiment, the purity of La is 99%, the purity of Y is 99%, the purity of Ce is 99%, the purity of Ni is 99.5%, the purity of Mn is 99.7%, and the purity of Al is 99.5%.

[0013] In a further embodiment, a method for preparing a hydrogen storage alloy for a two-stage metal hydride hydrogen compressor comprises the following steps:

[0014] Step 1: The metal is mixed according to the stoichiometric ratio, melted in an induction furnace under an argon atmosphere, refined at 1573-1623K for 10-15 minutes, and the melt is cast into a metal ingot mold to obtain an alloy ingot;

[0015] Step 2: Place the alloy ingot in an argon-filled tubular furnace tube, anneal at 1300-1350K for 6-9 hours, remove the furnace tube and air-cool to obtain a hydrogen storage alloy.

[0016] In a further embodiment, the alloy ingot is subjected to secondary smelting to prepare the hydrogen storage alloy; the steps include:

[0017] (1) placing the alloy ingot obtained by induction melting in step 1 in an argon atmosphere in a high-frequency induction melting furnace for secondary remelting, and then spraying it onto a rotating copper roller with a linear velocity of 30-35 m / s to obtain an alloy sheet; (2) placing the alloy sheet in an argon-filled tubular furnace, annealing at 1223-1273 K for 6-9 hours, and removing the furnace tube for air cooling to obtain a hydrogen storage alloy.

[0018] In a further embodiment, the hydrogen storage alloy is ground with metal-based graphene to obtain a hydrogen storage material; the metal-based graphene accounts for 1-3wt% of the hydrogen storage alloy, and specifically comprises the following steps:

[0019] Under an argon atmosphere, the hydrogen storage alloy and the metal-based graphene are evenly mixed, and grinding balls are added. Intermittent ball milling is carried out in a planetary ball mill with a ball-to-material ratio of (40-50):1. The speed of the ball mill is 400-500 r / min. During the process, the grinding is performed for 10-15 minutes each, with an interval of 10-15 minutes, and the total grinding time is 2-3 hours; thus, a hydrogen storage material is obtained.

[0020] In a further embodiment, the preparation method of the metal-based graphene is as follows: (1) placing graphene in a mixture of sulfuric acid and nitric acid, adding potassium permanganate in an ice bath, stirring at room temperature for 24 hours, adding deionized water to dilute, stirring at 70-80°C for 15-20 minutes, washing and drying; placing it in a 20wt% nitric acid solution, stirring at 70-80°C for 20-30 minutes, washing and drying to obtain graphene oxide; (2) dissolving copper nitrate and calcium nitrate in deionized water in sequence to obtain a solution; adding graphene oxide and ultrasonically dispersing it uniformly, stirring at room temperature for 3-6 hours, filtering and drying; placing it in a nitrogen atmosphere and heating it to 200-400°C, heat treating it for 60-70 minutes, replacing hydrogen and nitrogen mixed gas, heat treating it for 60-70 minutes, replacing nitrogen atmosphere and cooling to obtain modified graphene; (3) treating the modified graphene with a pulse microwave at 1000W for 1-2 seconds to obtain metal-based graphene.

[0021] In a further embodiment, the mass ratio of graphene oxide, copper nitrate and calcium nitrate is 9:2:1.

[0022] Compared with the prior art, the beneficial effects achieved by the present invention are as follows:

[0023] 1. In the scheme, a single CaCu5-type hexagonal crystal rare earth hydrogen storage alloy is prepared by optimization, which is suitable for the second stage of a two-stage metal hydride hydrogen compressor. 1-a-b Y a Ce b Ni c M d. By limiting and optimizing the chemical composition structure and stoichiometric ratio of hydrogen storage alloys, hydrogen storage alloys have the advantages of easy activation, good kinetic performance, and long cycle life. The maximum hydrogen absorption equilibrium pressure of the hydrogen storage alloy at 25°C is about 3MPa, and it is easy to accept the hydrogen supply of the first-stage compression working medium; and it only needs to be heated to about 190°C to output a hydrogen pressure of 45MPa, which has little effect on the mechanical properties of the structural materials of the hydrogenation reaction bed, so it is very suitable for the second-stage hydrogen storage alloy of the two-stage metal hydride hydrogen compressor.

[0024] 2. In the scheme, in order to further improve the uniformity of the hydrogen storage alloy structure, enhance its cycle life, and improve its applicability in hydrogen compressors, the hydrogen storage alloy is further subjected to secondary melting and rapid solidification in this application, and is ground and modified using metal-based graphene to obtain a further optimized hydrogen storage material.

[0025] Among them, the purpose of secondary smelting is to use rapid solidification technology to refine its grains and increase the rapid "diffusion channel" of hydrogen, so as to improve its hydrogen absorption and desorption kinetics and improve the operating efficiency of the hydrogen compressor; at the same time, make the element distribution more uniform, reduce the slope of the hydrogen absorption and desorption platform, and improve the cycle life of hydrogen absorption and desorption.

[0026] Among them, the introduction of metal-based graphene grinding modification can improve its dynamic performance and heat transfer performance, and increase the cycle life of the hydrogenation reactor bed. During the grinding modification process, first, ball milling produces nanocrystalline or amorphous structures on the surface of the hydrogen storage alloy, which increases the diffusion channel of hydrogen atoms and shortens the diffusion distance of hydrogen atoms to the inside, thereby increasing the adsorption and desorption rates. Second, the use of metal-based graphene for co-grinding can not only play a grinding aid, but also minimize agglomeration on the basis of promoting the refinement of hydrogen storage alloys. Moreover, it further adheres to the surface of the hydrogen storage alloy, which can improve the thermal conductivity, facilitate the rapid export / import of the thermal effect generated by the absorption and desorption of hydrogen by the alloy, thereby increasing the absorption and desorption rate of the reactor bed; at the same time, the graphene on the surface of the alloy powder can effectively inhibit the compaction and compaction of the metal powder and increase the service life of the reactor bed; in addition, the metal-based graphene and the hydrogen storage alloy contact to produce a phase interface, forming a special microstructure, which can promote the adsorption and diffusion of hydrogen, thereby optimizing the hydrogen storage performance.

[0027] In addition, compared with ordinary graphene, the copper- and calcium-doped metal-based graphene used in the scheme increases active sites, which can catalytically promote hydrogen adsorption, thereby improving kinetic performance and improving the rate and temperature of hydrogen absorption and desorption; in addition, compared with single copper doping, the introduction of calcium not only optimizes hydrogen storage performance, but also improves heat transfer performance, improves thermal diffusion efficiency, and reduces temperature-induced lattice strain during the cycle, thereby improving cyclic performance and increasing its application potential in hydrogen compressors. The final pulse process can further reduce graphene oxide, increase thermal conductivity, and thus improve heat transfer efficiency.

[0028] In addition, it should be noted that the amount of metal-based graphene introduced needs to be limited. Too much will hinder the diffusion of hydrogen atoms, resulting in a decrease in the performance of hydrogen storage materials. In addition, intermittent ball milling during the grinding process can avoid local temperature increases and inhibit the generation of defects. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:

[0030] Figure 1 For the present invention La 1-a-b Y a Ce b Ni c M d XRD diffraction pattern of the alloy;

[0031] Figure 2 For the present invention La 0.4 Y 0.55 Ce 0.05 Ni 4.8 Mn 0.1 Al 0.1 PCT curve of alloy;

[0032] Figure 3 For the present invention La 0.4 Y 0.55 Ce 0.05 Ni 4.8 Mn 0.1 Al 0.1 Hydrogen absorption kinetics curve of alloy;

[0033] Figure 4 For the present invention La 0.4 Y 0.55 Ce 0.05 Ni 4.8 Mn 0.1 Al 0.1 Hydrogen desorption kinetics curve of the alloy;

[0034] Figure 5 For the present invention La 0.3 Y 0.6 Ce 0.1 Ni 4.8 Al 0.2 PCT curve of alloy;

[0035] Figure 6 For the present invention La 0.3 Y 0.6 Ce 0.1 Ni 4.8 Al0.2 Hydrogen absorption kinetics curve of alloy;

[0036] Figure 7 For the present invention La 0.3 Y 0.6 Ce 0.1 Ni 4.8 Al 0.2 Hydrogen desorption kinetics curve of the alloy;

[0037] Figure 8 For the present invention La 0.3 Y 0.6 Ce 0.1 Ni 4.8 Mn 0.2 PCT curve of alloy;

[0038] Fig. 9 For the present invention La 0.3 Y 0.6 Ce 0.1 Ni 4.8 Mn 0.2 Hydrogen absorption kinetics curve of alloy;

[0039] Fig.10 For the present invention La 0.3 Y 0.6 Ce 0.1 Ni 4.8 Mn 0.2 Hydrogen desorption kinetics curve of the alloy;

[0040] Fig.11 For the present invention La 0.4 Y 0.5 Ce 0.1 Ni 4.8 Al 0.2 PCT curve of alloy;

[0041] Fig.12 For the present invention La 0.4 Y 0.5 Ce 0.1 Ni 4.8 Al 0.2 Hydrogen absorption kinetics curve of alloy;

[0042] Fig.13 For the present invention La 0.4 Y 0.5 Ce 0.1 Ni 4.8 Al 0.2 Hydrogen desorption kinetics curve of the alloy;

[0043] Fig.14 For the present invention La 0.4 Y 0.5 Ce 0.1Ni 4.8 Al 0.2 PCT curves of the alloy before and after hydrogen absorption and desorption cycles;

[0044] Fig.15 For the present invention La 0.4 Y 0.5 Ce 0.1 Ni 4.8 Mn 0.2 PCT curve of alloy;

[0045] Fig.16 For the present invention La 0.4 Y 0.5 Ce 0.1 Ni 4.8 Mn 0.2 Hydrogen absorption kinetics curve of alloy;

[0046] Fig.17 For the present invention La 0.4 Y 0.5 Ce 0.1 Ni 4.8 Mn 0.2 Hydrogen desorption kinetics curve of the alloy. DETAILED DESCRIPTION

[0047] The preferred embodiments of the present invention are described below in conjunction with the accompanying drawings. It should be understood that the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0048] It should be noted that the parameters of all raw materials involved in the present invention are exemplarily included without any special restrictions: in the following embodiments, the purity of La is 99%, the purity of Y is 99%, the purity of Ce is 99%, the purity of Ni is 99.5%, the purity of Mn is 99.7%, and the purity of Al is 99.5%; the thickness of graphene is less than 1.7 nm, and the purity is 99%; all are commercially available.

[0049] The preparation method of graphene oxide is as follows: by weight, 10 parts of graphene are placed in a mixed solution of 136 parts of sulfuric acid and nitric acid (mass ratio is 130:6), 20 parts of potassium permanganate are added under an ice bath, stirred at room temperature for 24 hours, 160 parts of deionized water are added to dilute, stirred at 80°C for 15 minutes, washed and dried; placed in 200 parts of 20wt% nitric acid solution, stirred at 80°C for 30 minutes, washed and dried to obtain graphene oxide.

[0050] Performance test 1: The hydrogen storage alloy samples were activated and the hydrogen storage performance was tested on the PCT-2SDWIN dual-channel fully automatic gas adsorption / desorption tester of Suzuki, Japan. The PCT curve test of hydrogen absorption and desorption adopts the volumetric method. The purity of hydrogen is 99.999%. Process: Weigh about 1g of sample and put it into the sample chamber, heat it to 353K, evacuate it for 30 minutes to remove impurities, then cool it to room temperature, and pass 6MPa of hydrogen to react with the sample. Repeat the absorption and desorption of hydrogen 10 times to ensure that the sample is fully activated, and then set different temperatures for hydrogen storage performance test. During the hydrogen absorption kinetics test, the initial inlet pressure of the sample chamber is 1MPa higher than the hydrogen absorption equilibrium pressure of the tested alloy. Record the change of pressure over time during the entire experiment, convert it into the change of hydrogen absorption amount over time, and you can get the hydrogen absorption kinetics curve of the alloy at this temperature. During the hydrogen desorption kinetics test, the alloy that has been saturated with hydrogen is allowed to directly desorb hydrogen into a gas storage chamber that is initially in a vacuum state. The change in pressure over time is recorded and converted into the change in the amount of hydrogen desorption over time, so that the hydrogen desorption kinetics curve of the alloy at that temperature can be obtained.

[0051] At the same time, the Van't Hoff formula is used to calculate the enthalpy change and reaction entropy change of the hydrogen absorption and desorption reaction of the hydrogen storage alloy: ,(in, To balance the pressure of hydrogen absorption or desorption, is standard atmospheric pressure, and are the standard enthalpy variable and standard entropy variable, respectively).

[0052] Embodiment 1: A method for preparing a hydrogen storage alloy for a two-stage metal hydride hydrogen compressor, comprising the following steps:

[0053] Step 1: The metal is mixed according to the stoichiometric ratio, melted in an induction furnace under an argon atmosphere, refined at 1593K for 10 minutes, and the melt is cast into a metal ingot mold to obtain an alloy ingot;

[0054] Step 2: Place the alloy ingot in an argon-filled tubular furnace, set the temperature to 1323K, anneal for 8 hours, remove the furnace tube and air-cool to obtain a hydrogen storage alloy. 0.4 Y 0.55 Ce 0.05 Ni 4.8 Mn 0.1 Al 0.1 .

[0055] Test results: The hydrogen storage capacity H / M of the hydride formed at 298K is 5.86, and the hydrogen absorption equilibrium pressure is 1.59MPa, which is easy to accept the hydrogen supply of the first-stage compressed working medium. Under the conditions of a temperature of 25°C and an initial hydrogen pressure of 2.59MPa, it only takes 116 seconds to reach 90% of the maximum hydrogen absorption capacity. It only takes 112 seconds to release hydrogen into a vacuum at 45°C to reach 90% of the maximum hydrogen release capacity. The kinetics of hydrogen absorption and desorption are fast and easy to activate. The enthalpy changes of hydrogen absorption and desorption are -24.10KJ / Mol and 25.62KJ / Mol, respectively, and the entropy changes of hydrogen absorption and desorption are -103.85J / K•Mol and 106.65J / K•Mol, respectively. The heating temperature when the output hydrogen pressure reaches 45MPa is 186°C.

[0056] Comparative Example 1: The preparation method is the same as that of Example 1, except that the hydrogen storage alloy is La 0.3 Y 0.6 Ce 0.1 Ni 4.8 Al 0.2 .

[0057] Test results: The hydrogen storage capacity H / M of the hydride formed at 298K is 5.15, and the hydrogen absorption equilibrium pressure is 3.07MPa, which is easy to accept the hydrogen supply of the first-stage compressed working medium. Under the conditions of temperature of 25℃ and initial hydrogen pressure of 4.07MPa, it only takes 186 seconds to reach 90% of the maximum hydrogen absorption capacity, and it only takes 146 seconds to release hydrogen into vacuum at 45℃ to reach 90% of the maximum hydrogen release capacity. The kinetics of hydrogen absorption and desorption are fast and easy to activate. The enthalpy changes of hydrogen absorption and desorption are -20.67KJ / Mol and 24.71KJ / Mol, respectively, and the entropy changes of hydrogen absorption and desorption are -97.84J / K•Mol and 106.02J / K•Mol, respectively. The heating temperature when the output hydrogen pressure reaches 45MPa is 174℃.

[0058] Comparative Example 2: The preparation method is the same as that of Example 1, except that the hydrogen storage alloy is La 0.3 Y 0.6 Ce 0.1 Ni 4.8 Mn 0.2 .

[0059] Test results: The hydrogen storage capacity H / M of the hydride formed at 298K is 5.13, and the hydrogen absorption equilibrium pressure is 2.75MPa, which is easy to accept the hydrogen supply of the first-stage compressed working medium. Under the conditions of temperature of 25℃ and initial hydrogen pressure of 3.75MPa, it only takes 236 seconds to reach 90% of the maximum hydrogen absorption capacity. It only takes 126 seconds to release hydrogen into vacuum at 45℃ to reach 90% of the maximum hydrogen release capacity. The kinetics of hydrogen absorption and desorption are fast and easy to activate. The enthalpy changes of hydrogen absorption and desorption are -21.25KJ / Mol and 24.79KJ / Mol, respectively, and the entropy changes of hydrogen absorption and desorption are -98.85J / K•Mol and 105.98J / K•Mol, respectively. The heating temperature when the output hydrogen pressure reaches 45MPa is 176℃.

[0060] Example 2: The preparation method is the same as that of Example 1, except that the hydrogen storage alloy is La 0.4 Y 0.5 Ce 0.1 Ni 4.8 Al 0.2 .

[0061] Test results: The hydrogen storage capacity H / M of the hydride formed at 298K is 5.10, and the hydrogen absorption equilibrium pressure is 1.28MPa, which is easy to accept the hydrogen supply of the first-stage compressed working medium. Under the conditions of temperature of 25℃ and initial hydrogen pressure of 2.28MPa, it only takes 202 seconds to reach 90% of the maximum hydrogen absorption capacity. It only takes 252 seconds to release hydrogen into vacuum at 45℃ to reach 90% of the maximum hydrogen release capacity. The kinetics of hydrogen absorption and desorption are fast and easy to activate. The enthalpy changes of hydrogen absorption and desorption are -24.72KJ / Mol and 26.65KJ / Mol, respectively, and the entropy changes of hydrogen absorption and desorption are -104.12J / K•Mol and 107.84J / K•Mol, respectively. The heating temperature when the output hydrogen pressure reaches 45MPa is 194℃. After 500 cycles of hydrogen absorption and desorption, the capacity and platform pressure of the PCT curve have no obvious changes, indicating that the alloy has a good cycle life.

[0062] Example 3: The preparation method is the same as that of Example 1, except that the hydrogen storage alloy is La 0.4 Y 0.5 Ce 0.1 Ni 4.8 Mn 0.2 .

[0063] Test results: The hydrogen storage capacity H / M of the hydride formed at 298K is 5.22, and the hydrogen absorption equilibrium pressure is 1.62MPa, which is easy to accept the hydrogen supply of the first-stage compressed working medium. Under the conditions of a temperature of 25°C and an initial hydrogen pressure of 2.62MPa, it only takes 218 seconds to reach 90% of the maximum hydrogen absorption capacity. At 45°C, it only takes 166 seconds to release hydrogen into a vacuum to reach 90% of the maximum hydrogen release capacity. The kinetics of hydrogen absorption and desorption are fast and easy to activate. The enthalpy changes of hydrogen absorption and desorption are -23.86KJ / Mol and 27.36KJ / Mol, respectively, and the entropy changes of hydrogen absorption and desorption are -103.22J / K•Mol and 110.26J / K•Mol, respectively. The heating temperature when the output hydrogen pressure reaches 45MPa is 187°C.

[0064] Conclusion: From the data of Examples 1-3 and Comparative Examples 1-2, it can be seen that compared with Y=0.6, when the stoichiometric value of Y is within 0.5-0.55, the hydrogen storage alloy has a lower hydrogen absorption equilibrium pressure (<2MPa), and when the hydrogen storage alloy contains both manganese and aluminum, the hydrogen absorption amount is the highest.

[0065] Example 4: Based on Example 2, the process scheme is further optimized to obtain a hydrogen storage material; the details are as follows:

[0066] Step 1: The metal is mixed according to the stoichiometric ratio, melted in an induction furnace under an argon atmosphere, refined at 1593K for 10 minutes, and the melt is cast into a metal ingot mold to obtain an alloy ingot;

[0067] Step 2: (1) The alloy ingot obtained in step 1 is placed in a high-frequency induction melting furnace under an argon atmosphere for secondary remelting, and then sprayed onto a rotating copper roller at a linear speed of 30 m / s to obtain an alloy sheet; (2) The alloy sheet is placed in an argon-filled tubular furnace tube, annealed at 1253 K for 8 hours, and the furnace tube is removed for air cooling to obtain a hydrogen storage alloy; in the scheme, the hydrogen storage alloy is La 0.4 Y 0.5 Ce 0.1 Ni 4.8 Al 0.2 ;

[0068] Step 3: (1) dissolving 2 parts of copper nitrate and 1 part of calcium nitrate in 100 parts of deionized water in turn to obtain a solution; adding 9 parts of graphene oxide and uniformly dispersing by ultrasonication, stirring at room temperature for 5 hours, filtering and drying; heating the solution to 400°C in a nitrogen atmosphere, heat treating for 60 minutes, replacing the hydrogen-nitrogen mixed gas, heat treating for 60 minutes, replacing the nitrogen atmosphere and cooling to obtain modified graphene; treating the modified graphene with a pulse microwave at 1000 W for 1 second to obtain metal-based graphene;

[0069] (2) Under an argon atmosphere, the hydrogen storage alloy and the metal-based graphene are uniformly mixed, with the metal-based graphene accounting for 2.5wt% of the hydrogen storage alloy. Grinding balls are added and intermittent ball milling is carried out in a planetary ball mill with a ball-to-material ratio of 50:1. The ball mill speed is 400r / min. During the process, the grinding is performed for 10 minutes each and the interval is 15 minutes. The total grinding time is 2 hours; thus, the hydrogen storage material is obtained.

[0070] Test results: The hydrogen absorption amount and hydrogen absorption and desorption platform pressure of the alloy have no significant changes compared with Example 2, but the kinetic performance is significantly improved: at a temperature of 25°C and an initial hydrogen pressure of 2.28MPa, it only takes 78 seconds to reach 90% of the maximum hydrogen absorption amount, and at 45°C, it only takes 126 seconds to release hydrogen into vacuum to reach 90% of the maximum hydrogen desorption amount. The kinetic speed of hydrogen absorption and desorption is fast and easy to activate. After 500 cycles of hydrogen absorption and desorption, the PCT curve capacity and platform pressure have no significant changes, indicating that the alloy has a good cycle life.

[0071] Comparative Example 1: The basic method is the same as that of Example 4, except that graphene is ground to obtain a hydrogen storage material; the specific changes are as follows:

[0072] Step 3: Under an argon atmosphere, the hydrogen storage alloy and graphene are evenly mixed, with the metal-based graphene accounting for 2.5wt% of the hydrogen storage alloy. Grinding balls are added and intermittent ball milling is carried out in a planetary ball mill with a ball-to-material ratio of 50:1. The ball mill speed is 400r / min. During the process, the grinding is performed for 10 minutes each, with an interval of 15 minutes, and the total grinding time is 2 hours; the hydrogen storage material is obtained.

[0073] Comparative Example 2: The basic method is the same as that of Example 4, except that copper-based graphene is ground to obtain a hydrogen storage material; the specific changes are as follows:

[0074] Step 3: (1) dissolving 3 parts of copper nitrate in 100 parts of deionized water to obtain a solution; adding 9 parts of graphene oxide and uniformly dispersing by ultrasonication, stirring at room temperature for 5 hours, filtering and drying; heating the solution to 400°C in a nitrogen atmosphere, heat treating the solution for 60 minutes, replacing the hydrogen-nitrogen mixed gas, heat treating the solution for 60 minutes, replacing the nitrogen atmosphere and cooling the solution to obtain modified graphene; subjecting the modified graphene to pulse microwave treatment at 1000 W for 1 second to obtain copper-based graphene;

[0075] (2) Under an argon atmosphere, the hydrogen storage alloy and copper-based graphene are evenly mixed, with the copper-based graphene accounting for 2.5wt% of the hydrogen storage alloy. Grinding balls are added and intermittent ball milling is carried out in a planetary ball mill with a ball-to-material ratio of 50:1. The ball mill speed is 400r / min. During the process, the grinding is performed for 10 minutes each and the interval is 15 minutes. The total grinding time is 2 hours; thus, the hydrogen storage material is obtained.

[0076] Performance Test 2: The hydrogen storage alloys or hydrogen storage materials in Example 2, Example 4, Comparative Example 1, and Comparative Example 2 were subjected to a hydrogen storage cycle performance test, with the number of cycles including 500 and 1000 times, and the hydrogen storage capacity attenuation rate was calculated.

[0077]

[0078] Conclusion: From the data in the above table, it can be seen that the further modification of the hydrogen storage alloy in the scheme further improves the hydrogen storage performance and cycle performance, indicating that secondary smelting and the introduction of metal-based graphene to grind and modify the hydrogen storage alloy can further improve the cycle life of the hydrogen storage alloy of this structure and improve its applicability in hydrogen compressors.

[0079] Finally, it should be noted that the above description is only a preferred example of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A hydrogen storage material for a two-stage metal hydride hydrogen compressor, characterized in that: The hydrogen storage material includes a hydrogen storage alloy and metal-based graphene; the metal-based graphene accounts for 1-3wt% of the hydrogen storage alloy; The hydrogen storage alloy is La 1-a-b Y a Ce b Ni c M d , 0.5≤a≤0.55, 0≤b≤0.7, 4.6≤c≤4.9, 0.1≤d≤0.4, 0.6≤a+b≤0.8, c+d=5; M includes at least one of Mn and Al; The preparation method of the metal-based graphene is as follows: (1) placing graphene in a mixture of sulfuric acid and nitric acid, adding potassium permanganate in an ice bath, stirring at room temperature for 24 hours, adding deionized water to dilute, stirring at 70-80° C. for 15-20 minutes, washing and drying; placing it in a 20wt% nitric acid solution, stirring at 70-80° C. for 20-30 minutes, washing and drying, and obtaining graphene oxide; (2) dissolving copper nitrate and calcium nitrate in deionized water in sequence to obtain a solution; Add graphene oxide and disperse it evenly by ultrasonication, stir at room temperature for 3-6 hours, filter and dry; place it in a nitrogen atmosphere and heat it to 200-400°C, heat treat it for 60-70 minutes, replace the hydrogen and nitrogen mixed gas, heat treat it for 60-70 minutes, replace the nitrogen atmosphere and cool it to obtain modified graphene; (3) treat the modified graphene with a pulse microwave at 1000 W for 1-2 seconds to obtain metal-based graphene; wherein the mass ratio of graphene oxide, copper nitrate and calcium nitrate is 9:2:

1.

2. The hydrogen storage material for a two-stage metal hydride hydrogen compressor according to claim 1, characterized in that: The hydrogen storage alloy has a single CaCu5 type hexagonal crystal structure.

3. The hydrogen storage material for a two-stage metal hydride hydrogen compressor according to claim 1, characterized in that: The purity of La is 99%, the purity of Y is 99%, the purity of Ce is 99%, the purity of Ni is 99.5%, the purity of Mn is 99.7%, and the purity of Al is 99.5%.

4. The method for preparing a hydrogen storage material for a two-stage metal hydride hydrogen compressor according to claim 1, characterized in that: The hydrogen storage alloy is melted in a vacuum induction furnace under an argon atmosphere to obtain an alloy ingot in advance; the process comprises the following steps: The metals are mixed according to a stoichiometric ratio, melted in an induction furnace under an argon atmosphere, refined at 1573-1623 K for 10-15 minutes, and the melt is cast into a metal ingot mold to obtain an alloy ingot.

5. The method for preparing a hydrogen storage material for a two-stage metal hydride hydrogen compressor according to claim 4, characterized in that: The alloy ingot is directly annealed to obtain a hydrogen storage alloy; the process comprises the following steps: The alloy ingot according to claim 4 is placed in an argon-filled tubular furnace tube, annealed at 1300-1350K for 6-9 hours, and the furnace tube is taken out for air cooling to obtain a hydrogen storage alloy.

6. The method for preparing a hydrogen storage material for a two-stage metal hydride hydrogen compressor according to claim 4, characterized in that: The alloy ingot is subjected to secondary smelting to prepare a hydrogen storage alloy; the process comprises the following steps: (1) placing the alloy ingot according to claim 4 in an argon atmosphere for secondary remelting in a high-frequency induction melting furnace, and then spraying it onto a rotating copper roller with a linear speed of 30-35 m / s to obtain an alloy sheet; (2) placing the alloy sheet in an argon-filled tubular furnace, annealing at 1223-1273 K for 6-9 hours, and then removing the furnace tube for air cooling to obtain a hydrogen storage alloy.

7. The method for preparing a hydrogen storage material for a two-stage metal hydride hydrogen compressor according to claim 6, characterized in that: The preparation of the hydrogen storage material comprises the following steps: Under an argon atmosphere, the hydrogen storage alloy and the metal-based graphene are evenly mixed, and grinding balls are added. Intermittent ball milling is carried out in a planetary ball mill with a ball-to-material ratio of (40-50):

1. The speed of the ball mill is 400-500 r / min. During the process, the grinding is performed for 10-15 minutes each, with an interval of 10-15 minutes, and the total grinding time is 2-3 hours; thus, a hydrogen storage material is obtained.