A sulfide ion oxidation electrode and its preparation method and application

The nickel-monopolytic oxide oxidation electrode coated with nickel-molybdenum oxide replaces the anode oxygen evolution reaction and combines the cathode reaction to solve the problems of high energy consumption and resource waste in alkaline electrolytic hydrogen production technology, achieving low energy consumption and low energy consumption Cost hydrogen production and avoid chlorine evolution reactions in electrolytic seawater, improving sulfur resource utilization.

CN118581514BActive Publication Date: 2024-11-05SONGSHAN LAKE MATERIALS LAB
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411074596.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-05
Estimated Expiration
2044-08-07

Smart Images

  • Figure CN118581514B_ABST
    Figure CN118581514B_ABST
Patent Text Reader

Abstract

The present invention provides a sulfur ion oxidation electrode and a preparation method and application thereof, and the present invention belongs to the technical field of new energy materials. The sulfur ion oxidation electrode comprises a substrate and nickel telluride coated with nickel molybdenum oxide supported on the substrate. The electrode of the present invention has excellent catalytic performance of sulfur ion oxidation reaction, replaces the oxygen evolution reaction of the electrolytic water anode, can break through the theoretical potential of traditional water electrolysis hydrogen production, and can reach 1A / cm under the condition of 0.7V cell voltage. 2 The high current density reduces the energy consumption of hydrogen production from the current lowest 47kWh / kgH2 in the market to 18.4kWh / kgH2, effectively cutting the cost of hydrogen production; the anode reaction products can be used as raw materials for chemical synthesis or sulfur-based batteries to achieve higher added value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of new energy materials and relates to a sulfide ion oxidation electrode and a preparation method and application thereof. Background Art

[0002] As a sustainable green energy carrier, hydrogen is widely regarded as one of the best alternatives to fossil energy in the future due to its high energy density, renewable compatibility and zero pollution emissions. Among several commonly used hydrogen production methods, renewable energy-driven water electrolysis hydrogen production (i.e. "green hydrogen") is a green and sustainable hydrogen production method that has no carbon dioxide emissions during the production process compared with other hydrogen production technologies. However, the currently developed alkaline water electrolysis hydrogen production technology is still based on the coupling of anode oxygen evolution and cathode hydrogen evolution. Due to the limitation of the theoretical potential of the anode oxygen evolution reaction (OER), it causes high energy consumption, making the electricity cost account for nearly 80% of the hydrogen production cost, and it is impossible to fundamentally break through the energy consumption limit of hydrogen production by electrolysis. In particular, the nickel-based electrodes currently widely used usually operate at a higher current density under the working conditions of the electrolyzer, so the actual potential of the anode may reach 1.8V (vs. reversible hydrogen electrode (RHE)) or above, and the energy consumption reaches 47-66kWh / kgH 2 ; Although some high-performance OER electrocatalysts can improve the energy conversion efficiency to a certain extent, they cannot fundamentally change the thermodynamic potential of the oxygen evolution reaction (i.e., 1.23V (vs. RHE)). In order to improve the electrolysis efficiency, the high-concentration alkaline solution used has high corrosion resistance requirements for the electrolyzer, making it difficult to reduce the equipment cost; At present, the optimization of the diaphragm properties in the alkaline electrolyzer has reduced the gas cross-talk phenomenon, but the optimization method is difficult to change the inherent properties of the existing diaphragm (porous fiber membrane and ion exchange membrane), and it is impossible to completely avoid the interpenetration of hydrogen and oxygen, so it is impossible to output high-pressure, high-purity hydrogen, and it is difficult to solve this problem from the perspective of equipment improvement; Adding additional hydrogen compression and purification links also increases the complexity of the equipment and system cost. In addition, the product of the anode is oxygen, which has a low application value. Although it can be used as a raw material for industrial reactions, it is difficult to purify and transport it, and it is difficult to use it at a high value. In most cases, it can only be directly discharged, resulting in a waste of energy and resources. Although some high-performance OER catalysts have been developed for hydrogen production by electrolysis of seawater, these catalysts have poor selectivity and good catalytic performance for chlorine evolution reaction (CER). Therefore, when the electrolyzer actually works at a high current density, it is difficult to completely decouple CER from OER. - Therefore, it is urgent to explore other alternative anode reactions to overcome the above shortcomings and achieve cost-effective and safe hydrogen production by water electrolysis.

[0003] In order to promote the large-scale commercial application of green hydrogen, it is an effective and important way to reduce the cost of hydrogen production by reducing the power consumption in the water splitting process. The power consumption in the water splitting process mainly comes from the high theoretical potential of OER and the slow kinetics caused by the multi-electron-proton coupling reaction process (see formula 1). Sulfur ions (S 2- ) as an electron donor is more likely to provide electrons through oxidation reactions, so the sulfide oxidation reaction (SOR) is thermodynamically more favorable than OER (Formula 2), and can be used as an alternative reaction to OER, coupled with the hydrogen evolution reaction (HER) at the cathode to complete the process of electrolyzing water to produce hydrogen, and greatly reduce the energy consumption of the electrolysis process. In addition, SOR reactants and oxidation products have no adverse effect on HER, and its product polysulfide is soluble in an alkaline environment, and no solid product will be adsorbed on the surface of the electrode or equipment; the anode product will not mix with hydrogen, avoiding the risk of explosion and gas purity problems, and the cathode will be easier to output high-pressure, high-purity hydrogen; the reactant reserves and abundance are very high, which can avoid the limitation of resource issues; SOR is the core step of electrochemical desulfurization, and its product is an important raw material for industrial reactions and sulfur-based batteries, S 2- The coupling of resource conversion and energy-saving hydrogen production is of great significance for environmental remediation, sulfur source recovery and utilization. Using SOR to replace OER will also overcome the long-standing difficulties in hydrogen production by electrolysis of seawater. - ), so the chlorine evolution reaction (CER) is easily triggered at the anode, which not only competes with OER to reduce the Faradaic efficiency of the anode, but also produces ClO - Ions can easily corrode catalysts and plates, shortening the life of the electrolyzer. SOR can occur at a very low anode voltage, so the voltage required under high current density conditions is also far from the starting potential of OER and CER, which can effectively avoid the interference of OER and CER. In summary, coupling the HER at the cathode with the SOR at the anode in the electrolyzer can not only effectively reduce hydrogen production and equipment costs and achieve valuable sulfur recovery at the same time, but also solve many problems caused by chlorine evolution at the anode in hydrogen production by electrolysis of seawater.

[0004] ;

[0005] .

[0006] In the development of SOR catalysts and electrodes, Dalian Institute of Chemical Physics and China University of Science and Technology's Chinese invention patent CN110607531A, although through the intermediate medium (such as hydroquinone, K 3 Fe(CN) 6 , ) is achieved at the anode by a two-step indirect reaction of H 2The oxidation reaction of S replaces OER, but the intermediate medium needs to be excessive and is toxic, and needs to be further removed, which increases the cost of hydrogen production equipment and technical complexity, and limits large-scale application. In addition, the currently developed SOR electrode synthesis process is complex and the synthesis conditions are harsh (such as high temperature, high pressure, etc.), which increases the production cost. The high temperature and high pressure synthesis process inevitably requires fossil fuels to provide a reaction environment, resulting in a large amount of carbon dioxide emissions, which is not conducive to the full chain decarbonization of green hydrogen production, nor is it conducive to the full play of hydrogen in the decarbonization process; the catalyst and electrode synthesis process are difficult to simplify, which is not conducive to large-scale production, and greatly limits the development of SOR and hydrogen production coupling equipment. For example, the graphene-coated metal (CoNi alloy) nanoparticle electrode published by Dalian Institute of Chemical Physics can achieve efficient sulfur ion oxidation reaction (Zhang et al., Highly efficient H 2 production from H 2 S via a robust graphene-encapsulated metal catalyst,Energy & Environmental Science, 2020, 13,119). However, the electrode material preparation requires sintering at 600 ° C in a hydrogen-argon reducing atmosphere and requires multiple post-processing steps. On the other hand, sulfur ions (S 2- ) can easily etch or poison metals, reducing the activity and stability of devices and key components, especially electrodes. The SOR electrodes reported so far have a low operating current density (e.g., 0.1-0.3 A / cm 2 ) The voltage required is too high, and the effect of reducing energy consumption is not obvious, which makes it difficult to meet the conditions for industrial application; the electrode stability that is more important in industrial applications is also poor, making it difficult to truly apply; it has not been verified in a flow electrolysis cell or membrane electrode, and it is unknown whether the electrode material can maintain its electrocatalytic performance in the model solution system in the actual electrolysis device. For example, Chengdu University’s Chinese invention patent CN115652323A discloses an amorphous cobalt sulfide electrode and its application in sulfide ion oxidation-assisted hydrogen production. In an asymmetric acid-base coupled electrolysis system, additional electricity can be generated during the hydrogen production process for sulfur production. However, the electrode failed to investigate the industrial current density (0.5A / cm 2and above), or still has a large potential when reaching industrial current density, and the energy-saving hydrogen production effect is very limited, resulting in doubts about whether the electrode can be used for industrial water electrolysis to produce hydrogen. Finally, the electrodes currently developed for SOR coupled hydrogen production can only be applied to a single alkaline aqueous solution, and the alkali purity requirements for the configured solution are too high. Impurity ions will cause electrode performance degradation, and it is difficult to directly use seawater as an electrolyte, which hinders the development of SOR technology. For example, Shanghai Jiao Tong University’s Chinese invention patent CN112962115A discloses a nickel foam-loaded sulfide electrocatalyst that has both sulfur ion oxidation and water decomposition hydrogen. The electrolyte at the anode is NaOH+Na 2 The electrode cannot be applied or its activity in other solutions has not been investigated, such as widely available seawater, which also limits the scope of application of the electrode. Summary of the invention

[0007] In view of the deficiencies in the prior art, the object of the present invention is to provide a sulfide ion oxidation electrode and a preparation method and application thereof.

[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0009] In one aspect, the present invention provides a sulfide ion oxidation electrode, which includes a substrate and nickel telluride coated with nickel molybdenum oxide supported on the substrate.

[0010] In the present invention, the substrate is supported by nickel molybdenum oxide (NiMoO x ) coated with nickel telluride (NiTe), as a whole as S 2- Ions (Na 2 S or K 2 The anode of the S) electro-oxidation reaction is used to replace the anode oxygen evolution reaction of water electrolysis, and couple the cathode reaction to produce hydrogen. Compared with the existing alkaline water electrolysis hydrogen production technology, since SOR has a lower theoretical potential of the anode reaction, in actual tests, the starting potential of the sulfur ion oxidation electrode is only 0.3V (vs. RHE), which is much smaller than the starting potential of the oxygen evolution reaction and the chlorine evolution reaction. When the sulfur ion oxidation electrode of the present invention catalyzes SOR, it only needs a potential of 0.55V (vs. RHE) to reach 0.5A / cm 2 of high current density.

[0011] In the present invention, SOR is used to replace the anode oxygen evolution reaction, which can break through the theoretical potential limit of electrolytic hydrogen production, greatly reduce electrolytic energy consumption and electricity costs, and thus reduce hydrogen production costs; sulfur ions are typical harmful byproducts in industrial production, and the electrochemical SOR of the sulfur ion oxidation electrode of the present invention can recover sulfur ions without introducing additional oxidants, and electric energy can be provided by renewable energy, which is a greener and more economical method; in addition, the coupling of the anode SOR and the cathode HER makes electrolytic hydrogen production more energy-efficient and reduces the production cost, and at the same time, pollutants can be treated, thereby improving the overall economy of the electrolysis system.

[0012] The high-efficiency sulfur ion oxidation electrode (SOR electrode) provided by the present invention is 2- ions are oxidized to short-chain soluble polysulfides, or subsequently treated with acid or by the addition of carbon dioxide (CO 2 ) and then extract S 8 Solid powder, can achieve S 2- ions and other harmful products, suitable for industrial production processes to produce S 2- ion processing scenarios, and can provide low-priced green hydrogen, polysulfide or solid sulfur powder.

[0013] The high-efficiency SOR electrode provided by the present invention can be used as a raw material for industrial synthesis or sulfur-based batteries, and can achieve higher added value utilization; no gas is generated at the anode, which effectively avoids the problem of hydrogen and oxygen interpenetration, and is also conducive to simplifying the hydrogen purification steps and achieving high-pressure hydrogen output, further reducing production costs.

[0014] The high-efficiency SOR electrode provided by the present invention has an initial potential of only 0.3V (vs. RHE), which is much smaller than the initial potential of the chlorine evolution reaction. It can solve the chlorine evolution problem in the process of seawater electrolysis, greatly promote the development and application of seawater electrolysis hydrogen production technology, and further reduce the cost of hydrogen production.

[0015] Preferably, the substrate comprises a metal, a metal alloy or a non-metal.

[0016] Preferably, the metal includes nickel, titanium or copper.

[0017] Preferably, the metal alloy includes 304L stainless steel, 316 stainless steel or 316L stainless steel, etc.

[0018] Preferably, the non-metal is a carbon material.

[0019] In the present invention, the substrate is in the form of a flat plate or porous or fiber-woven material, and the surface of the substrate contains a corrosion-resistant coating or no coating; the corrosion-resistant coating includes a gold coating or a platinum coating.

[0020] Preferably, the substrate is a nickel substrate, including a nickel sheet, nickel foam (NF), nickel fiber felt or a nickel sintered porous plate.

[0021] When the substrate is nickel foam, the sulfide ion oxidation electrode of the present invention uses nickel foam as the substrate and current collector, and is loaded with nickel molybdenum oxide (NiMoO x ) coated nickel telluride (NiTe) (referred to as NiTe@NiMoO x / NF).

[0022] On the other hand, the present invention provides a method for preparing the sulfide ion oxidation electrode as described above, the preparation method comprising the following steps:

[0023] (1) Loading nickel telluride on a substrate by deposition or in-situ growth;

[0024] (2) Electrochemical deposition is performed on a nickel telluride-loaded substrate to obtain a nickel-molybdenum oxide coating layer on the nickel telluride-loaded substrate, thereby obtaining the sulfide ion oxidation electrode.

[0025] Preferably, the method of loading nickel telluride by deposition or in-situ growth in step (1) comprises the following steps:

[0026] I. Add a water-soluble tellurium source into water, add a reducing agent to the obtained solution, stir, and then add a substrate to react to obtain a substrate loaded with nickel telluride, or;

[0027] II. Add a water-soluble tellurium source into water, and add Ni 2+ A salt and a reducing agent are reacted by stirring to obtain NiTe powder; the NiTe powder is deposited on a substrate by coating or spraying to obtain a substrate loaded with nickel telluride.

[0028] In method I and method II, the water-soluble tellurium source is selected from Na 2 TeO 3 or Te powder;

[0029] In method I and method II, the reducing agent is selected from NaBH 4 or hydrazine hydrate;

[0030] In method II, the The salt is selected from Ni(NO 3 ) 2 、NiCl 2 or Ni(CH 3 COO 2 ;

[0031] In method I and method II, the molar ratio of the water-soluble tellurium source to the reducing agent is independently 1:1 to 1:3, for example 1:1, 1:1.5, 1:1.8, 1:2, 1:2.3, 1:2.5, 1:2.8 or 1:3.

[0032] In method I and method II, the reaction is carried out in a stainless steel or polymer shell autoclave reactor lined with polytetrafluoroethylene or Hastelloy, or can also be carried out in other suitable reaction devices.

[0033] In method I and method II, the reaction temperature is independently 100-140°C, such as 100°C, 110°C, 120°C, 130°C or 140°C, the reaction time is 2-12 hours, such as 2 hours, 4 hours, 6 hours, 8 hours, 10 hours or 12 hours, and the reaction is carried out under a pressure of 0.5-1.5 MPa (e.g., 0.5 MPa, 0.7 MPa, 0.8 MPa, 0.9 MPa, 1.0 MPa, 1.2 MPa, 1.4 MPa or 1.5 MPa).

[0034] In method I and method II, after the reaction is completed, the substrate is naturally cooled to room temperature, washed with anhydrous ethanol and deionized water, and dried in a vacuum oven at 50-100° C. (e.g., 50° C., 60° C., 70° C., 80° C., 90° C. or 100° C.) for 1-24 hours (e.g., 1 hour, 3 hours, 5 hours, 8 hours, 10 hours, 12 hours, 15 hours, 18 hours, 20 hours, 22 hours or 24 hours).

[0035] Preferably, the electrochemical deposition in step (2) specifically comprises the following steps: using a platinum wire as a counter electrode, a saturated calomel electrode (SCE) as a reference electrode, a substrate loaded with nickel telluride (e.g., NiTe / NF) as a working electrode, and a solution containing nickel ions and molybdate ions as an electrodeposition solution to perform electrodeposition to obtain the sulfide ion oxidation electrode.

[0036] Preferably, the electrodeposition solution contains Ni(NO 3 ) 2 6H 2 O and Na 2 MoO 4 ·2H 2 O solution.

[0037] Preferably, the Ni(NO 3 ) 2 6H 2 The concentration of O is 0.1-0.5 mol / L, for example 0.1 mol / L, 0.2 mol / L, 0.3 mol / L, 0.4 mol / L or 0.5 mol / L.

[0038] Preferably, the Na in the electrodeposition solution 2 MoO 4 ·2H 2 The concentration of O is 0.1-0.15 mol / L, for example 0.1 mol / L, 0.12 mol / L, 0.14 mol / L or 0.15 mol / L.

[0039] Preferably, the pH value of the electrodeposition solution is 6.0-6.8, for example, 6.0, 6.1, 6.2, 6.3, 6.4, 6.5, 6.6, 6.7 or 6.8.

[0040] Preferably, the solution resistance between the working electrode and the reference electrode is 3.0-3.5Ω, such as 3.0Ω, 3.1Ω, 3.2Ω, 3.3Ω, 3.4Ω or 3.5Ω.

[0041] Preferably, the electrodeposition is performed in a constant potential mode, wherein the deposition voltage is 0.8-1.0 V (vs. SCE), for example, the deposition voltage may be 0.8 V, 0.9 V or 1.0 V, and the deposition time is 5-10 minutes (eg, 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes or 10 minutes).

[0042] In the present invention, after the electrochemical deposition in step (2), the electrode is carefully cleaned with ultrapure water for 3 times and then vacuum dried at 60° C. for 12 hours.

[0043] In the present invention, the methods for synthesizing the sulfide ion oxidation electrode cannot be listed in full, and the above methods are only for illustration, and other methods for synthesizing the sulfide ion oxidation electrode known in the art may also be used.

[0044] The electrode synthesis process of the present invention is simple, and can be realized by hydrothermal synthesis and electrodeposition. The synthesis process does not require a high temperature environment, and renewable energy can be used to provide electricity, thereby achieving low-carbon or even zero-carbon emissions throughout the synthesis process; the electrodeposition equipment is simple and easier to achieve large-scale production. The electrode is at an industrial current density (0.5A / cm 2 ) has excellent electrolysis stability, which is more beneficial for operation in industrial electrolyzers, helping to promote the development of SOR-coupled hydrogen production technology and the application of hydrogen energy as a key technology for carbon peak and carbon neutrality. Using seawater as the electrolyte is less corrosive than the high-concentration (6M) KOH currently used in alkaline electrolyzers, saving the cost of corrosion-resistant equipment and high-purity KOH.

[0045] On the other hand, the present invention provides a device for producing hydrogen by electrolyzing seawater, which comprises an anode, a cathode and an electrolyte, wherein the anode is the sulfide ion oxidation electrode as described above, and the cathode is based on a metal, a metal alloy or a non-metal and is loaded with nickel phosphide; the electrolyte is seawater.

[0046] In the present invention, NiTe@NiMoO x When the flow cell was loaded with Ni-P / NF as anode and Ni-P / NF as cathode for seawater electrolysis test, the electrolytic cell could reach 5A / cm at only 1.33V at 70℃. 2 The ultra-large current density can reach 1A / cm 2 It can run stably for more than 300 hours at a current density of 1.5000 W without obvious attenuation, and its energy consumption is only 18.4 kWh / kgH 2 The product of the anode is polysulfide, which can be obtained after acidification treatment. It has higher added value than oxygen and can be used as a raw material for industrial reactions or sulfur-based batteries. In addition, no gas is generated at the anode, which avoids mixing with the hydrogen generated by the cathode, which is beneficial to the purification and high-voltage output of hydrogen. The present invention simultaneously realizes energy-saving hydrogen production and green and efficient resource utilization of sulfur ions and seawater.

[0047] The electrolyte of the sulfide ion oxidation electrode of the present invention has wider applicability. After coupling with cathode hydrogen production, only 0.7V cell voltage is required in simulated seawater and natural seawater electrolyte to reach 1.0A / cm 2 and can achieve a current density of 1A / cm 2 It can run for 180 and nearly 300 hours at a current density of 1A / cm2. It is suitable for using offshore wind power generation, solar power generation or tidal power generation in coastal or offshore areas to drive water electrolysis to produce hydrogen. It can directly use seawater as the electrolyte, eliminating the use of high-concentration alkali solution. 2 The DC energy consumption is only 18.4kWh / kg, which can achieve more energy-efficient hydrogen production.

[0048] On the other hand, the present invention provides the use of the sulfide ion oxidation electrode or the seawater electrolysis hydrogen production device as described above in seawater electrolysis hydrogen production.

[0049] Compared with the prior art, the present invention has the following beneficial effects:

[0050] (1) The sulfide oxidation electrode (also called nickel molybdenum oxide / nickel telluride electrode) of the present invention has excellent sulfide oxidation reaction (SOR) catalytic performance, replacing the oxygen evolution reaction at the anode of water electrolysis, and can break through the theoretical potential of traditional water electrolysis to produce hydrogen, reaching 1A / cm under the condition of 0.7V cell voltage. 2The high current density effectively reduces the electrolysis energy consumption, and the DC energy consumption is only 18.4kWh / kgH 2 , which is much lower than the minimum energy consumption of 46kWh / kgH of traditional alkaline electrolyzer 2 .

[0051] (2) Using nickel oxide molybdenum / nickel telluride electrode as SOR catalyst coupled with hydrogen production, the anode reaction product is short-chain soluble polysulfide, which can be obtained after filtration and extraction. 8 Solid powder, anode S 2- To S 8 The conversion rate of the single substance is close to 92%. In addition, both the liquid and solid products can be used as raw materials for industrial reactions or lithium-sulfur batteries, and their added value is higher than the oxygen produced by the traditional electrolysis of water to produce hydrogen.

[0052] (3) The SOR of nickel molybdenum oxide / nickel telluride electrodes can use seawater as the electrolyte. Compared with the alkaline electrolysis of water to produce hydrogen, it can avoid the use of high-purity and high-concentration alkali, reduce the requirements for corrosion-resistant materials in the electrolyzer, and make the electrolyte easier to obtain, saving equipment and production costs, which is conducive to the application and promotion of this technology in coastal and offshore areas.

[0053] (4) The anode SOR product of the nickel molybdenum oxide / nickel telluride electrode is a short-chain soluble polysulfide, without gas generation, which avoids the risk of explosion caused by the interpenetration of hydrogen and oxygen in the traditional electrolytic hydrogen production process. The hydrogen produced by the cathode contains only a small amount of volatile impurities (such as water vapor), which is conducive to simplifying the hydrogen purification steps. More importantly, the cathode can achieve high-pressure hydrogen output, further reducing production costs.

[0054] (5) The nickel molybdenum oxide / nickel telluride electrode is synthesized using low-temperature hydrothermal and electrodeposition methods. Compared with most of the currently reported SOR electrodes, its production process is simpler and more economical, avoids high temperature conditions, reduces carbon emissions during the synthesis process, and can utilize electricity provided by renewable energy, which is more conducive to the large-scale production of electrodes and promotes the development of SOR-coupled hydrogen production technology.

[0055] (6) Compared with other reported SOR electrodes, the electrolyte applicability of nickel molybdenum oxide / nickel telluride electrode is wider. Salt water can be widely used as electrolyte in inland areas, and seawater can be used as electrolyte in coastal or offshore areas. It has more advantages in application to SOR coupled hydrogen production technology.

[0056] (7) Compared with other reported SOR electrodes, the NiO-Mo / NiTe electrode can achieve industrial current density at a lower cell voltage (e.g. ), achieving lower energy consumption for hydrogen production and sulfur ion extraction, and being able to operate stably in seawater for a long time at high current density, achieving more practical energy-saving hydrogen production. BRIEF DESCRIPTION OF THE DRAWINGS

[0057] Figure 1a for NiTe@NiMoO x Scanning electron microscopy image of / NF electrode;

[0058] Figure 1b for NiTe@NiMoO x Transmission electron microscope image of the NF electrode; the small image in the upper left corner is the electron diffraction image of the selected area within the white circle;

[0059] Figure 1c for NiTe@NiMoO x High-resolution transmission electron microscopy image of / NF electrode;

[0060] Figure 1d for NiTe@NiMoO x High-angle annular dark-field scanning transmission electron microscopy image of the / NF electrode;

[0061] Figure 1e for NiTe@NiMoO x Element distribution of transmission electron microscopy-energy spectrum of / NF electrode;

[0062] Figure 1f are X-ray diffraction patterns of different electrodes;

[0063] Figure 1g NiMoO x Scanning electron microscopy images of electrodes;

[0064] Figure 1h NiMoO x Scanning electron microscopy-energy spectrum of the electrode element distribution;

[0065] Figure 2a for NiTe@NiMoO x Ni 2p X-ray photoelectron (XPS) spectra of NiTe / NF electrode and NiTe / NF electrode;

[0066] Figure 2b for NiTe@NiMoO x Te 3d X-ray photoelectron spectra of NiTe / NF electrode and NiTe / NF electrode;

[0067] Figure 2c for NiTe@NiMoO x Mo 3d X-ray photoelectron spectra of NiTe / NF electrode and NiTe / NF electrode;

[0068] Figure 2d for NiTe@NiMoO xRaman spectra of NiTe / NF electrode and NiTe / NF electrode;

[0069] Figure 2e for NiTe@NiMoO x Synchrotron radiation X-ray absorption spectroscopy Mo K-edge spectrum of / NF electrode;

[0070] Figure 2f for NiTe@NiMoO x Fourier transform curve of EXAFS spectrum of / NF electrode;

[0071] Figure 3a is the polarization curve of sulfur ion oxidation reaction at different electrodes;

[0072] Figure 3b for NiTe@NiMoO x Polarization curves of sulfur ion oxidation and oxygen evolution reaction of / NF electrode;

[0073] Figure 3c for NiTe@NiMoO x S / NF electrode after different reaction times of sulfur ion oxidation 2- Absorption in the UV-visible spectrum;

[0074] Figure 3d for NiTe@NiMoO x UV-visible spectra of polysulfides after different reaction times of sulfur ion oxidation on / NF electrode;

[0075] Figure 4a for NiTe@NiMoO x Raman spectra of the / NF electrode at different sulfide ion oxidation reaction times;

[0076] Figure 4b for NiTe@NiMoO x / The color of the anolyte at different sulfide ion oxidation reaction times of the NF electrode;

[0077] Figure 4c for NiTe@NiMoO x X-ray diffraction pattern of the precipitate from the sulfur ion oxidation reaction of the / NF electrode;

[0078] Figure 4d for NiTe@NiMoO x Time-voltage curves of / NF electrode and NiTe / NF electrode at constant current density;

[0079] Figure 5a for NiTe@NiMoO x Polarization curves of / NF electrode in simulated seawater and natural seawater electrolytes;

[0080] Figure 5b for NiTe@NiMoO x / Time-voltage curve of NF electrode under constant current density in simulated seawater;

[0081] Figure 5c for NiTe@NiMoO x Time-voltage curves of the / NF electrode at constant current density in natural seawater. DETAILED DESCRIPTION

[0082] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only used to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0083] Example 1

[0084] NiMoO x The synthesis method of / NF is as follows: electrochemical deposition is carried out in a single-cell three-electrode system, with a clean platinum wire as the counter electrode, a saturated calomel electrode (SCE) as the reference electrode, NF as the working electrode, and the electrodeposition solution as Ni(NO 3 ) 2 6H 2 O (0.15 mol / L) and Na 2 MoO 4 ·2H 2 O (0.15 mol / L), the solution pH is 6.8. Electrodeposition was performed using a constant potential mode, where the deposition voltage was -0.9 V vs. SCE. After a deposition time of 5 minutes, the electrode was cleaned with ultrapure water and dried to obtain NiMo / NF.

[0085] The preparation process of NiTe / NF is as follows: 1mmolNa 2 TeO 3 The powder was dissolved in 65 mL of deionized water and, after continuous magnetic stirring, 5 mmol of NaBH 4 Add the solution and continue stirring until dissolved, then transfer it to a 100mL polytetrafluoroethylene (PTFE)-lined stainless steel autoclave reactor, add clean NF, and heat the reactor to 140°C in an oven for 20 hours. Finally, the reactor was naturally cooled to room temperature, the NF was washed with anhydrous ethanol and deionized water, and dried in a vacuum oven at 60°C for 12 hours to obtain NiTe / NF. Another method is that no NF is added to the reactor, and NiTe powder is first synthesized under the same conditions. Then the NiTe powder is filtered, dispersed in the solution, and loaded on the NF surface by deposition such as coating or spraying to form a NiTe / NF electrode.

[0086] Electrochemical deposition was carried out in a single-cell three-electrode system, with a clean platinum wire as the counter electrode, a saturated calomel electrode (SCE) as the reference electrode, and NiTe / NF prepared by any of the above methods or other methods as the working electrode. The electrodeposition solution was Ni(NO 3 ) 2 6H 2 O (0.15 mol / L) and Na 2 MoO 4 ·2H 2 O (0.15 mol / L), the solution pH was 6.8, and the solution resistance between the working electrode and the reference electrode was about 3.5 Ω. Electrodeposition was performed using a constant potential mode, where the deposition voltage was -0.9 V vs. SCE. After a deposition time of 5 minutes, the electrode was carefully cleaned 3 times with ultrapure water and then vacuum dried at 60 °C for 12 hours to obtain NiTe@NiMoOx / NF.

[0087] Preparation of cathode electrode: weigh 0.4g red phosphorus powder with an electronic analytical balance and put it into one end of the porcelain boat, then put the cleaned nickel foam (3cm×4cm) into the other end of the porcelain boat, about 1cm away from the red phosphorus, and then cover the porcelain boat with a lid. Put the porcelain boat with the above raw materials into a high-temperature tube furnace. In order to ensure that the phosphating is carried out under inert atmosphere, high-purity nitrogen (99.999%) is continuously introduced into the tube furnace, and the gas flow rate is about 50mL / min. This process is maintained for at least 30 minutes to completely exhaust the air in the tube furnace cavity. The heating program is from room temperature to 450℃ at a heating rate of 5℃ / min, and then cooled to 250℃ at a cooling rate of 5℃ / min after 30 minutes of heat preservation, and kept at this temperature for 120 minutes, and finally cooled naturally to room temperature as a NiP / NF electrode.

[0088] Figure 1a Scanning electron microscope (SEM) images and Figure 1b Transmission electron microscope (TEM) images taken using a FEI Tecnai G2 F20 revealed that the nickel molybdenum oxide / nickel telluride catalyst deposited on the NF exhibited a rod-like nanostructure with a diameter of 170 nm and a length of approximately 650 nm. Figure 1b The selected area electron diffraction (SAED) pattern in the inset shows several diffraction spots, and the four brightest diffraction spots in the center are the (101) crystal plane with the strongest diffraction of hexagonal NiTe. Figure 1cHigh-resolution transmission electron microscopy (HRTEM) images show that the nanorods have a typical amorphous structure on the outside and a crystalline structure on the inside. The lattice spacing of 0.296 nm corresponds to the NiTe (101) crystal plane spacing, and no crystal planes of metallic Mo or NiMo alloy were observed. There is no gap between the NiTe crystalline phase and the amorphous structure, indicating that the amorphous phase is deposited in a conformal manner on the entire NiTe nanorod surface. Figure 1d The high-angle annular dark-field scanning transmission electron microscopy (HAADF-STEM) images also show a clear core-shell structure. Figure 1e The TEM-EDS image shows that the outer amorphous phase contains Ni, Mo, and O elements, and the interior is Ni and Te elements. The Malven Panalytical Aeris test X-ray diffraction (XRD) pattern in Figure 1 shows that the diffraction peaks of the synthesized nickel oxide molybdenum / nickel telluride and nickel telluride at 30.9°, 42.8°, 45.7°, 56.2°, 58.2°, and 75.3° match the (101), (102), (110), (201), (103), and (102) plane diffraction peaks of the standard hexagonal NiTe (standard database card number PDF#89-7179), and the other three main diffraction peaks at 44.5°, 51.8°, and 76.4° come from the NF substrate (PDF#87-0712). No diffraction peaks attributed to NiMo or Mo were observed. This also proves that the NiMo electrodeposited on NiTe is amorphous. In addition, the synthesized NiTe / NF electrode only contains the same diffraction peaks as the NiTe@NiMoOx / NF electrode, indicating that only hexagonal NiTe in the crystalline phase was synthesized. x SEM of the electrode ( Figure 1g ) and the corresponding EDS ( Figure 1h ) shows that Ni, Mo, and O elements are uniformly attached to the NF surface, but XRD only shows the diffraction peak of the base NF, which indicates that NiMoO x It is an amorphous structure.

[0089] Figure 2a In the Ni 2p X-ray photoelectron (XPS) spectrum measured using Thermo Fisher Scientific, Thermo Escalab 250Xi, the two binding energy peaks at 853.3 and 870.7 eV can be attributed to the Ni-Te bonding. state, while the binding energy peaks at 856.4 and 874.1 eV correspond to the Ni-O bonded Ni 2+ Compared with NiTe / NF electrode, The signal is greatly reduced in the NiTe@NiMoOx / NF electrode, indicating that most of the NiTe surface is covered by the NiMo layer, but the signal of the internal NiTe can still be detected when the thickness of the NiMo coating is less than 10 nm somewhere. Figure 2b The Te3d spectrum shows that the Te 3d 5 / 2 and Te 3d 3 / 2 From the anion in the Ni-Te bond ; The 577.0 and 587.4 eV signals come from 0-valent Te, which is a phenomenon that can be commonly observed in hydrothermally synthesized tellurides; compared with the NiTe / NF electrode, the 0-valent Te signal is significantly weakened in the NiTe@NiMoOx / NF electrode, which also proves that NiTe is covered by nickel molybdenum oxide. Figure 2c The high-resolution Mo 3d XPS spectrum shows that the Mo in nickel molybdenum oxide / nickel telluride is mainly in the high-valent state. and (231.8 and 234.8 eV), indicating the oxide form of Mo. Figure 2d Raman spectra of NiTe / NF and NiTe@NiMoO measured by Thermo Fisher Scientific, Horiba LabRam HR Evolution x / NF electrodes are all at 50cm -1 -200cm -1 Two NiTe characteristic peaks appear between the wavenumber ranges; NiTe@NiMoO x / 345cm in NF electrode -1 and 900cm -1 The signals at 520 cm and 530 cm come from the bending and stretching vibration modes of the Mo-O bond, respectively. -1 The peak at comes from Ni-O bonding, indicating that nickel and molybdenum exist in the form of oxides. Figure 2e The synchrotron X-ray absorption spectroscopy (XAS) shows that the Mo K-edge XANES spectrum of the NiTe@NiMoOx / NF electrode exhibits a strong edge pre-peak, indicating that the triply degenerate 3d and 4p orbitals that form the antibonding state have the same symmetry and can hybridize, resulting in the 3d orbital having the properties of the 4p orbital. The 1s to 3d transition can be achieved in the Mo atom, and the charge transfer from the ligand to the metal occurs, resulting in a strong edge pre-peak, and the existence of a square planar D4h symmetry in the Mo central atom. Figure 2f The Fourier transform curve of EXAFS spectrum is The significant peak at comes from Mo-O coordination, indicating that Mo exists mainly in the form of Mo-O bonds with a coordination number of about 4, indicating that the surface of the nickel molybdenum oxide / nickel telluride electrode is in the form of oxide, which is consistent with the above XPS results. The nickel molybdenum oxide on the surface of the NiTe@NiMoOx / NF electrode can repel Cl in seawater - ions and prevent them from being adsorbed on the electrode surface, thereby inhibiting Cl - The corrosion effect of ions improves the stability of the electrode.

[0090] Example 2

[0091] The present invention also provides the use of nickel oxide molybdenum / nickel telluride electrodes in the production of hydrogen by sulphur ion oxidation coupling.

[0092] Simulated seawater was prepared as the anolyte, containing 1M KOH, 0.5M NaCl and 1M Na 2 S. Figure 3a The SOR polarization curves of different electrodes show that NiTe@NiMoO x The / NF electrode can achieve 500 mA / cm at a potential of 0.55 V (vs. RHE). 2 The high current density is better than that of the comparative electrodes (NiTe / NF, NiMoO x / NF) and commonly used commercial electrode materials (Pt / C, RuO 2 and NF). Figure 3b NiTe@NiMoO x The SOR and OER performance of NF are compared at 500 mA cm -2 The potential required under the current density condition is reduced by 1.12V, which is equivalent to a 29.7kWh / kg reduction in the DC energy consumption for hydrogen production, which is greatly reduced compared to the energy consumption (47-66kWh / kg) of alkaline electrolyzers currently on the market. x / NF electrode at 500mA / cm 2 After running at a certain current density for a certain time, the anolyte was characterized by UV-visible spectroscopy and Raman spectroscopy. Figure 3c In the UV-visible spectrum tested by HATACHI UH4150, S 2- The absorption peak gradually decreases with the electrolysis time, indicating that S 2- At the same time, Figure 3d Polysulfide (S x 2-, 2≤x≤4) and the intensity gradually increases with time. According to the Lambert-Beer law, the absorbance is proportional to the ion concentration, indicating that SOR continuously forms short-chain soluble polysulfides. Figure 4a The SOR reaction time-dependent 2D Raman map shows that as the reaction time increases, the peak at 449 cm -1 The Raman peak at 8 2- and S 4 2- The characteristic peak of 2573cm -1 The Raman peak at 2- The characteristic peak of Figure 4b The color of the anolyte also changes from colorless and light yellow to brownish red. These characteristics indicate that the concentration of polysulfide formation increases over time. Acidification of the anolyte with 37% hydrochloric acid can obtain a solid precipitate. Figure 4c The XRD diffraction pattern of the precipitate proves that it is S 8 Powder (standard database card number PDF#89-2600), indicating that after a certain period of electrolysis, harmful S ions can be oxidized into S single substance with a certain added value. After calculation, S 2- The conversion rate of NiTe@NiMoO x / NF electrode at industrial current density (500mA / cm 2 ) also has excellent stability under . Figure 4d It shows that NiTe / NF electrode is at 500mA / cm 2 The catalytic SOR can only run for 2 hours at a current density of 1.37 W, while NiTe@NiMoO x The / NF electrode showed no obvious attenuation after operating at this current density for more than 100 hours, indicating that the electrode has the prospect of being used in commercial high-power electrolyzers.

[0093] The performance of hydrogen production from seawater assisted by SOR was tested in a flow electrolysis cell using homemade nickel phosphide as cathode and nickel molybdenum oxide / nickel telluride electrode as anode. Figure 5a As shown in Figure 2, at 70°C, the polarization curves of natural seawater and simulated seawater electrolytes almost overlap, and a current of 1.0 A / cm2 can be achieved at a cell voltage of 0.7 V. 2 The current density of 4A / cm2 in simulated seawater shows that the performance of nickel molybdenum oxide / nickel telluride electrode is universal in different electrolytes and is suitable for a variety of electrolyte formulations, and can achieve energy-saving hydrogen production and sulfur ion extraction. More importantly, in simulated seawater, the current density of 4A / cm2 is 2The current density required is only 1.2V, which is still lower than the theoretical potential of water electrolysis, proving the large-scale application prospect of nickel oxide molybdenum / nickel telluride electrode in SOR coupled hydrogen production technology. The stability test of the electrolytic cell shows that the electrolytic cell has a stable performance at 1.0A / cm 2 Under the current density of simulated seawater ( Figure 5b ) and natural seawater ( Figure 5c ) for 180 hours and nearly 300 hours respectively. The slight performance degradation during operation was mainly due to the consumption of sulfide ions. 2 The performance can be fully restored after S. In this electrolyzer, the hydrogen production current density is 1.0A / cm 2 The DC energy consumption is only 18.4kWh / kgH 2 , which is much lower than the minimum energy consumption of 46kWh / kgH of traditional alkaline electrolyzer 2 , which fully demonstrated the energy-saving hydrogen production and sulfur extraction performance of the electrode at industrial current density.

[0094] The applicant declares that the present invention illustrates the sulfide ion oxidation electrode and its preparation method and application through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A hydrogen production device by electrolyzing seawater, characterized in that: The device for producing hydrogen by electrolyzing seawater includes an anode, a cathode and an electrolyte, wherein the anode is a sulfur ion oxidation electrode, and the cathode is based on a metal, a metal alloy or a non-metal and is loaded with nickel phosphide; the anode electrolyte contains KOH, NaCl and Na2S, and the sulfur ion oxidation electrode includes a substrate and nickel telluride coated with nickel molybdenum oxide loaded on the substrate, wherein the nickel telluride coated with nickel molybdenum oxide presents a rod-shaped nanostructure with a diameter of 170 nm, and the nickel molybdenum oxide is an amorphous structure.

2. The hydrogen production device by electrolysis of seawater according to claim 1, characterized in that: The substrate comprises a metal, a metal alloy or a non-metal; The metal includes nickel, titanium or copper; The metal alloy includes 304L stainless steel, 316 stainless steel or 316L stainless steel; The non-metal is a carbon material.

3. The hydrogen production device by electrolysis of seawater according to claim 1 or 2, characterized in that: The substrate is in the form of a flat plate or porous or fiber-woven material, and the surface of the substrate contains a corrosion-resistant coating or does not contain a coating; the corrosion-resistant coating includes a gold coating or a platinum coating.

4. The hydrogen production device by electrolysis of seawater according to claim 1, characterized in that: The substrate is a nickel substrate, including a nickel sheet, nickel foam, nickel fiber felt or a nickel sintered porous plate.

5. The hydrogen production device by electrolysis of seawater according to claim 1, characterized in that: The preparation method of the sulfide ion oxidation electrode comprises the following steps: (1) Loading nickel telluride on a substrate by deposition or in-situ growth; (2) Electrochemical deposition is performed on a nickel telluride-loaded substrate to obtain a nickel-molybdenum oxide coating layer on the nickel telluride-loaded substrate, thereby obtaining the sulfide ion oxidation electrode.

6. The hydrogen production device by electrolysis of seawater according to claim 5, characterized in that: The method of loading nickel telluride by deposition or in-situ growth in step (1) comprises: I. Add a water-soluble tellurium source into water, add a reducing agent to the obtained solution, stir, and then add a substrate to react to obtain a substrate loaded with nickel telluride, or; II. Add a water-soluble tellurium source into water, and add Ni 2+ A salt and a reducing agent are added, and NiTe powder is obtained after stirring and reacting; the NiTe powder is deposited on a substrate by coating or spraying to obtain a substrate loaded with nickel telluride; In method I and method II, the water-soluble tellurium source is selected from Na2TeO3 or Te powder; In method I and method II, the reducing agent is selected from NaBH4 or hydrazine hydrate; In method II, the Ni 2+ The salt is selected from Ni(NO3)2, NiCl2 or Ni(CH3COO)2; In method I and method II, the molar ratio of the water-soluble tellurium source to the reducing agent is independently 1:1 to 1:5; In Method I and Method II, the reaction is carried out in a stainless steel or polymer shell autoclave reactor lined with polytetrafluoroethylene or Hastelloy; In method I and method II, the reaction temperature is independently 100-140° C., the reaction time is 2-30 hours, and the reaction is carried out under a pressure of 0.5-1.5 MPa; In method I and method II, after the reaction is completed, the substrate is naturally cooled to room temperature, washed with anhydrous ethanol and deionized water, and dried in a vacuum oven at 50-100° C. for 1-24 hours.

7. The hydrogen production device by electrolysis of seawater according to claim 5, characterized in that: The electrochemical deposition in step (2) specifically comprises the following steps: using a platinum wire as a counter electrode, a saturated calomel electrode as a reference electrode, a substrate loaded with nickel telluride as a working electrode, and a solution containing nickel ions and molybdate ions as an electro-deposition solution to perform electro-deposition to obtain the sulfide ion oxidation electrode.

8. The hydrogen production device by electrolysis of seawater according to claim 7, characterized in that: The electrodeposition solution is a solution containing Ni(NO3)2·6H2O and Na2MoO4·2H2O; The concentration of Ni(NO3)2·6H2O in the electrodeposition solution is 0.1-0.5 mol / L; The concentration of Na2MoO4·2H2O in the electrodeposition solution is 0.1-0.15 mol / L; The pH value of the electrodeposition solution is 6.0-6.8; The solution resistance between the working electrode and the reference electrode is 3.0-3.5Ω; The electrodeposition was performed using a constant potential mode, wherein the deposition voltage was 0.8-1.0 V vs. SCE and the deposition time was 5-10 minutes.

9. Use of the seawater electrolysis hydrogen production device according to any one of claims 1 to 8 in seawater electrolysis hydrogen production.