A high silicon ultra-low carbon nitric acid resistant stainless steel flux-cored welding wire
By preparing high-silicon, ultra-low-carbon, nitric acid-resistant stainless steel flux-cored welding wire, the problem of insufficient resistance to nitric acid corrosion in traditional welding materials has been solved, enabling efficient welding of the wire in highly corrosive environments, and exhibiting excellent welding performance and cost-effectiveness.
Patent Information
- Application Number
- CN202411045786.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-08-01
AI Technical Summary
Traditional C4 stainless steel welding materials are insufficient in terms of resistance to nitric acid corrosion, making it difficult to meet the requirements of demanding applications.
High-silicon ultra-low carbon flux powder is prepared by uniformly mixing silicon powder, nickel powder, chromium powder, manganese powder, molybdenum powder, aluminum powder, titanium powder, and iron powder and vacuum drying. It is rolled into U-shape and drawn into wire to form flux-cored welding wire. A corrosion-resistant coating is sprayed on the surface and cured to form a corrosion-resistant coating, thus producing high-silicon ultra-low carbon nitric acid resistant stainless steel flux-cored welding wire.
It significantly improves the corrosion resistance of welding wire, especially in highly corrosive media such as nitric acid, reduces the carbon content in the welding wire, improves the crack resistance and welding quality of the welding wire, has excellent welding process performance, reduces production costs, and meets the needs of large-scale production.
Smart Images

Figure CN118595665B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of C4 stainless steel welding materials, and in particular to a high-silicon ultra-low carbon nitric acid-resistant stainless steel flux-cored welding wire. Background Art
[0002] C4 steel is a high carbon and high chromium die steel, belonging to cold working die steel, with excellent hardness and wear resistance. It is usually used to manufacture cold working dies that require high wear resistance and impact resistance, such as stamping dies, shear blades, cold extrusion dies, etc.
[0003] C4 steel is mainly composed of chromium, nickel and silicon, and also contains molybdenum, zirconium and casting auxiliary elements. Due to its excellent corrosion resistance and comprehensive performance, C4 steel is widely used in the following fields:
[0004] Petrochemical industry: used to manufacture pipelines, storage tanks, reactors and other equipment;
[0005] Marine engineering field: used in manufacturing ships, offshore platforms, submarine pipelines and other equipment;
[0006] Energy field: used to manufacture nuclear power plant reactor parts, boiler pipes and other equipment
[0007] Environmental protection field: used to manufacture environmental protection equipment such as waste gas treatment equipment and sewage treatment facilities;
[0008] In the field of C4 stainless steel welding materials, with the development of industrial technology, the requirements for welding materials are increasing. Especially in the above fields, they are often exposed to various corrosive substances. Therefore, the corrosion resistance of the material is very important. When facing strong acid corrosion environments such as nitric acid, the corrosion resistance of the equipment directly affects its service life and safety. Traditional C4 stainless steel welding materials have deficiencies in nitric acid corrosion resistance and are difficult to meet high-demand application scenarios. Therefore, it is of great practical significance to develop a high-silicon ultra-low carbon nitric acid-resistant stainless steel flux-cored welding wire. Summary of the invention
[0009] In order to overcome the above-mentioned technical problems, the purpose of the present invention is to provide a high-silicon ultra-low carbon nitric acid-resistant stainless steel flux-cored welding wire: by uniformly mixing silicon powder, nickel powder, chromium powder, manganese powder, molybdenum powder, aluminum powder, titanium powder and iron powder and vacuum drying to obtain high-silicon ultra-low carbon powder, rolling a low-carbon steel strip into a U-shape, adding high-silicon ultra-low carbon powder, then sealing and rolling into an O-shape, and then drawing to make a flux-cored welding wire, spraying a corrosion-resistant coating on the surface of the flux-cored welding wire, curing to form a corrosion-resistant coating, and then drying to obtain a high-silicon ultra-low carbon nitric acid-resistant stainless steel flux-cored welding wire, which solves the problem that traditional welding materials are insufficient in nitric acid corrosion resistance and are difficult to meet high-demand application scenarios.
[0010] The purpose of the present invention can be achieved by the following technical solutions:
[0011] A high-silicon ultra-low carbon nitric acid-resistant stainless steel flux-cored welding wire is prepared by the following steps:
[0012] Step 1: Weigh 4.8-6.8 parts of silicon powder, 13.8-15.6 parts of nickel powder, 17.1-19.5 parts of chromium powder, 0.8-1.6 parts of manganese powder, 0.3-0.5 parts of molybdenum powder, 3-7 parts of aluminum powder, 1-3 parts of titanium powder and 42-56 parts of iron powder according to weight parts, and set aside;
[0013] Step 2: Evenly mix silicon powder, nickel powder, chromium powder, manganese powder, molybdenum powder, aluminum powder, titanium powder and iron powder and vacuum dry them to obtain high silicon ultra-low carbon powder;
[0014] Step 3: Roll a low-carbon steel strip with a width of 10 mm and a thickness of 0.3 mm into a U-shape, add high-silicon ultra-low carbon powder with a filling amount of 30%, then seal and roll it into an O-shape, and then draw it to make a flux-cored welding wire;
[0015] Step 4: Spray the corrosion-resistant coating on the surface of the flux-cored welding wire, solidify it to form a corrosion-resistant coating, and then dry it at a temperature of 80-100°C to obtain a high-silicon ultra-low carbon nitric acid-resistant stainless steel flux-cored welding wire;
[0016] Wherein, the corrosion-resistant coating is prepared by the following steps:
[0017] Step s1: pentaerythritol, sodium hydroxide and anhydrous tetrahydrofuran are added to a four-necked flask equipped with a stirrer, a thermometer, an air guide tube, a constant pressure dropping funnel and a reflux condenser, and nitrogen is introduced for protection. The mixture is stirred for reaction for 10-15 minutes at a temperature of 25-30° C. and a stirring rate of 300-400 r / min. Then, propylene bromide is added dropwise while stirring, and the dropping rate is controlled to be 1-2 drops / s. After the dropwise addition is completed, the temperature is raised to reflux and the stirring reaction is continued for 10-15 hours. After the reaction is completed, the reaction product is cooled to room temperature, and then washed with saturated brine and distilled water for 2-3 times in sequence, and then dried with anhydrous sodium sulfate, and then vacuum filtered, and the filtrate is rotary evaporated to remove the solvent to obtain an intermediate product A;
[0018] Step s2: Add pentafluoro-1-butanol, mercaptopropionic acid, p-toluenesulfonic acid and toluene into a three-necked flask equipped with a stirrer, a thermometer and an air duct, stir and react for 25-30 minutes at a temperature of 25-30° C. and a stirring rate of 300-400 r / min, then heat to 90-95° C. and continue stirring and reacting for 6-8 hours. After the reaction is completed, cool the reaction product to room temperature, and then remove the solvent by rotary evaporation to obtain an intermediate product B;
[0019] Step s3: add intermediate product A, intermediate product B, triethylamine and dichloromethane into a three-necked flask equipped with a stirrer, a thermometer, an air duct and a reflux condenser, introduce nitrogen protection, stir and react for 20-30 minutes at a temperature of 25-30°C and a stirring rate of 300-400r / min, then heat to reflux and continue stirring and reacting for 2-3 hours. After the reaction is completed, cool the reaction product to room temperature, then vacuum filter, and rotary evaporate the filtrate to remove the solvent to obtain a corrosion-resistant material;
[0020] Step s4: adding graphite powder and sodium nitrate to a three-necked flask equipped with an agitator and a thermometer, stirring the mixture for 20-30 minutes at a temperature of 0-5°C and a stirring rate of 300-400 r / min, then adding concentrated sulfuric acid while stirring, continuing to stir the mixture for 20-30 minutes after the addition is complete, then adding potassium permanganate and continuing to stir the mixture for 20-30 minutes, then adding deionized water and heating the mixture to 90-95°C and continuing to stir the mixture for 3-4 hours, after the reaction is completed, pouring the reaction product into a hydrogen peroxide solution, then allowing it to stand and precipitate, then vacuum filtering, washing the filter cake with a hydrochloric acid solution and distilled water for 3-5 times in sequence, then placing it in a vacuum drying oven, and drying it at a temperature of 70-75°C for 2-3 hours to obtain graphene oxide;
[0021] Step s5: adding graphene oxide, N,N-dimethylformamide and dithionyl chloride into a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a reflux condenser, introducing nitrogen protection, stirring the reaction at a temperature of 25-30°C and a stirring rate of 300-400r / min for 10-15min, then heating to reflux and continuing to stir the reaction for 10-15h, after the reaction is completed, cooling the reaction product to room temperature, then centrifuging, placing the precipitate in a vacuum drying oven, and drying it at a temperature of 70-75°C for 2-3h to obtain graphene chloride;
[0022] Step s6: adding chlorinated graphene and 2-mercaptoethanol to a three-necked flask equipped with a stirrer, a thermometer and an air duct, introducing nitrogen protection, stirring the reaction at a temperature of 25-30° C. and a stirring rate of 300-400 r / min for 10-15 min, then heating to 60-65° C. and continuing to stir the reaction for 20-25 h. After the reaction is completed, the reaction product is cooled to room temperature, then centrifuged, and the precipitate is placed in a vacuum drying oven and dried at a temperature of 70-75° C. for 2-3 h to obtain mercapto graphene;
[0023] Step s7: Add the corrosion-resistant material, mercapto graphene, triethylamine and N,N-dimethylformamide into a three-necked flask equipped with a stirrer and a thermometer, stir and react for 2-3 hours at a temperature of 45-50°C and a stirring rate of 300-400 r / min to obtain a corrosion-resistant coating.
[0024] As a further solution of the present invention: the usage ratio of the pentaerythritol, sodium hydroxide, anhydrous tetrahydrofuran and propylene bromide in step s1 is 10 mmol: 45-50 mmol: 50-60 mL: 40-45 mmol.
[0025] As a further solution of the present invention: the usage ratio of pentafluoro-1-butanol, mercaptopropionic acid, p-toluenesulfonic acid and toluene in step s2 is 10 mmol: 11-13 mmol: 0.05-0.09 g: 40-50 mL.
[0026] As a further solution of the present invention: the usage ratio of the intermediate product A, the intermediate product B, triethylamine and dichloromethane in step s3 is 10 mmol: 20-35 mmol: 35-40 mmol: 70-80 mL.
[0027] As a further solution of the present invention: the usage ratio of the graphite powder, sodium nitrate, concentrated sulfuric acid, potassium permanganate and deionized water in step s4 is 5g:1.2-1.8g:30-35mL:12-16g:100-120mL.
[0028] As a further solution of the present invention: the mass fraction of the concentrated sulfuric acid in step s4 is 96-98%, the mass fraction of the hydrogen peroxide solution is 20-25%, and the mass fraction of the hydrochloric acid solution is 15-20%.
[0029] As a further solution of the present invention: the usage ratio of the graphene oxide, N,N-dimethylformamide and dithionyl chloride in step s5 is 1 g: 10-15 mL: 35-40 mL.
[0030] As a further solution of the present invention: the usage ratio of the chlorinated graphene and 2-mercaptoethanol in step s6 is 1 g: 30-35 mL.
[0031] As a further solution of the present invention: the usage ratio of the corrosion-resistant material, mercapto graphene, triethylamine and N,N-dimethylformamide in step s7 is 30-40g: 1-5g: 2-8g: 60-70g.
[0032] Beneficial effects of the present invention:
[0033] The invention discloses a high-silicon ultra-low carbon nitric acid-resistant stainless steel flux-cored welding wire. The high-silicon ultra-low carbon powder is obtained by uniformly mixing silicon powder, nickel powder, chromium powder, manganese powder, molybdenum powder, aluminum powder, titanium powder and iron powder and vacuum drying. A low-carbon steel strip is rolled into a U-shape, and the high-silicon ultra-low carbon powder is added. The strip is then sealed and rolled into an O-shape, and then wire-drawn to obtain a flux-cored welding wire. A corrosion-resistant coating is sprayed on the surface of the flux-cored welding wire, cured to form a corrosion-resistant coating, and then dried to obtain a high-silicon ultra-low carbon nitric acid-resistant stainless steel flux-cored welding wire. The invention discloses a high-silicon ultra-low carbon nitric acid-resistant stainless steel flux-cored welding wire. The invention discloses a high-silicon ultra-low carbon nitric acid-resistant stainless steel flux-cored welding wire. The corrosion resistance of the welding wire is effectively improved, especially in highly corrosive media such as nitric acid, its corrosion resistance is significantly improved, and it is suitable for welding operations in highly corrosive environments, and the carbon content in the welding wire is reduced, thereby improving the crack resistance and welding quality of the welding wire, so that the welding wire has excellent welding process performance, is easy to operate, easy to use, and has good tensile strength, yield point and elongation mechanical properties; the present invention reduces production costs and improves production efficiency by optimizing the formula and preparation process, and meets the needs of large-scale production.
[0034] In the process of preparing high-silicon ultra-low carbon nitric acid-resistant stainless steel flux-cored welding wire, a corrosion-resistant coating is first prepared, pentaerythritol and propylene bromide are reacted, the hydroxyl group on the pentaerythritol reacts with the bromine atom on the propylene bromide, an olefin group is introduced, and an intermediate product A is obtained, then pentafluoro-1-butanol and mercaptopropionic acid are reacted, the hydroxyl group on the pentafluoro-1-butanol reacts with the carboxyl group on the mercaptopropionic acid, a thiol group is introduced, and an intermediate product B is obtained, then the intermediate product A and the intermediate product B react, the olefin group on the intermediate product A and the thiol group on the intermediate product B undergo a click chemical reaction, and a corrosion-resistant material is obtained, then graphite powder is used as a raw material to prepare graphene oxide, then the graphene oxide is treated with thionyl chloride, so that the carboxyl group on the graphene oxide is converted into an acyl chloride group, and acyl chloride graphene is obtained, then the acyl chloride graphene and 2-mercaptoethanol react, the acyl chloride group on the acyl chloride graphene and the hydroxyl group on the 2-mercaptoethanol react, The invention relates to a method for preparing a corrosion-resistant coating by reacting a thiol group with a thiol group, introducing a thiol group, and obtaining thiol graphene. Finally, the corrosion-resistant material and the thiol graphene are used as main raw materials to prepare the corrosion-resistant coating. The molecular structure of the corrosion-resistant material in the corrosion-resistant coating contains a large number of CF bonds, which give it excellent chemical resistance and can prevent the welding wire from being corroded by nitric acid. The corrosion-resistant material also contains olefin groups, which can connect it with the thiol graphene in the form of chemical bonds, thereby ensuring the bonding force of the coating. The graphene is distributed in layers in the coating and can form a dense physical isolation layer with good physical isolation effect. At the same time, the graphene has good electrical conductivity and can transfer the electrons lost on the surface of the metal substrate through the graphene, thereby inhibiting the oxidation reaction of the metal and slowing down the corrosion rate. Therefore, under the synergistic effect of the corrosion-resistant material and the thiol graphene, it is given excellent corrosion resistance and can further enhance the corrosion resistance of the welding wire. DETAILED DESCRIPTION
[0035] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0036] Embodiment 1:
[0037] This embodiment is a high-silicon ultra-low carbon nitric acid-resistant stainless steel flux-cored welding wire, which is prepared by the following steps:
[0038] Step T1: 10 mmol of pentaerythritol, 45 mmol of sodium hydroxide and 50 mL of anhydrous tetrahydrofuran are added to a four-necked flask equipped with a stirrer, a thermometer, a gas guide tube, a constant pressure dropping funnel and a reflux condenser, and nitrogen is introduced for protection. The mixture is stirred for reaction at a temperature of 25° C. and a stirring rate of 300 r / min for 10 min, and then 40 mmol of propylene bromide is added dropwise while stirring, and the dropping rate is controlled to be 1 drop / s. After the dropwise addition is completed, the temperature is raised to reflux and the stirring reaction is continued for 10 h. After the reaction is completed, the reaction product is cooled to room temperature, and then washed with saturated brine and distilled water twice in sequence, and then dried with anhydrous sodium sulfate, and then vacuum filtered, and the filtrate is rotary evaporated to remove the solvent to obtain an intermediate product A;
[0039] Step T2: 10 mmol of pentafluoro-1-butanol, 11 mmol of mercaptopropionic acid, 0.05 g of p-toluenesulfonic acid and 40 mL of toluene were added to a three-necked flask equipped with a stirrer, a thermometer and a gas guide tube, and stirred for reaction at a temperature of 25° C. and a stirring rate of 300 r / min for 25 min, then heated to 90° C. and continued to stir for reaction for 6 h. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation to obtain an intermediate product B;
[0040] Step T3: 10 mmol of intermediate product A, 20 mmol of intermediate product B, 35 mmol of triethylamine and 70 mL of dichloromethane were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and nitrogen was introduced for protection. The reaction was stirred for 20 minutes at a temperature of 25° C. and a stirring rate of 300 r / min, and then the temperature was raised to reflux and the stirring reaction was continued for 2 hours. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered, and the filtrate was rotary evaporated to remove the solvent to obtain a corrosion-resistant material;
[0041] Step T4: 5 g of graphite powder and 1.2 g of sodium nitrate were added to a three-necked flask equipped with a stirrer and a thermometer, and stirred for 20 min at a temperature of 0 ° C and a stirring rate of 300 r / min, and then 30 mL of 96% concentrated sulfuric acid was added while stirring, and the stirring reaction was continued for 20 min after the addition was completed, and then 12 g of potassium permanganate was added and the stirring reaction was continued for 20 min, and then 100 mL of deionized water was added and the temperature was raised to 90 ° C and the stirring reaction was continued for 3 h. After the reaction was completed, the reaction product was poured into a 20% hydrogen peroxide solution, and then allowed to stand and precipitate, and then vacuum filtered, and the filter cake was washed with a 15% hydrochloric acid solution and distilled water for 3 times in sequence, and then placed in a vacuum drying oven and dried at a temperature of 70 ° C for 2 h to obtain graphene oxide;
[0042] Step T5: 1 g of graphene oxide, 10 mL of N,N-dimethylformamide and 35 mL of thionyl chloride were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and nitrogen was introduced for protection. The mixture was stirred for 10 min at a temperature of 25° C. and a stirring rate of 300 r / min, and then the mixture was heated to reflux and continued to stir for 10 h. After the reaction was completed, the reaction product was cooled to room temperature and then centrifuged. The precipitate was placed in a vacuum drying oven and dried at a temperature of 70° C. for 2 h to obtain graphene chloride;
[0043] Step T6: 1 g of acyl chloride graphene and 30 mL of 2-mercaptoethanol were added to a three-necked flask equipped with a stirrer, a thermometer and an air guide tube, and nitrogen was introduced for protection. The reaction was stirred at a temperature of 25° C. and a stirring rate of 300 r / min for 10 min, and then the temperature was raised to 60° C. and the stirring reaction was continued for 20 h. After the reaction was completed, the reaction product was cooled to room temperature and then centrifuged. The precipitate was placed in a vacuum drying oven and dried at a temperature of 70° C. for 2 h to obtain mercapto graphene;
[0044] Step T7: 30 g of corrosion-resistant material, 1 g of mercapto graphene, 2 g of triethylamine and 60 g of N,N-dimethylformamide were added to a three-necked flask equipped with a stirrer and a thermometer, and stirred for reaction at a temperature of 45° C. and a stirring rate of 300 r / min for 2 h to obtain a corrosion-resistant coating;
[0045] Step T8: Weigh 4.8 parts of silicon powder, 13.8 parts of nickel powder, 17.1 parts of chromium powder, 0.8 parts of manganese powder, 0.3 parts of molybdenum powder, 3 parts of aluminum powder, 1 part of titanium powder and 42 parts of iron powder according to weight parts, and set aside;
[0046] Step T9: mixing silicon powder, nickel powder, chromium powder, manganese powder, molybdenum powder, aluminum powder, titanium powder and iron powder uniformly and vacuum drying to obtain high silicon ultra-low carbon powder;
[0047] Step T10: rolling a low-carbon steel strip with a width of 10 mm and a thickness of 0.3 mm into a U-shape, adding high-silicon ultra-low carbon powder with a filling amount of 30%, then sealing and rolling into an O-shape, and then drawing to make a flux-cored welding wire;
[0048] Step T11: Spray the corrosion-resistant coating onto the surface of the flux-cored welding wire, solidify it to form a corrosion-resistant coating, and then dry it at a temperature of 80° C. to obtain a high-silicon ultra-low carbon nitric acid-resistant stainless steel flux-cored welding wire.
[0049] Embodiment 2:
[0050] This embodiment is a high-silicon ultra-low carbon nitric acid-resistant stainless steel flux-cored welding wire, which is prepared by the following steps:
[0051] Step T1: 10 mmol of pentaerythritol, 48 mmol of sodium hydroxide and 55 mL of anhydrous tetrahydrofuran were added to a four-necked flask equipped with a stirrer, a thermometer, a gas guide tube, a constant pressure dropping funnel and a reflux condenser, and nitrogen was introduced for protection. The reaction was stirred for 12 min at a temperature of 28° C. and a stirring rate of 350 r / min, and then 42 mmol of propylene bromide was added dropwise while stirring, and the dropping rate was controlled to be 1 drop / s. After the dropwise addition was completed, the temperature was raised to reflux and the stirring reaction was continued for 12 h. After the reaction was completed, the reaction product was cooled to room temperature, and then washed with saturated brine and distilled water three times in sequence, and then dried with anhydrous sodium sulfate, and then vacuum filtered, and the filtrate was rotary evaporated to remove the solvent to obtain an intermediate product A;
[0052] Step T2: 10 mmol of pentafluoro-1-butanol, 12 mmol of mercaptopropionic acid, 0.07 g of p-toluenesulfonic acid and 45 mL of toluene were added to a three-necked flask equipped with a stirrer, a thermometer and a gas guide tube, and stirred for reaction at a temperature of 28° C. and a stirring rate of 350 r / min for 28 min, then heated to 92° C. and continued to stir for reaction for 7 h. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation to obtain an intermediate product B;
[0053] Step T3: 10 mmol of intermediate product A, 27 mmol of intermediate product B, 38 mmol of triethylamine and 75 mL of dichloromethane were added to a three-necked flask equipped with a stirrer, a thermometer, a gas duct and a reflux condenser, and nitrogen was introduced for protection. The mixture was stirred for reaction at a temperature of 28° C. and a stirring rate of 350 r / min for 25 min, and then the mixture was heated to reflux and continued to stir for 2.5 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered. The filtrate was rotary evaporated to remove the solvent to obtain a corrosion-resistant material;
[0054] Step T4: 5 g of graphite powder and 1.5 g of sodium nitrate were added to a three-necked flask equipped with a stirrer and a thermometer, and stirred for 25 min at a temperature of 3 ° C and a stirring rate of 350 r / min, and then 32 mL of 97% concentrated sulfuric acid was added while stirring. After the addition was completed, the stirring reaction was continued for 25 min, and then 14 g of potassium permanganate was added and the stirring reaction was continued for 25 min, and then 110 mL of deionized water was added and the temperature was raised to 92 ° C and the stirring reaction was continued for 3.5 h. After the reaction was completed, the reaction product was poured into a 22% hydrogen peroxide solution, and then allowed to stand and precipitate, and then vacuum filtered, and the filter cake was washed 4 times with a 18% hydrochloric acid solution and distilled water in turn, and then placed in a vacuum drying oven and dried at a temperature of 72 ° C for 2.5 h to obtain graphene oxide;
[0055] Step T5: 1 g of graphene oxide, 12 mL of N,N-dimethylformamide and 38 mL of thionyl chloride were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and nitrogen was introduced for protection. The mixture was stirred at 28° C. and a stirring rate of 350 r / min for 12 min, and then the mixture was heated to reflux and continued to stir for 12 h. After the reaction was completed, the reaction product was cooled to room temperature and then centrifuged. The precipitate was placed in a vacuum drying oven and dried at 72° C. for 2.5 h to obtain graphene chloride;
[0056] Step T6: 1 g of acyl chloride graphene and 32 mL of 2-mercaptoethanol were added to a three-necked flask equipped with a stirrer, a thermometer and an air duct, and nitrogen was introduced for protection. The mixture was stirred at 28° C. and a stirring rate of 350 r / min for 12 min, and then the mixture was heated to 62° C. and stirred for 22 h. After the reaction, the reaction product was cooled to room temperature and then centrifuged. The precipitate was placed in a vacuum drying oven and dried at 72° C. for 2.5 h to obtain mercapto graphene;
[0057] Step T7: 35 g of corrosion-resistant material, 3 g of mercapto graphene, 5 g of triethylamine and 65 g of N,N-dimethylformamide were added to a three-necked flask equipped with a stirrer and a thermometer, and stirred for reaction at a temperature of 48° C. and a stirring rate of 350 r / min for 2.5 h to obtain a corrosion-resistant coating;
[0058] Step T8: Weigh 5.8 parts of silicon powder, 14.7 parts of nickel powder, 18.3 parts of chromium powder, 1.2 parts of manganese powder, 0.4 parts of molybdenum powder, 5 parts of aluminum powder, 2 parts of titanium powder and 49 parts of iron powder according to weight parts, and set aside;
[0059] Step T9: mixing silicon powder, nickel powder, chromium powder, manganese powder, molybdenum powder, aluminum powder, titanium powder and iron powder uniformly and vacuum drying to obtain high silicon ultra-low carbon powder;
[0060] Step T10: rolling a low-carbon steel strip with a width of 10 mm and a thickness of 0.3 mm into a U-shape, adding high-silicon ultra-low carbon powder with a filling amount of 30%, then sealing and rolling into an O-shape, and then drawing to make a flux-cored welding wire;
[0061] Step T11: Spray the corrosion-resistant coating onto the surface of the flux-cored welding wire, solidify it to form a corrosion-resistant coating, and then dry it at a temperature of 90° C. to obtain a high-silicon ultra-low carbon nitric acid-resistant stainless steel flux-cored welding wire.
[0062] Embodiment 3:
[0063] This embodiment is a high-silicon ultra-low carbon nitric acid-resistant stainless steel flux-cored welding wire, which is prepared by the following steps:
[0064] Step T1: 10 mmol of pentaerythritol, 50 mmol of sodium hydroxide and 60 mL of anhydrous tetrahydrofuran are added to a four-necked flask equipped with a stirrer, a thermometer, a gas guide tube, a constant pressure dropping funnel and a reflux condenser, and nitrogen is introduced for protection. The mixture is stirred for reaction at a temperature of 30° C. and a stirring rate of 400 r / min for 15 min, and then 45 mmol of propylene bromide is added dropwise while stirring, and the dropping rate is controlled to be 2 drops / s. After the dropwise addition is completed, the temperature is raised to reflux and the stirring reaction is continued for 5 h. After the reaction is completed, the reaction product is cooled to room temperature, and then washed with saturated brine and distilled water for 3 times in sequence, and then dried with anhydrous sodium sulfate, and then vacuum filtered, and the filtrate is rotary evaporated to remove the solvent to obtain an intermediate product A;
[0065] Step T2: 10 mmol of pentafluoro-1-butanol, 13 mmol of mercaptopropionic acid, 0.09 g of p-toluenesulfonic acid and 50 mL of toluene were added to a three-necked flask equipped with a stirrer, a thermometer and a gas guide tube, and stirred for reaction at a temperature of 30° C. and a stirring rate of 400 r / min for 30 min, then heated to 95° C. and continued to stir for reaction for 8 h. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation to obtain an intermediate product B;
[0066] Step T3: 10 mmol of intermediate product A, 35 mmol of intermediate product B, 40 mmol of triethylamine and 80 mL of dichloromethane were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and nitrogen was introduced for protection. The reaction was stirred for 30 minutes at a temperature of 30°C and a stirring rate of 400 r / min, and then the temperature was raised to reflux and the stirring reaction was continued for 3 hours. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered, and the filtrate was rotary evaporated to remove the solvent to obtain a corrosion-resistant material;
[0067] Step T4: 5 g of graphite powder and 1.8 g of sodium nitrate were added to a three-necked flask equipped with a stirrer and a thermometer, and stirred for 30 min at a temperature of 5 ° C and a stirring rate of 400 r / min, and then 35 mL of 98% concentrated sulfuric acid was added while stirring. After the addition was completed, the stirring reaction continued for 30 min, and then 16 g of potassium permanganate was added and the stirring reaction continued for 30 min. Then, 120 mL of deionized water was added and the temperature was raised to 95 ° C and the stirring reaction continued for 4 h. After the reaction was completed, the reaction product was poured into a 25% hydrogen peroxide solution, and then allowed to stand and precipitate, and then vacuum filtered. The filter cake was washed 5 times with a 20% hydrochloric acid solution and distilled water in turn, and then placed in a vacuum drying oven and dried at a temperature of 75 ° C for 3 h to obtain graphene oxide;
[0068] Step T5: 1 g of graphene oxide, 15 mL of N,N-dimethylformamide and 40 mL of thionyl chloride were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and nitrogen was introduced for protection. The reaction was stirred for 15 min at a temperature of 30° C. and a stirring rate of 400 r / min, and then the temperature was raised to reflux and the stirring reaction was continued for 15 h. After the reaction was completed, the reaction product was cooled to room temperature and then centrifuged. The precipitate was placed in a vacuum drying oven and dried at a temperature of 75° C. for 3 h to obtain graphene chloride;
[0069] Step T6: 1 g of acyl chloride graphene and 35 mL of 2-mercaptoethanol were added to a three-necked flask equipped with a stirrer, a thermometer and a gas duct, and nitrogen was introduced for protection. The reaction was stirred at a temperature of 30° C. and a stirring rate of 400 r / min for 15 min, and then the temperature was raised to 65° C. and the stirring reaction was continued for 25 h. After the reaction was completed, the reaction product was cooled to room temperature and then centrifuged. The precipitate was placed in a vacuum drying oven and dried at a temperature of 75° C. for 3 h to obtain mercapto graphene;
[0070] Step T7: 40 g of corrosion-resistant material, 5 g of mercapto graphene, 8 g of triethylamine and 70 g of N,N-dimethylformamide were added to a three-necked flask equipped with a stirrer and a thermometer, and stirred for reaction at a temperature of 50° C. and a stirring rate of 400 r / min for 3 h to obtain a corrosion-resistant coating;
[0071] Step T8: Weigh 6.8 parts of silicon powder, 15.6 parts of nickel powder, 19.5 parts of chromium powder, 1.6 parts of manganese powder, 0.5 parts of molybdenum powder, 7 parts of aluminum powder, 3 parts of titanium powder and 56 parts of iron powder according to weight parts, and set aside;
[0072] Step T9: mixing silicon powder, nickel powder, chromium powder, manganese powder, molybdenum powder, aluminum powder, titanium powder and iron powder uniformly and vacuum drying to obtain high silicon ultra-low carbon powder;
[0073] Step T10: rolling a low-carbon steel strip with a width of 10 mm and a thickness of 0.3 mm into a U-shape, adding high-silicon ultra-low carbon powder with a filling amount of 30%, then sealing and rolling into an O-shape, and then drawing to make a flux-cored welding wire;
[0074] Step T11: Spray the corrosion-resistant coating onto the surface of the flux-cored welding wire, solidify it to form a corrosion-resistant coating, and then dry it at a temperature of 100° C. to obtain a high-silicon ultra-low carbon nitric acid-resistant stainless steel flux-cored welding wire.
[0075] Comparative Example 1:
[0076] This comparative example is a high-silicon ultra-low carbon nitric acid-resistant stainless steel flux-cored welding wire, which is prepared by the following steps:
[0077] Step T1: Weigh 6.8 parts of silicon powder, 15.6 parts of nickel powder, 19.5 parts of chromium powder, 1.6 parts of manganese powder, 0.5 parts of molybdenum powder, 7 parts of aluminum powder, 3 parts of titanium powder and 56 parts of iron powder according to weight parts, and set aside;
[0078] Step T2: mixing silicon powder, nickel powder, chromium powder, manganese powder, molybdenum powder, aluminum powder, titanium powder and iron powder uniformly and vacuum drying to obtain high silicon ultra-low carbon powder;
[0079] Step T3: Roll a low-carbon steel strip with a width of 10 mm and a thickness of 0.3 mm into a U-shape, add high-silicon ultra-low carbon powder with a filling amount of 30%, then seal and roll it into an O-shape, and then draw it to obtain a high-silicon ultra-low carbon nitric acid-resistant stainless steel flux-cored welding wire.
[0080] Comparative Example 2:
[0081] This comparative example is a high-silicon ultra-low carbon nitric acid-resistant stainless steel flux-cored welding wire, which is prepared by the following steps:
[0082] Step T1: 10 mmol of pentaerythritol, 50 mmol of sodium hydroxide and 60 mL of anhydrous tetrahydrofuran are added to a four-necked flask equipped with a stirrer, a thermometer, a gas guide tube, a constant pressure dropping funnel and a reflux condenser, and nitrogen is introduced for protection. The mixture is stirred for reaction at a temperature of 30° C. and a stirring rate of 400 r / min for 15 min, and then 45 mmol of propylene bromide is added dropwise while stirring, and the dropping rate is controlled to be 2 drops / s. After the dropwise addition is completed, the temperature is raised to reflux and the stirring reaction is continued for 5 h. After the reaction is completed, the reaction product is cooled to room temperature, and then washed with saturated brine and distilled water for 3 times in sequence, and then dried with anhydrous sodium sulfate, and then vacuum filtered, and the filtrate is rotary evaporated to remove the solvent to obtain an intermediate product A;
[0083] Step T2: 10 mmol of pentafluoro-1-butanol, 13 mmol of mercaptopropionic acid, 0.09 g of p-toluenesulfonic acid and 50 mL of toluene were added to a three-necked flask equipped with a stirrer, a thermometer and a gas guide tube, and stirred for reaction at a temperature of 30° C. and a stirring rate of 400 r / min for 30 min, then heated to 95° C. and continued to stir for reaction for 8 h. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation to obtain an intermediate product B;
[0084] Step T3: 10 mmol of intermediate product A, 35 mmol of intermediate product B, 40 mmol of triethylamine and 80 mL of dichloromethane were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and nitrogen was introduced for protection. The reaction was stirred for 30 minutes at a temperature of 30°C and a stirring rate of 400 r / min, and then the temperature was raised to reflux and the stirring reaction was continued for 3 hours. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered, and the filtrate was rotary evaporated to remove the solvent to obtain a corrosion-resistant material;
[0085] Step T4: 40 g of corrosion-resistant material, 8 g of triethylamine and 70 g of N,N-dimethylformamide were added to a three-necked flask equipped with a stirrer and a thermometer, and stirred for reaction at a temperature of 50° C. and a stirring rate of 400 r / min for 3 h to obtain a corrosion-resistant coating;
[0086] Step T5: Weigh 6.8 parts of silicon powder, 15.6 parts of nickel powder, 19.5 parts of chromium powder, 1.6 parts of manganese powder, 0.5 parts of molybdenum powder, 7 parts of aluminum powder, 3 parts of titanium powder and 56 parts of iron powder according to weight parts, and set aside;
[0087] Step T6: mixing silicon powder, nickel powder, chromium powder, manganese powder, molybdenum powder, aluminum powder, titanium powder and iron powder uniformly and vacuum drying to obtain high silicon ultra-low carbon powder;
[0088] Step T7: rolling a low-carbon steel strip with a width of 10 mm and a thickness of 0.3 mm into a U-shape, adding high-silicon ultra-low carbon powder with a filling amount of 30%, then sealing and rolling into an O-shape, and then drawing to make a flux-cored welding wire;
[0089] Step T8: Spray the corrosion-resistant coating onto the surface of the flux-cored welding wire, solidify it to form a corrosion-resistant coating, and then dry it at a temperature of 100° C. to obtain a high-silicon ultra-low carbon nitric acid-resistant stainless steel flux-cored welding wire.
[0090] The performance of the weld metal of the high silicon ultra-low carbon nitric acid resistant stainless steel flux-cored welding wire of Examples 1-3 and Comparative Examples 1-2 was tested by the following method:
[0091] The corrosion resistance test was carried out in a nitric acid solution with a temperature of 25°C and a mass fraction of 65% and a nitric acid solution with a temperature of 80°C and a mass fraction of 65% respectively;
[0092] The test results are shown in the following table:
[0093]
[0094] Referring to the data in the above table, according to the comparison between Examples 1-3 and Comparative Examples 1-2, it can be known that the high-silicon ultra-low carbon nitric acid-resistant stainless steel flux-cored welding wire of the present invention has excellent nitric acid resistance.
[0095] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0096] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A high silicon ultra-low carbon nitric acid resistant stainless steel flux-cored welding wire, characterized in that: Prepared by the following steps: Step 1: Weigh 4.8-6.8 parts of silicon powder, 13.8-15.6 parts of nickel powder, 17.1-19.5 parts of chromium powder, 0.8-1.6 parts of manganese powder, 0.3-0.5 parts of molybdenum powder, 3-7 parts of aluminum powder, 1-3 parts of titanium powder and 42-56 parts of iron powder according to weight parts, and set aside; Step 2: Evenly mix silicon powder, nickel powder, chromium powder, manganese powder, molybdenum powder, aluminum powder, titanium powder and iron powder and vacuum dry them to obtain high silicon ultra-low carbon powder; Step 3: Roll a low-carbon steel strip with a width of 10 mm and a thickness of 0.3 mm into a U-shape, add high-silicon ultra-low carbon powder with a filling amount of 30%, then seal and roll it into an O-shape, and then draw it to make a flux-cored welding wire; Step 4: Spray the corrosion-resistant coating on the surface of the flux-cored welding wire, solidify it to form a corrosion-resistant coating, and then dry it at a temperature of 80-100°C to obtain a high-silicon ultra-low carbon nitric acid-resistant stainless steel flux-cored welding wire; Wherein, the corrosion-resistant coating is prepared by the following steps: Step s1: stirring pentaerythritol, sodium hydroxide and anhydrous tetrahydrofuran for reaction, then adding propylene bromide dropwise while stirring, and continuing to stir the reaction after the addition is complete. After the reaction is completed, the reaction product is cooled, washed, dried, and then vacuum filtered, and the filtrate is rotary evaporated to obtain an intermediate product A; Step s2: stirring pentafluoro-1-butanol, mercaptopropionic acid, p-toluenesulfonic acid and toluene for reaction, cooling the reaction product after the reaction is completed, and then rotary evaporating to obtain an intermediate product B; Step s3: stirring the intermediate product A, the intermediate product B, triethylamine and dichloromethane for reaction, cooling the reaction product after the reaction is completed, and then vacuum filtering, and rotary evaporating the filtrate to obtain a corrosion-resistant material; Step s4: stirring the graphite powder and sodium nitrate for reaction, then adding concentrated sulfuric acid, potassium permanganate and deionized water and continuing stirring the reaction, and after the reaction is completed, pouring the reaction product into a hydrogen peroxide solution, and then standing to precipitate, and then vacuum filtering, washing and drying the filter cake to obtain graphene oxide; Step s5: stirring graphene oxide, N,N-dimethylformamide and dithionyl chloride for reaction, cooling the reaction product after the reaction is completed, then centrifuging and drying the precipitate to obtain chlorinated graphene; Step s6: stirring the chlorinated graphene and 2-mercaptoethanol to react, cooling the reaction product after the reaction is completed, then centrifuging, and drying the precipitate to obtain mercapto graphene; Step s7: stirring and reacting the corrosion-resistant material, mercapto graphene, triethylamine and N,N-dimethylformamide to obtain a corrosion-resistant coating.
2. The high silicon ultra-low carbon nitric acid resistant stainless steel flux-cored welding wire according to claim 1, characterized in that: The usage ratio of the pentaerythritol, sodium hydroxide, anhydrous tetrahydrofuran and propylene bromide in step s1 is 10 mmol: 45-50 mmol: 50-60 mL: 40-45 mmol.
3. The high silicon ultra-low carbon nitric acid resistant stainless steel flux-cored welding wire according to claim 1, characterized in that: The usage ratio of pentafluoro-1-butanol, mercaptopropionic acid, p-toluenesulfonic acid and toluene in step s2 is 10 mmol: 11-13 mmol: 0.05-0.09 g: 40-50 mL.
4. The high silicon ultra-low carbon nitric acid resistant stainless steel flux-cored welding wire according to claim 1, characterized in that: The usage ratio of the intermediate product A, the intermediate product B, triethylamine and dichloromethane in step s3 is 10mmol:20-35mmol:35-40mmol:70-80mL.
5. The high silicon ultra-low carbon nitric acid resistant stainless steel flux-cored welding wire according to claim 1, characterized in that: The usage ratio of the graphite powder, sodium nitrate, concentrated sulfuric acid, potassium permanganate and deionized water in step s4 is 5g:1.2-1.8g:30-35mL:12-16g:100-120mL.
6. The high silicon ultra-low carbon nitric acid resistant stainless steel flux-cored welding wire according to claim 1, characterized in that: The mass fraction of the concentrated sulfuric acid in step s4 is 96-98%, and the mass fraction of the hydrogen peroxide solution is 20-25%.
7. The high silicon ultra-low carbon nitric acid resistant stainless steel flux-cored welding wire according to claim 1, characterized in that: The usage ratio of the graphene oxide, N,N-dimethylformamide and thionyl chloride in step s5 is 1 g: 10-15 mL: 35-40 mL.
8. The high silicon ultra-low carbon nitric acid resistant stainless steel flux-cored welding wire according to claim 1, characterized in that: The usage ratio of the acyl chloride graphene and 2-mercaptoethanol in step s6 is 1 g: 30-35 mL.
9. The high silicon ultra-low carbon nitric acid resistant stainless steel flux-cored welding wire according to claim 1, characterized in that: The usage ratio of the corrosion-resistant material, mercapto graphene, triethylamine and N,N-dimethylformamide in step s7 is 30-40g: 1-5g: 2-8g: 60-70g.