Composite material pressure-resistant shell of ratchet metal end frame and forming method thereof

Through ratchet metal end frame and fiber winding technology, combined with liquid rubber sealant, the compression, tensile, bending strength and sealing problems of the connection between the composite pressure-resistant shell and the metal flange are solved, and the complex service is achieved High reliability connection in the environment overcomes the shortcomings of bonding connections and has wide promotion and application value.

CN118596631BActive Publication Date: 2024-11-08BEIJING COMPOSITE MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411080868.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-08
Estimated Expiration
2044-08-08

AI Technical Summary

Technical Problem

The existing composite pressure-resistant shell and metal flange connection structure have problems such as seal failure, pressure-resistant structure failure, and insufficient tensile and bending moment loading capabilities, especially in multiple operating conditions, it is difficult to meet the complex service environment requirements.

Method used

The composite material pressure-resistant shell forming method using ratchet metal end frame, and the high-strength tensile load and sealing structure are achieved by setting an annular step and ratchet on the metal end frame, combined with fiber winding technology and liquid rubber sealant. Integrated forming of

Benefits of technology

The compressive, tensile and bending strength of the composite compressive shell is improved, and the compression strength and adaptability of the sealing structure is ensured, and the bonding connection cannot meet the fatigue of high tensile strength and alternating load resistance. Enhanced the reliability and application value of underwater equipment pressure-resistant shells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118596631B_ABST
    Figure CN118596631B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of composite materials, and in particular to a composite pressure-resistant shell of a ratchet metal end frame and a molding method thereof. The molding method comprises the following steps: preparing two metal end frames arranged opposite to each other, and installing the two metal end frames on a core shaft at intervals; winding fibers in an alternating manner of circumferential winding and ratchet oblique winding; first curing and molding to obtain a preform of a pressure-resistant shell of the ratchet metal end frame; machining to form an inverted trapezoidal groove at the connection between the metal end frame and the composite shell; coating rubber in the inverted trapezoidal groove; second curing and molding to coat a waterproof coating on the outer surface of each metal end frame and the composite shell to obtain a composite pressure-resistant shell of the ratchet metal end frame; the present invention well solves the technical difficulties of the compressive, tensile and bending strength problems and the sealing problems of the connection between the composite pressure-resistant shell and the metal flange, making the connection of the pressure-resistant shell port more reliable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite pressure-resistant shells, and in particular relates to a composite pressure-resistant shell of a ratchet-type metal end frame and a molding method thereof. Background Art

[0002] Since the advent of composite materials, their excellent performance has been favored by various industries and has been widely used in national defense, military, aerospace, information technology, energy engineering, shipbuilding and marine engineering and other fields; compared with traditional materials, composite materials have the advantages of light weight, high specific strength, high specific stiffness, good corrosion resistance and fatigue resistance, and layer designability.

[0003] Composite ships are one of the most important applications of composite materials in the field of shipbuilding and marine engineering. Compared with steel materials, their advantages are: light weight, high specific strength, good impact strength; good fatigue resistance; non-magnetic, can achieve good stealth function, can effectively avoid a variety of strike equipment; good corrosion resistance, can extend the life, resist the attachment of marine organisms, and reduce maintenance; can be made according to the required performance; multiple surface processing; in addition, there are a series of advantages such as excellent acoustic / dielectric properties, high temperature resistance, shock absorption, etc.; therefore, composite materials are widely used in underwater equipment.

[0004] With the wide application of composite pressure hulls, the connection structure design between the composite main hull and the metal flange is a very critical and important link. After years of rapid development in the field of composite materials, the composite hull itself now has good design capabilities and the realization of pressure resistance, anti-seepage and other functions. However, with the continuous improvement of technical parameters such as the water depth of the pressure hull application, the size of the hull, and the subsequent working environment, higher performance and reliability requirements are put forward for the connection structure of the composite hull. At present, the composite hull is connected with the metal flange to form a pressure hull of a separate compartment, and then the metal flange is used to connect with other compartments. This is a more reasonable form, but in the design process of the pressure hull and the metal flange, a series of problems such as sealing failure and pressure structure failure usually occur; further, with the continuous expansion of the application field of the pressure hull, the pressure hull bearing requirements have gradually evolved from a single water external pressure environment to a service environment that requires multiple working conditions in parallel, and the pressure hull connection structure requirements have changed from the original high compression bearing capacity to the ability to withstand axial tension, large bending moment loads and other complex working conditions.

[0005] For example, Chinese patent CN217179398U discloses a carbon fiber composite material launch tube, which includes a carbon fiber composite material barrel body, a metal end frame with grooves, and a metal embedded part embedded in the barrel body reinforcement ribs. The composite material body includes, from the inside to the outside, an ablation-resistant layer, a first flame retardant layer, a second flame retardant layer, a third flame retardant layer, an electromagnetic shielding layer inside the third flame retardant layer, and a local annular reinforcement rib layer, and the surface of the metal part in contact with the carbon fiber is provided with an insulating layer for isolating galvanic corrosion; the patent uses a metal end frame with grooves, the grooves of which can form a mechanical bite, so that the composite material and the metal end frame form a mechanical connection structure, which is suitable for the prepreg laying process, but cannot be normally applied to the fiber winding molding process; at the same time, due to the large number of folded angles in the grooves, the prepreg fiber fabric will have wrinkles during the laying process, resulting in a decrease in structural performance;

[0006] For example, Chinese patent CN202158099 U discloses a connection structure between a metal flange and a carbon fiber composite material drive shaft, wherein the metal flange is inserted into the composite material drive shaft, and the connection surface between the metal flange and the composite material drive shaft is a polished surface, which is covered with glass fiber, an epoxy resin bonding layer is provided between the glass fiber and the inner surface of the drive shaft, and a bolt reinforcement is also provided between the metal flange and the drive shaft; the purpose of the patent is to provide a connection structure between a metal flange and a carbon fiber composite material drive shaft, which is simple in method, easy to operate, low in cost, high in strength, and easy to implement in production; however, the disadvantages are very obvious, the composite material is a defect-sensitive material, and the concentrated stress caused by the opening position will cause local damage caused by stress concentration when bearing, and these damages will further expand as the service life of the product increases, thereby reducing the reliability of the product; at the same time, opening the hole after the composite material and the metal flange are bonded will cause the adhesive on the bonding surface to debond, while opening the hole before bonding will make it difficult to accurately position, resulting in interference between the bonding surface positioning and the pin hole positioning, causing the thickness of the bonding surface adhesive to be out of control, or the pin cannot be installed.

[0007] For example, Chinese patent CN106545566A discloses a composite material transmission shaft and a molding process of the composite material transmission shaft. The composite material transmission shaft includes: a hard foam tube, two metal flanges fixedly sleeved at both ends of the axial direction of the hard foam tube, and a composite material shaft tube. The composite material shaft tube is formed by winding the impregnated fiber around the metal flange and the outer peripheral wall of the hard foam tube and curing by heating; the structure can realize large-angle unidirectional winding molding. Except for the circumferential winding (90°), which is a unidirectional laying of a complete layer, such as the large angle 80, all are reciprocating laying, that is, ±80° cross-realized. The detailed explanation is that after a yarn width of ±80° is completed, it will be followed by a reverse -80° as a cycle, and after several cycles, the entire mold surface is covered. The thread structure of the invention can realize mechanical engagement with the large-angle laying in one direction, but cannot be effectively engaged in the reverse direction, and an overhead phenomenon will be formed above the thread, reducing the connection strength. The winding angle is limited by the thread angle, and only the large-angle laying can be wound, which can improve the strength of the connection structure under the torque load environment to a certain extent, but the tensile load is not greatly improved.

[0008] Therefore, in view of the above problems, the present invention urgently needs to provide a composite pressure-resistant shell of a ratchet-type metal end frame and a molding method thereof. Summary of the invention

[0009] The present invention provides a composite pressure-resistant shell with a ratchet-type metal end frame and a molding method thereof, and specifically relates to an integrated molding preparation method for a metal end frame connection structure resistant to high-strength tensile loads of a composite pressure-resistant shell for underwater equipment, which can be widely used in the fields of aerospace, weapons and ships.

[0010] The present invention provides a method for forming a composite pressure-resistant shell of a ratchet-type metal end frame, comprising the following steps:

[0011] 1) preparing two metal end frames arranged opposite to each other, wherein the inner end surface of each metal end frame has at least one layer of protruding annular steps, and the side surface of each layer of annular steps is also provided with at least one row of ratchet teeth at intervals in the circumferential direction; and fitting the two metal end frames onto the two ends of the mandrel;

[0012] 2) Using a fiber hoop mandrel, when the fiber winding height is equal to the height of the first annular step close to the mandrel, stop the hoop winding to obtain the first fiber layer;

[0013] 3) If the ratchet teeth are in one row, the ratchet teeth of the two metal end frames are wound with fibers, and the fibers are wound between two relatively offset ratchet teeth in turn. After winding to a first set height, the fibers are wound circumferentially to fill the gap between the ratchet teeth and the inner end surface, until the circumferential winding height is equal to the first set height, and the above process is repeated until the winding height is equal to the ratchet height, thereby obtaining a second fiber layer; if the ratchet teeth are in two rows or more, the ratchet teeth of the two metal end frames are wound with fibers, and the fibers are wound between two relatively offset ratchet teeth in turn. After winding to a first set height, the fibers are wound circumferentially to fill the gap between the ratchet teeth and the inner end surface and the gap between two adjacent rows of ratchet teeth on the same metal end frame, until the circumferential winding height is equal to the first set height, and the above process is repeated until the winding height is equal to the ratchet height, thereby obtaining a second fiber layer;

[0014] 4) If the annular step is one layer, the fiber annular winding is continued on the second fiber layer to obtain the third fiber layer, and the outer end surface of the third fiber layer is flush with the outer wall of the metal end frame; if the annular step is two or more layers, it includes the first annular step and the second annular step from the inside to the outside, and the fiber annular winding is continued on the second fiber layer to obtain the third fiber layer, so that the outer end surface of the third fiber layer is flush with the outer wall of the second annular step; repeat step 3 until the height of the fiber winding is equal to the height of the outer wall of the metal end frame, and stop winding;

[0015] 5) First curing and molding to obtain a composite shell and a pressure-resistant shell preform of a ratchet-type metal end frame;

[0016] 6) Machining the pressure hull preform to form an inverted trapezoidal groove that is wide outside and narrow inside at the connection between each metal end frame and the composite shell; applying rubber in the inverted trapezoidal groove, and performing a second curing molding to form a pressure hull preform with a ratchet-type metal end frame having a sealing ring;

[0017] 7) Apply a waterproof coating on the outer surface of each metal end frame and the composite shell, demould, and obtain a composite pressure-resistant shell of the ratchet metal end frame.

[0018] Preferably, the distance a between each row of ratchet teeth satisfies the following formula: a=D / (cosθ*sinθ), wherein D is the width of the fiber, and θ is the angle between the fiber and the busbars of each metal end frame; the distance b between each row of ratchet teeth satisfies the following formula: b=n*D / cosθ, wherein D is the width of the fiber, θ is the angle between the fiber and the busbars of each metal end frame, and n is the number of rows of ratchet teeth.

[0019] Preferably, coating rubber in the inverted trapezoidal groove comprises the following steps:

[0020] 1) Use liquid rubber to fully impregnate the reinforcement fibers;

[0021] 2) Apply the first layer of rubber in the inverted trapezoidal groove;

[0022] 3) Winding the fully impregnated reinforcement fibers into the inverted trapezoidal grooves;

[0023] 4) Continue to apply a second layer of rubber in the inverted trapezoidal groove, so that the outer surface of the second layer of rubber is highly consistent with the outer surfaces of each metal end frame and the composite shell.

[0024] Preferably, the first set height is 0.2 mm.

[0025] Preferably, the diameter of each ratchet tooth is 1 / 3 to 1 / 4 of the fiber width.

[0026] Preferably, the distance x0 between the plane where the annular step is located and the plane where the outer side wall of the metal end frame is located satisfies the following formula: D≤x0≤1.5D, wherein D is the width of the fiber.

[0027] Preferably, the waterproof coating is a chloroprene rubber paint layer or a polyurea coating.

[0028] The present invention also provides a composite pressure-resistant shell of a ratchet metal end frame obtained according to the above-mentioned composite pressure-resistant shell molding method of a ratchet metal end frame, comprising a composite shell, and metal end frames are connected to both ends of the composite shell;

[0029] The inner end surface of each metal end frame is also provided with at least one layer of protruding annular steps, and the side surface of each layer of annular steps is also provided with at least one row of ratchet teeth spaced circumferentially;

[0030] The connection between each metal end frame and the composite shell is sealed by a sealing structure.

[0031] Preferably, the sealing structure comprises a first sealing groove annularly arranged at the connection between the inner end surface of each metal end frame and the outer surface of the metal end frame;

[0032] A second sealing groove is circumferentially arranged at the connection between the outer end surface of the composite shell matched with the inner end surface of each metal end frame and the outer surface of the composite shell;

[0033] The first sealing groove and the second sealing groove are arranged to form a sealing groove with a cross section of an inverted trapezoidal shape that is wide outside and narrow inside;

[0034] It also includes a sealing ring which is tightly mounted in the sealing groove.

[0035] Preferably, each metal end frame and the outer surface of the composite shell are also provided with a waterproof coating, and the waterproof coating is a chloroprene rubber paint layer or a polyurea coating.

[0036] Compared with the prior art, the present invention has the following beneficial effects:

[0037] 1) The composite pressure-resistant shell of the ratchet metal end frame provided by the present invention and its molding method, metal end frames are placed at both ends of the mold, and the metal end frames are arranged with a ratchet-shaped fixed structure for positioning small-angle winding. After the metal end frames are fixed, wet winding molding of the composite material is performed, and after molding, curing is performed, the outer surface is processed according to the drawing, and a V-groove is processed at the contact position between the metal end frame and the composite shell, and a sealant is used for sealing. After the sealing is completed, the carbon fiber pressure-resistant shell and the metal end frame are encapsulated with a hydrophobic coating; in terms of molding, the present invention solves the accumulation phenomenon caused by small-angle winding at the angle alternation by designing the ratchet size and multi-layer arrangement, and no longer relies on manual laying of unidirectional reinforced fabrics to solve the problem. Axial laying; stepped multi-layer ratchet, which effectively solves the problem that the pressure hull needs to be wound at a small angle within the specified thickness range. The process is easy to implement, has high feasibility, and high fiber utilization rate, ensuring the consistency of structural design and molding performance. In terms of sealing, the present invention improves the compression strength of the sealing structure by combining liquid rubber sealant with reinforcement. It has good adaptability to different service environments such as compression, tension, bending conditions and alternating pressure, and the process is easy to implement. At the same time, the present invention has good adaptability to composite pressure hulls of different wall thicknesses. At the same time, the metal flange can realize the connection design with other compartments, with a large degree of design freedom, suitable for secondary development, and has a wide range of promotion and application value.

[0038] 2) The present invention solves the technical problems of compressive, tensile and bending strength and sealing problems of the connection between the composite pressure hull and the metal flange, making the connection of the pressure hull port more reliable and overcoming the problem that the adhesive connection cannot simultaneously meet the requirements of high tensile strength and resistance to alternating load fatigue. It has high application value and promotion significance in the promotion and application of composite materials for pressure hulls of underwater equipment. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 It is a structural schematic diagram (cross-sectional view) of a composite material pressure-resistant casing of a ratchet-type metal end frame according to an embodiment of the present invention;

[0040] Figure 2 yes Figure 1 The enlarged view of point A in the middle;

[0041] Figure 3 1 is a schematic structural diagram (front view) of a metal end frame with a double-layer annular step with double rows of ratchets according to an embodiment of the present invention;

[0042] Figure 4 It is a structural schematic diagram (cross-sectional view) of a metal end frame with a double-layer annular step with double rows of ratchets according to an embodiment of the present invention;

[0043] Figure 51 is a schematic structural diagram (front view) of a metal end frame having a layer of annular steps with a row of ratchets according to an embodiment of the present invention;

[0044] Figure 6 1 is a schematic structural diagram (cross-sectional view) of a metal end frame having a layer of annular steps with a row of ratchets according to an embodiment of the present invention;

[0045] Figure 7 It is a flow chart of a method for preparing a composite pressure-resistant shell of a ratchet-type metal end frame according to an embodiment of the present invention;

[0046] Figure 8 yes Figure 2 Structural diagram of the middle ratchet metal end frame (section view);

[0047] Fig. 9 yes Figure 2 Schematic diagram of the structure of the composite shell (cross-sectional view).

[0048] Wherein: 1. composite shell; 101. outer end face; 102. second sealing groove; 2. metal end frame; 201. annular step; 202. ratchet; 203. inner end face; 204. first sealing groove; 3. sealing ring; 4. core shaft. DETAILED DESCRIPTION

[0049] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solution of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0050] like Figure 1 , Figure 2 , Figure 3 , Figure 4 , Figure 5 , Figure 6 , Figure 7 , Figure 8 , Fig. 9 As shown, a method for forming a composite pressure-resistant shell of a ratchet-type metal end frame comprises the following steps:

[0051] 1) preparing two metal end frames 2 arranged opposite to each other, wherein the inner end surface 203 of each metal end frame 2 has at least one layer of protruding annular steps 201, and the side surface of each layer of annular steps 201 is also provided with at least one row of ratchet teeth 202 at intervals in the circumferential direction; and putting the two metal end frames 2 on both ends of the core shaft 4;

[0052] 2) Using the fiber hoop mandrel 4, when the fiber winding height is equal to the height of the first annular step 201 close to the mandrel, the hoop winding is stopped to obtain the first fiber layer;

[0053] 3) If the ratchet teeth 202 are in one row, fibers are wound around the ratchet teeth 202 of the two metal end frames 2, and the fibers are wound between the two relatively offset ratchet teeth 202 in turn. After winding to the first set height, fibers are wound circumferentially to fill the gap between the ratchet teeth 202 and the inner end surface 203, until the circumferential winding height is equal to the first set height, and the above process is repeated until the winding height is equal to the height of the ratchet teeth 202, and a second fiber layer is obtained; if the ratchet teeth 202 are in two or more rows, fibers are wound around the ratchet teeth 202 of the two metal end frames 2, and the fibers are wound between the two relatively offset ratchet teeth 202 in turn. After winding to the first set height, fibers are wound circumferentially to fill the gap between the ratchet teeth and the inner end surface 203 and the gap between two adjacent rows of ratchet teeth 202 on the same metal end frame 2, until the circumferential winding height is equal to the first set height, and the above process is repeated until the winding height is equal to the height of the ratchet teeth 202, and a second fiber layer is obtained;

[0054] 4) If the annular step 201 is a single layer, the fiber annular winding is continued on the second fiber layer to obtain a third fiber layer, and the outer end surface of the third fiber layer is flush with the outer wall of the metal end frame 2; if the annular step 201 is two or more layers, it includes the first annular step and the second annular step from the inside to the outside, and the fiber annular winding is continued on the second fiber layer to obtain a third fiber layer, so that the outer end surface of the third fiber layer is flush with the outer wall of the second annular step; repeat step 3 until the height of the fiber winding is equal to the height of the outer wall of the metal end frame 2, and stop winding;

[0055] 5) First curing and molding to obtain a composite shell 1 and a pressure-resistant shell preform of a ratchet-type metal end frame;

[0056] 6) Machining the pressure hull preform to form an inverted trapezoidal groove that is wide outside and narrow inside at the connection between each metal end frame 2 and the composite shell 1; applying rubber in the inverted trapezoidal groove, and performing a second curing molding to form a pressure hull preform of a ratchet-type metal end frame with a sealing ring 3;

[0057] 7) A waterproof coating is applied to the outer surface of each metal end frame 2 and the composite shell 1, and the mold is removed to obtain a composite pressure-resistant shell of a ratchet metal end frame.

[0058] The composite pressure-resistant shell of the ratchet-type metal end frame provided by the present invention and the molding method thereof, the metal end frame 2 is placed at both ends of the mold, the metal end frame 2 is provided with ratchet teeth 202 for positioning small-angle winding, after the metal end frame 2 is fixed, the ratchet teeth 202 are used to perform wet winding molding of the composite material, and after molding, it is cured, the outer surface is processed according to the drawing, and an inverted trapezoidal groove is processed at the contact position between the metal end frame 2 and the composite shell 1, and a sealant is used for sealing. After the sealing is completed, the carbon fiber pressure-resistant shell and the metal end frame are encapsulated with a hydrophobic coating; in terms of molding, the present invention solves the accumulation phenomenon caused by small-angle winding at the angle alternation by designing the size of the ratchet teeth 202 and arranging the multi-layer ratchet teeth 202, and no longer relies on unidirectional increase The strong fabric is manually laid to solve the axial layering problem; at the same time, the stepped multi-layer ratchet wheel solves the problem that the pressure hull needs to be wound at a small angle within the specified thickness range. The process is easy to implement, has high feasibility, and has a high fiber utilization rate, ensuring the consistency of the structural design and molding performance. In terms of sealing, the present invention improves the compression strength of the sealing structure by combining liquid rubber sealant with a reinforcement. It has good adaptability to different service environments such as compression, tension, bending conditions and alternating pressure, and the process is easy to implement. At the same time, the present invention has good adaptability to composite pressure hulls of different wall thicknesses. At the same time, the metal flange can realize the connection design with other compartments, with a large degree of design freedom, suitable for secondary development, and has a wide range of promotion and application value.

[0059] In summary, the present invention has effectively solved the technical problems of compressive, tensile and bending strength and sealing problems of the connection between the composite pressure-resistant shell and the metal flange, making the connection of the pressure-resistant shell port more reliable and overcoming the problem that the adhesive connection cannot simultaneously meet the requirements of high tensile strength and resistance to alternating load fatigue. It has high application value and promotion significance in the promotion and application of composite materials for pressure-resistant shells of underwater equipment.

[0060] In this embodiment, the distance a between each row of ratchet teeth 202 satisfies the following formula: a=D / (cosθ*sinθ), wherein D is the width of the fiber, and θ is the angle between the fiber and the busbar of each metal end frame 2; the distance b between each row of ratchet teeth 202 satisfies the following formula: b=n*D / cosθ, wherein D is the width of the fiber, θ is the angle between the fiber and the busbar of each metal end frame 2, and n is the number of rows of ratchet teeth 202.

[0061] In this embodiment, coating rubber in the inverted trapezoidal groove includes the following steps:

[0062] 1) Use liquid rubber to fully impregnate the reinforcement fibers;

[0063] 2) Apply the first layer of rubber in the inverted trapezoidal groove;

[0064] 3) Winding the fully impregnated reinforcement fibers into the inverted trapezoidal grooves;

[0065] 4) Continue to apply a second layer of rubber in the inverted trapezoidal groove, so that the outer surface of the second layer of rubber is highly consistent with the outer surfaces of each metal end frame 2 and the composite shell 1 .

[0066] The integrated molding structure of the composite pressure-resistant shell and the metal end frame involved in the present invention is mainly a connection structure for high-strength loads. Due to the difference in thermal expansion coefficients during the curing process of the composite material, the metal end frame 2 and the composite shell 1 may be debonded, causing the pressure-resistant shell to lack a sealing function; therefore, the sealing structure adopted in the present invention is to process an inverted trapezoidal groove at the position where the metal end frame 2 contacts the outer surface of the composite shell 1, pour hard sealing functional rubber into the groove, and then use reinforcements such as fibers or metal wires to improve the rigidity of the rubber so that its compressive strength is greater than the external water pressure load pressure; by using the idea of ​​combining liquid rubber sealant with reinforcements, the compressive strength of the sealing structure is improved, and it has good adaptability to different service environments such as compression, tension, bending conditions and alternating pressure, and the process is easy to implement.

[0067] In this embodiment, the first set height is 0.2 mm.

[0068] In the present invention, the second fiber layer is divided into several winding layers with a first set height. Each layer is firstly wound around the ratchet teeth 202, and then wound in a ring shape to fill the gaps between each row of ratchet teeth 202. If the first set height is too high, empty layers will appear between each winding layer, affecting the strength of the pressure-resistant shell; if the first set height is too low, unnecessary workload will be caused, extending the preparation cycle.

[0069] In this embodiment, the diameter of each ratchet tooth 202 is 1 / 3 to 1 / 4 of the fiber width.

[0070] In this embodiment, the distance x0 between the plane where the annular step 201 is located and the plane where the outer wall of the metal end frame 2 is located satisfies the following formula: D≤x0≤1.5D, where D is the width of the fiber.

[0071] In this embodiment, the waterproof coating is a chloroprene rubber paint layer or a polyurea coating.

[0072] like Figure 1 , Figure 2 , Figure 3 , Figure 4 , Figure 5 , Figure 6 , Figure 7 , Figure 8 , Fig. 9As shown, the present invention provides a composite pressure-resistant shell of a ratchet metal end frame obtained according to the composite pressure-resistant shell molding method of a ratchet metal end frame as described above, comprising a composite shell 1, and metal end frames 2 are respectively connected to both ends of the composite shell 1;

[0073] The inner end surface 203 of each metal end frame 2 is also provided with at least one layer of protruding annular steps 201, and the side surface of each layer of annular steps 201 is also provided with at least one row of ratchet teeth 202 spaced circumferentially;

[0074] The connection between each metal end frame 2 and the composite shell 1 is sealed by a sealing structure.

[0075] The composite pressure-resistant shell of the ratchet-type metal end frame provided by the present invention and the molding method thereof, the metal end frame 2 is placed at both ends of the mold, the metal end frame 2 is provided with ratchet teeth 202 for positioning small-angle winding, after the metal end frame 2 is fixed, the ratchet teeth 202 are used to perform wet winding molding of the composite material, and after molding, it is cured, the outer surface is processed according to the drawing, and an inverted trapezoidal groove is processed at the contact position between the metal end frame 2 and the composite shell 1, and a sealant is used for sealing. After the sealing is completed, the carbon fiber pressure-resistant shell and the metal end frame are encapsulated with a hydrophobic coating; in terms of molding, the present invention solves the accumulation phenomenon caused by small-angle winding at the angle alternation by designing the size of the ratchet teeth 202 and arranging the multi-layer ratchet teeth 202, and no longer relies on unidirectional increase The strong fabric is manually laid to solve the axial layering problem; at the same time, the stepped multi-layer ratchet wheel solves the problem that the pressure hull needs to be wound at a small angle within the specified thickness range. The process is easy to implement, has high feasibility, and has a high fiber utilization rate, ensuring the consistency of the structural design and molding performance. In terms of sealing, the present invention improves the compression strength of the sealing structure by combining liquid rubber sealant with a reinforcement. It has good adaptability to different service environments such as compression, tension, bending conditions and alternating pressure, and the process is easy to implement. At the same time, the present invention has good adaptability to composite pressure hulls of different wall thicknesses. At the same time, the metal flange can realize the connection design with other compartments, with a large degree of design freedom, suitable for secondary development, and has a wide range of promotion and application value.

[0076] In summary, the present invention has effectively solved the technical problems of compressive, tensile and bending strength and sealing problems of the connection between the composite pressure-resistant shell and the metal flange, making the connection of the pressure-resistant shell port more reliable and overcoming the problem that the adhesive connection cannot simultaneously meet the requirements of high tensile strength and resistance to alternating load fatigue. It has high application value and promotion significance in the promotion and application of composite materials for pressure-resistant shells of underwater equipment.

[0077] like Figure 8 , Fig. 9As shown, the sealing structure includes a first sealing groove 204 circumferentially arranged at the connection between the inner end surface 203 of each metal end frame 2 and the outer surface of the metal end frame 2;

[0078] A second sealing groove 102 is circumferentially arranged at the connection between the outer end surface 101 of the composite shell 1 matched with the inner end surface 203 of each metal end frame 2 and the outer surface of the composite shell 1;

[0079] The first sealing groove 204 and the second sealing groove 102 are arranged to form a sealing groove with a cross section of an inverted trapezoidal shape that is wide outside and narrow inside.

[0080] It also includes a sealing ring 3 which is tightly mounted in the sealing groove.

[0081] In this embodiment, each metal end frame 2 and the outer surface of the composite shell 1 are further provided with a waterproof coating, and the waterproof coating is a chloroprene rubber paint layer or a polyurea coating.

[0082] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A method for forming a composite pressure-resistant shell of a ratchet metal end frame, characterized in that: The steps include: 1) preparing two metal end frames (2) arranged opposite to each other, wherein the inner end surface (203) of each metal end frame (2) has at least one layer of protruding annular steps (201), and the side surface of each layer of annular steps (201) is also provided with at least one row of ratchet teeth (202) spaced circumferentially; and fitting the two metal end frames (2) onto the two ends of a core shaft (4); 2) Circumferentially winding the fibers around the outer surface of the core shaft (4), and when the height of the fiber winding is equal to the height of the first annular step (201) close to the core shaft (4), the circumferential winding is stopped to obtain a first fiber layer; 3) If the ratchet teeth (202) are in one row, fibers are used to wind the ratchet teeth (202) of the two metal end frames (2), and the fibers are sequentially wound between the two relatively offset ratchet teeth (202). After winding to a first set height, the fibers are used to wind in an annular direction to fill the gap between the ratchet teeth (202) and the inner end surface (203), until the annular winding height is equal to the first set height, and the above process is repeated until the winding height is equal to the height of the ratchet teeth (202), thereby obtaining a second fiber layer; if the ratchet teeth (202) are in two rows or When there are more than two rows, fibers are used to wind the ratchet teeth (202) of the two metal end frames (2), and the fibers are sequentially wound between two relatively offset ratchet teeth (202). After winding to a first set height, the fibers are used to perform circumferential winding to fill the gap between the ratchet teeth and the inner end surface (203) and the gap between two adjacent rows of ratchet teeth (202) on the same metal end frame (2), until the circumferential winding height is equal to the first set height, and the above process is repeated until the winding height is equal to the ratchet teeth (202) height, thereby obtaining a second fiber layer; 4) If the annular step (201) is a single layer, the fiber annular winding is continued on the second fiber layer to obtain a third fiber layer, and the outer end surface of the third fiber layer is flush with the outer wall of the metal end frame (2); if the annular step (201) is a double layer or more, it includes the first annular step and the second annular step in sequence from the inside to the outside, and the fiber annular winding is continued on the second fiber layer to obtain a third fiber layer, so that the outer end surface of the third fiber layer is flush with the outer wall of the second annular step; repeat step 3 until the height of the fiber winding is equal to the height of the outer wall of the metal end frame (2), and stop winding; 5) first curing and molding to obtain a composite shell (1) and a pressure-resistant shell preform of a ratchet-type metal end frame; 6) machining the pressure hull preform to form an inverted trapezoidal groove that is wide outside and narrow inside at the connection between each metal end frame (2) and the composite shell (1); applying rubber in the inverted trapezoidal groove, and performing a second curing molding to form a pressure hull preform with a ratchet-type metal end frame having a sealing ring (3); 7) coating a waterproof coating on the outer surface of each metal end frame (2) and the composite shell (1), demoulding, and obtaining a composite pressure-resistant shell of a ratchet-type metal end frame; The distance a between each row of ratchet teeth (202) satisfies the following formula: a=D / (cosθ*sinθ), wherein D is the width of the fiber, and θ is the angle between the fiber and the busbar of each metal end frame (2); the distance b between each row of ratchet teeth (202) satisfies the following formula: b=n*D / cosθ, wherein D is the width of the fiber, θ is the angle between the fiber and the busbar of each metal end frame (2), and n is the number of rows of ratchet teeth (202).

2. The molding method of the composite material pressure-resistant shell of the ratchet metal end frame according to claim 1, characterized in that: The steps of applying rubber in the inverted trapezoidal groove include: 1) Use liquid rubber to fully impregnate the reinforcement fibers; 2) Applying a first layer of rubber in the inverted trapezoidal groove; 3) Winding the fully impregnated reinforcement fibers into the inverted trapezoidal grooves; 4) Continue to apply a second layer of rubber in the inverted trapezoidal groove, so that the outer surface of the second layer of rubber is highly consistent with the outer surfaces of each metal end frame (2) and the composite shell (1).

3. The molding method of the composite pressure-resistant shell of the ratchet metal end frame according to claim 2, characterized in that: The first set height is 0.2 mm.

4. The method for forming a composite pressure-resistant shell of a ratchet-type metal end frame according to claim 3, characterized in that: The diameter of each ratchet (202) is 1 / 3 to 1 / 4 of the fiber width.

5. The method for forming a composite pressure-resistant shell of a ratchet metal end frame according to claim 4, characterized in that: The distance x0 between the plane where the annular step (201) is located and the plane where the outer wall of the metal end frame (2) is located satisfies the following formula: D≤x0≤1.5D, wherein D is the width of the fiber.

6. The method for forming a composite material pressure-resistant shell of a ratchet metal end frame according to claim 5, characterized in that: The waterproof coating is a paint layer or polyurea coating of chloroprene rubber.

7. A composite pressure-resistant shell of a ratchet metal end frame obtained by the composite pressure-resistant shell molding method of a ratchet metal end frame according to any one of claims 1 to 6, characterized in that: It comprises a composite shell (1), with metal end frames (2) respectively connected to both ends of the composite shell (1); The inner end surface (203) of each metal end frame (2) is also provided with at least one layer of protruding annular steps (201), and the side surface of each layer of annular steps (201) is also provided with at least one row of ratchet teeth (202) spaced apart in the circumferential direction; The connection between each metal end frame (2) and the composite material shell (1) is sealed by a sealing structure.

8. The composite pressure-resistant casing of the ratchet metal end frame according to claim 7, characterized in that: The sealing structure comprises a first sealing groove (204) arranged in an annular direction at the connection between the inner end surface (203) of each metal end frame (2) and the outer surface of the metal end frame (2); A second sealing groove (102) circumferentially arranged at the connection between the outer end surface (101) of the composite shell (1) matched with the inner end surface (203) of each metal end frame (2) and the outer surface of the composite shell (1); The first sealing groove (204) and the second sealing groove (102) are arranged to form a sealing groove having a cross section of an inverted trapezoidal shape with a wide outer side and a narrow inner side; It also includes a sealing ring (3) tightly mounted in the sealing groove.

9. The composite pressure-resistant casing of the ratchet metal end frame according to claim 8, characterized in that: The outer surfaces of each metal end frame (2) and the composite shell (1) are also provided with a waterproof coating, which is a chloroprene rubber paint layer or a polyurea coating.