Inorganic tunnel paint and preparation method thereof

Through the design of inorganic system tunnel paint, the use of phosphate layers and energy-storage luminescent composite materials combined with inorganic polymer layers solves the problems of short service life and environmental pollution of tunnel luminescent materials, achieving high adhesion strength, long afterglow time and environmental protection , improving the safety and light environment in the tunnel.

CN118599348BActive Publication Date: 2024-10-22JILIN JIANZHU UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410848837.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-22
Estimated Expiration
2044-06-27

AI Technical Summary

Technical Problem

Due to the dark and humid environment, existing tunnel luminescent materials have short service life, poor luminous effect, are prone to mold and fall off, are not fire-proof and flame-retardant, and contain volatile harmful substances, polluting the environment and endangering human health.

Method used

Inorganic system tunnel paint is used, including phosphate layer materials, energy storage luminescent composite materials and inorganic polymer layer materials. The paint film is formed through uniform distribution and mixing and curing, which enhances adhesion strength, prolongs afterglow time, improves acid and alkali resistance and Solvent resistance reduces preparation costs, and improves the overall performance of the paint film through the fire retardancy of the phosphate layer and the mechanical properties of the silicate layer.

Benefits of technology

It achieves the high adhesion strength, long afterglow time, good durability and environmental protection of the tunnel paint, reduces environmental pollution and human hazards, reduces maintenance costs, and improves the driving safety and light environment in the tunnel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004916330710000071
    Figure BDA0004916330710000071
  • Figure BDA0004916330710000081
    Figure BDA0004916330710000081
  • Figure BDA0004916330710000091
    Figure BDA0004916330710000091
Patent Text Reader

Abstract

The present invention belongs to the technical field of green and low-carbon building materials, and specifically relates to an inorganic system tunnel paint and a preparation method. The inorganic system tunnel paint comprises a phosphate layer material, an energy storage luminescent composite material and an inorganic polymer layer material; the phosphate layer material, the energy storage luminescent composite material and the inorganic polymer layer material are used by respectively coating and co-curing or by partially mixing and curing in steps; the constituent components of the phosphate layer material include phosphate, an auxiliary agent and a solvent; the constituent components of the inorganic polymer layer material include silicate, a metal oxide and an auxiliary agent. The inorganic tunnel paint of the present invention has good physical and chemical properties and can form fluorescent afterglow.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of green and low-carbon building materials, and specifically relates to an inorganic system tunnel paint and a preparation method thereof. Background Art

[0002] In recent years, with the implementation of the "Strong Transportation Country" strategy, mountain highways have developed rapidly, and the scale of tunnel construction has become larger and larger. China has become the country with the largest scale and the largest number of highway tunnels in the world. By the end of 2022, the total mileage of tunnels in my country will reach 48,762 kilometers, an increase of 3,008.1 kilometers from 2021. Among them, the mileage of highway tunnels accounts for 54.93% of the total mileage of tunnels in the country, and the mileage of railway tunnels accounts for 45.07% of the total mileage of tunnels in the country. While tunnel engineering is developing rapidly, some difficulties have also arisen in the operation of highway tunnels. The main contradiction is the high cost of operation and maintenance of the lighting system. In other words, under the premise of ensuring traffic safety, reducing the energy consumption of tunnel lighting has become a key issue that needs to be solved urgently. Traditional solutions usually focus on the design and improvement of lighting systems, and the introduction of auxiliary lighting technology of tunnel wall luminous materials provides new ideas for the development of tunnel engineering.

[0003] Most tunnel luminous materials on the market choose organic resins or emulsions as film-forming materials. For example, patent CN113214730A provides a water-based energy storage luminous paint with fireproof function for tunnels, including the following components by weight: 30-40 parts of water-based polyurea resin, 10-15 parts of water-based fluorocarbon resin, 10-15 parts of water-based epoxy resin, 15-25 parts of energy storage luminous material, 5-8 parts of flame retardant, 3-4 parts of dispersant, 1-2 parts of leveling agent, 5-8 parts of curing agent, 50-60 parts of water; wherein the energy storage luminous material can improve the stability of the luminous material in the system, improve the luminous intensity, and prolong the afterglow time. The water-based energy storage luminous paint for tunnels provided by the present invention can reduce the brightness difference between the inside and outside of the tunnel, eliminate the black hole and white hole phenomenon in the tunnel, and improve the driving safety in the tunnel. However, volatile organic compounds (VOCs) will be generated during the preparation and use process, which will not only pollute the environment, but also pose a potential threat to human health. At the same time, in dark and humid environments, the paint will become moldy, fall off, and peel off, which seriously reduces the safety of tunnel driving. In order to improve the tunnel light environment, reduce lighting energy consumption, and reduce maintenance costs, it is necessary to develop an environmentally friendly inorganic energy storage luminescent material.

[0004] At present, the luminous materials used in tunnels generally use organic matter as the film-forming substance, which mainly has two problems: first, the tunnel environment is dark, humid and lacks light. Organic luminous materials have problems such as short service life, poor luminous effect, easy mold and fall off, and no fire retardancy in tunnels; second, the film-forming substance of organic luminescent materials contains volatile harmful substances such as formaldehyde, toluene, TVOC, etc., which will pollute the environment. Summary of the invention

[0005] Based on the above content, in order to solve the problems of poor tunnel light environment, high energy consumption of lighting system, high maintenance cost of lighting system, environmental pollution and short service life, the present invention proposes an inorganic system tunnel paint and a preparation method.

[0006] The objects of the present invention are:

[0007] 1. Enhance the adhesion strength of tunnel paint after curing;

[0008] 2. Extend the afterglow time of tunnel paint;

[0009] 3. Enhance the acid, alkali and solvent resistance of tunnel paint and extend its service life;

[0010] 4. Reduce preparation costs.

[0011] To achieve the above objectives, the present invention adopts the following technical solutions.

[0012] An inorganic system tunnel paint,

[0013] The inorganic system tunnel paint comprises a phosphate layer material, an energy storage luminescent composite material and an inorganic polymer layer material;

[0014] The phosphate layer material, the energy storage luminescent composite material and the inorganic polymer layer material are used in a manner of being coated separately and cured together or in a manner of being partially mixed and cured in steps;

[0015] The phosphate layer material comprises phosphate, an additive and a solvent;

[0016] The inorganic polymer layer material comprises components of silicate, metal oxide and auxiliary agent.

[0017] As a preference,

[0018] The tunnel paint is used in any one of the following three ways:

[0019] Method A: Evenly distribute the phosphate layer material, the energy storage luminescent composite material and the inorganic polymer layer material respectively, and wait for drying and curing to form a paint film;

[0020] Method B: Evenly distribute the phosphate layer material, take the energy storage luminescent composite material and the inorganic polymer layer material and mix them evenly, evenly distribute them on the dry phosphate layer, and wait for drying and curing to form a paint film;

[0021] Method C: Take the phosphate layer material and the energy storage luminescent composite material, mix them evenly, distribute them evenly, evenly distribute the inorganic polymer layer material after drying, and dry and solidify to form a paint film.

[0022] A method for preparing an inorganic system tunnel paint,

[0023] The methods respectively include:

[0024] The preparation method of the phosphate layer material comprises: taking phosphate, an auxiliary agent and a solvent and mixing them evenly;

[0025] The preparation method of the energy storage luminescent composite material comprises: mixing aluminate and fluoride evenly, then grinding and sieving, adding a reducing agent and performing microwave sintering;

[0026] The preparation method of the inorganic polymer layer material comprises: dispersing silicate and metal oxide in acid solution, controlling the amount of acid solution to adjust the pH value to a weakly acidic condition, and then adding an auxiliary agent and mixing evenly;

[0027] The phosphate layer material, the energy storage luminescent composite material and the inorganic polymer layer material are prepared and packaged and stored independently.

[0028] As a preference,

[0029] In the preparation method of the phosphate layer material:

[0030] The phosphate is aluminum phosphate and / or zirconium phosphate and / or magnesium phosphate and / or aluminum chromium phosphate;

[0031] The auxiliary agent is a defoamer and / or a dispersant and / or a thickener, and its dosage is 0.01-0.1 mL / g phosphate;

[0032] The solvent is ethanol, and its usage is 1-2 mL / g phosphate.

[0033] As a preference,

[0034] In the preparation method of the inorganic polymer layer material:

[0035] The aluminate is calcium aluminate;

[0036] The fluoride is yttrium fluoride, and its dosage is 0.05-0.1 g / g aluminate;

[0037] The reducing agent is graphene, and the amount used is 0.1-0.2 g / g aluminate.

[0038] As a preference,

[0039] In the preparation method of the inorganic polymer layer material:

[0040] The grinding is to grind the mixed materials to a particle size of 1 to 3 μm;

[0041] The microwave sintering is carried out at a temperature of 1200-1300° C. and a constant temperature of 4-6 hours.

[0042] As a preference,

[0043] In the preparation method of the inorganic polymer layer material:

[0044] The silicate is potassium silicate and / or lithium silicate and / or ammonium silicate;

[0045] The metal oxide is titanium dioxide and / or cuprous oxide and / or zinc oxide and / or tin dioxide and / or aluminum oxide, and its particle size is 1 to 3 μm, and its dosage is 0.2 to 0.4 g / g silicate;

[0046] The acid solution is an aqueous solution of acetic acid, and its concentration is 1 to 3 mol / L;

[0047] The auxiliary agent is dibutyltin dilaurate, and its dosage is 0.05-0.1 mL / g silicate.

[0048] As a preference,

[0049] In the preparation method of the inorganic polymer layer material:

[0050] The pH value of the weakly acidic condition is 4 to 5.5.

[0051] In the technical solution of the present invention, on the one hand, phosphate contains a P=O double bond, provides a pair of free electrons, can form a coupling substance with calcium aluminate, and enhance the binding force between the phosphate layer material and the energy storage luminescent composite material. Among them, the phosphate layer material is the main film-forming material, acting as a skeleton, and the energy storage luminescent composite material is filled in the pores of the phosphate layer, which enhances the compactness of the coating, makes the coating highly hydrophobic, and at the same time, reduces the curing shrinkage of the phosphate layer and improves the mechanical properties of the coating. On the other hand, the bonding between the hydroxyl groups contained in the phosphate layer material and the metal atoms can effectively improve the bonding strength inside the phosphate layer after curing, protect the energy storage luminescent composite material, passivate metal oxides, enhance the corrosion resistance of the tunnel paint to the coated substrate, shield the corrosive medium, and reduce the corrosion current density in the paint film.

[0052] In addition, the phosphate layer is fireproof and flame retardant. When a fire occurs, on the one hand, the phosphate layer is decomposed by heat to form a polyphosphoric acid film and a non-volatile glassy substance, which blocks the heat source from contacting the coated substrate and reduces the combustion rate. On the other hand, it dilutes the concentration of combustibles in the gas phase, thereby preventing flame retardancy. In addition, the agent can further improve the aging resistance and wear resistance of the energy storage luminescent composite material.

[0053] Energy storage luminescent composite materials are an important component of coating luminescence, and directly affect the luminescent properties of the paint film. Compared with fluorescein isothiocyanate, rhodamine and its derivatives, the chelate obtained by yttrium element excitation has a wide range of light excitation wavelengths, a narrow range of emitted light wavelengths, high initial luminescence brightness, good particle dispersion, and extended afterglow time. When the paint film is irradiated with bright light and excited by light of that wavelength, electrons with a certain energy difference in the crystal transition to orbits of higher energy levels, and the energy of the light of that wavelength is transferred to the excited electrons, that is, the light of this wavelength is absorbed and energy storage occurs. However, electrons in high-energy orbits are in a metastable state, releasing the energy of the light of that wavelength and jumping back to low-energy orbits, thereby emitting light. When Y 3+ Replace Ca 2+ , occupying two lattice positions of the luminescent center. As the concentration of yttrium ions in the system increases, the crystal structure changes from partially disordered stacking to ordered. Due to the change in the crystal structure, Y 3+ The emission band of the energy storage luminescent composite material moves to the short wave, so that the energy storage luminescent composite material has better color rendering. According to the research of technical personnel in this field, with the increase of the concentration of doped ions, more emission centers are formed inside the material, the energy absorbed by the doped ions increases, the interaction is enhanced, and the afterglow time is prolonged. However, when the concentration of doped ions increases further, that is, the supersaturated state, the ions in the excited state interact with each other, forming a new energy loss mechanism, and concentration quenching occurs. At the same time, the larger the particle size of the energy storage luminescent composite material, the higher the initial brightness after light absorption, and the longer the afterglow time. The paint film of the large-particle energy storage luminescent composite material still has a high brightness after the light stops irradiating, but the excessively large particles will affect the uniformity of the tunnel paint and have a negative impact on the surface gloss of the paint film, which is not conducive to light output. Experiments have found that when the particle size of the energy storage luminescent composite material is too large, the initial brightness of the paint film decreases. At the same time, the dispersion of the large-particle powder is poor, resulting in precipitation, which leads to poor wear resistance of the paint film. After comprehensively considering factors such as initial brightness, film forming properties, light transmittance, and afterglow time, the particle size of the material is determined. In addition, microwave sintering promotes Y 3+ Replace Ca 2+ , it is possible to obtain an energy-storage luminescent composite material with a wide excitation spectrum and emission spectrum, ensuring that it can be excited by blue light at 468nm, which is conducive to the activation of the paint film by full-color white light.

[0054] However, the paint film made of only phosphate layer and energy storage luminescent composite material is brittle, poor in toughness, and requires a high curing temperature. When subjected to a certain external load, it is easy to have holes and cracks and be easily damaged. In order to extend the service life of the paint film, improve the density of the paint film, and improve the flexibility of the paint film, the present invention evenly coats the inorganic polymer layer.

[0055] With silicate as binder and metal oxide as filler, the newly generated Si(OH)4 silica sol in an acidic environment has high activity and can form high activation energy hydroxyl groups with yttrium-doped alkali metal aluminate luminescent materials in energy storage luminescent composite materials. Hydroxyl groups are adsorbed by bonding, and silica sol is condensed to form hydrated silicate, which is quickly connected on the surface of metal particles until a stable paint film is formed, thereby improving the strength of the paint film surface. During the connection process, silica sol is catalyzed by dibutyltin dilaurate and grows together with semiconductor metal oxide to form silicon-oxygen tetrahedron. Metal oxide provides a larger area to disperse the impact force, thereby improving the mechanical properties of the paint film. A certain content of semiconductor can enhance the afterglow of the paint film and ensure that the light decay time exceeds 12h. Too little semiconductor leads to a small strengthening effect of the paint film on the incident light, and the paint film has a weak absorption effect on light, that is, the luminous intensity of the paint film becomes poor after being excited by light. Excessive semiconductors enhance the absorption of incident light, thereby reducing the afterglow time of the paint film.

[0056] Among metal oxides, alkali metal ions with small ionic radius have higher charge density, can form hydrated ions with larger radius, and have stronger reaction activity. As the content of silicate and alkali metal ions increases, the hydroxyl content in the system will increase accordingly, shortening the curing time of the paint film and significantly enhancing the bonding strength inside the coating. However, excessive silicate and alkali metal oxides will reduce the flexibility and stability of the paint film. In particular, the content of silicate directly affects the curing time and adhesion strength of the paint film.

[0057] The additive used in the silicate layer of the present invention can ensure that the electrons in the trap energy level can return to the excited state energy level and the excited transition speed is not too fast, thereby inhibiting the failure of the energy storage luminescent composite material in a short time and prolonging the afterglow time. In addition, it is important that according to the research of those skilled in the art, Na + The addition of sodium salt will affect the crystal structure of the energy storage luminescent material, resulting in a significant reduction in the luminescence intensity of the material. Therefore, the present invention avoids the use of sodium salt.

[0058] When applied, the trivalent phosphate ions formed by phosphate dissolving in ethanol polymerize with the metal oxides in the inorganic polymer layer. At this time, active sites are formed on the divalent phosphate ions, which promote the adsorption of the surrounding dimethylphosphate ions. Further, monovalent phosphate ions are formed in the solution, which continue to adsorb and highly connect, thereby forming a spatial three-dimensional network and improving the density of the paint film. The phosphate layer material is coupled with the metal oxide in the energy storage luminescent composite material. The phosphate layer material enters the cracks of the metal oxide and plays a filling and "pinning" role. At the same time, with the help of the load, the inorganic system is transferred and embedded in the microscopic gaps of the coated substrate, thereby improving the adhesion strength of the energy storage luminescent composite material, the phosphate layer and the coated substrate. However, the single-layer inorganic polymer layer has problems such as high porosity, insufficient bonding strength with the coated substrate, and poor corrosion resistance. Therefore, the inorganic polymer layer needs to be used in conjunction with the phosphate layer and the energy storage luminescent composite material.

[0059] During drying and curing, an environment with moderate humidity and temperature is provided, and a protective layer of hydrated silicate compounds is formed on the surface of the tunnel paint. This protective layer not only reduces the curing temperature and avoids cracks and pores caused by rapid drying of thermal curing, but also effectively increases the electrochemical transfer resistance of the paint film, significantly enhancing the anti-static effect of the paint film, thereby avoiding fire caused by accumulated static electricity in the tunnel. At the same time, the vibration of metal crystals causes atomic diffusion between metal crystals and inorganic systems, and a diffusion solid solution interface is formed between metal and non-metal atoms, which significantly enhances the adhesion strength of the paint film.

[0060] In addition, compared with method A, the energy storage luminescent composite material of method B is evenly distributed in the inorganic polymer layer. Under the influence of the catalyst, although it shows excellent luminescent performance, due to the exposure of a large amount of energy storage luminescent composite materials, the service life of the tunnel paint is slightly shorter and the afterglow time is relatively short. In addition, the antistatic performance of the inorganic polymer layer covered with particles is much lower than that of the layered inorganic polymer material, and static electricity accumulates rapidly, increasing the risk of fire. In method C, the prepared paint film presents a mixed topological structure at the microscopic level, and the energy storage luminescent composite material settles between the phosphate layer and the coated substrate and agglomerates, which makes the coordination between the energy storage luminescent composite material and the phosphate layer more effective, and the paint film presents a longer afterglow time.

[0061] In the production process of the coating, since there is no release of volatile organic compounds, the emission of harmful substances is greatly reduced, so the tunnel paint of the present invention is environmentally friendly. While maintaining the performance, the present invention reduces the production cost as much as possible to facilitate large-scale commercial applications. The present invention improves the luminous efficiency of the paint film, prolongs the afterglow time, and can maintain a long-term luminous state without an external light source. The coating can maintain good durability and stability in extreme temperature and high humidity environments, and the curing shrinkage is smaller than that of general organic binders, and has good durability in the service environment.

[0062] The beneficial effects of the present invention are as follows:

[0063] (1) The tunnel paint prepared by the present invention has good suspension stability, and can be easily mixed evenly by stirring when slightly stratified. It can be applied to rough surfaces such as walls, cement concrete, masonry materials, etc. in tunnels, and has high adhesion strength;

[0064] (2) The energy storage luminescent composite material used in the present invention is non-toxic, non-radioactive, non-polluting to the environment, and harmless to the human body. The prepared tunnel paint has high brightness and an afterglow time of more than 12 hours. Natural light, vehicle lights, LED lights, etc. can effectively excite the tunnel paint, which can significantly improve the brightness of the tunnel inner wall and road surface, and can achieve a delayed luminescence effect. It can be applied to accident scenes such as fires to play an emergency lighting role;

[0065] (3) The tunnel paint prepared by the present invention is an inorganic system, which avoids the aging problem of organic materials and has long-term durability and service life in the tunnel environment;

[0066] (4) The water-based inorganic multifunctional tunnel paint prepared by the present invention is non-toxic, mildew-proof, antibacterial, and aging-resistant, and does not contain volatile harmful substances such as formaldehyde, toluene, and TVOC, so it is green, low-carbon, energy-saving and environmentally friendly;

[0067] (5) The tunnel paint prepared by the present invention can be processed under normal temperature and pressure conditions, and has the characteristics of simple preparation process, low production cost, easy operation and strong practical value. DETAILED DESCRIPTION

[0068] The present invention is further described in detail below in conjunction with specific embodiments. Those of ordinary skill in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all embodiments. Therefore, based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work should fall within the scope of protection of the present invention.

[0069] Unless otherwise specified, the raw materials used in the examples of the present invention are all commercially available or available to those skilled in the art; unless otherwise specified, the methods used in the examples of the present invention are all methods known to those skilled in the art.

[0070] Example 1

[0071] A method for preparing an inorganic system tunnel paint,

[0072] The method comprises:

[0073] 1) Preparation of phosphate layer material: 5 g aluminum phosphate, 0.1 mL defoamer SPJ-301, 0.1 mL dispersant WL-302, 0.1 mL CB-903 thickener, and 10 mL ethanol were mixed evenly;

[0074] 2) Preparation of energy storage luminescent composite material: 10 g of calcium aluminate and 0.5 g of yttrium fluoride were mixed and ground to a particle size of 1 μm, and then 1 g of graphene was added, and the mixture was kept at 1200° C. for 6 h;

[0075] 3) Preparation of inorganic polymer layer material: 12 g potassium silicate and 2.4 g titanium dioxide with a particle size of 1 μm were dispersed in a 3 mol / L acetic acid aqueous solution, and the pH value of the system was adjusted to 4 with a 3 mol / L acetic acid aqueous solution, and 1 mL dibutyltin dilaurate was added and mixed evenly;

[0076] 4) Forming tunnel paint by any of the following three methods:

[0077] Method A: uniformly distributing the phosphate layer material, the energy storage luminescent composite material and the inorganic polymer layer material, and drying and curing them at about 18° C. to form a paint film 1;

[0078] Method B: Evenly distribute the phosphate layer material and dry and solidify it at about 18°C, take the energy storage luminescent composite material and the inorganic polymer layer material and mix them evenly, evenly distribute them on the dry phosphate layer, and dry and solidify them at about 18°C ​​to form a paint film 2;

[0079] Method C: Evenly mix the phosphate layer material and the energy storage luminescent composite material, evenly distribute them and dry and solidify them at about 18° C. After drying, evenly distribute the inorganic polymer layer material, dry and solidify them at about 18° C. to form a paint film 3;

[0080] Step 4) The coating amount of the phosphate layer material is controlled so that the paving thickness is 4 μm, the coating amount of the energy storage luminescent composite material is controlled so that the paving thickness is 5 μm, and the coating amount of the inorganic polymer layer material is controlled so that the paving thickness is 6 μm. The performance of the paint film prepared in this example is tested as follows.

[0081] 1. Initial brightness

[0082] Irradiate the paint film sample with 2000lm (lumens) of light simulating a car light for 30 minutes, and place it in a dark box to detect its initial brightness.

[0083] 2. Afterglow time

[0084] Based on test (1), record the time from when the paint film sample glows to when the brightness is ≤3cd / m 2 time.

[0085] 3. Water resistance

[0086] Immerse the paint film sample in water and record the time for which the paint film sample does not show blistering, cracking or peeling, which shall be no more than 50 days. If ≥50 days, mark it as 50 days.

[0087] 4. Alkali resistance

[0088] Carry out alkali resistance test according to standard GB / T 9265-2009 "Determination of alkali resistance of architectural paint coatings" and record the time for which the paint film sample does not show blistering, cracking or peeling, which shall be no more than 480 hours. If it is ≥480 hours, it shall be marked as 480 hours.

[0089] 5. Resistance to temperature change

[0090] At a temperature of -20 to 40°C, the paint film sample is subjected to 50 cycles of rapid heating and rapid cooling. If no blistering, cracking or peeling occurs, it is recorded as "√", otherwise it is recorded as "×".

[0091] 6. Wear resistance

[0092] Use 500-grit sandpaper to grind the paint film sample for 20,000 circles. If no coated substrate is observed, it means that the paint film sample is not leaking and the wear resistance meets the requirements.

[0093] 7. High temperature resistance

[0094] At 600℃, keep the formed paint film sample at a constant temperature for 1 hour. If there is no blistering, cracking or peeling, it is recorded as "√", otherwise it is recorded as "×".

[0095]

[0096]

[0097] According to the results in the table, the paint film samples in this example can emit light for more than 12 hours after being excited by light. Natural light, vehicle lights, LED lights, etc. can effectively excite tunnel paint, which can significantly improve the brightness of the tunnel walls and road surfaces, and can achieve a delayed luminescence effect. It can be used in accident scenes such as fires to play an emergency lighting role. In addition, the initial brightness of the excited fluorescence is only about 50-65cd / m 2 This brightness will not cause glare, will not affect the driving of vehicles in the tunnel, can avoid the glare to the vehicle driver caused by excessive fluorescence excitation, and avoid the occurrence of safety hazards. At the same time, generally 30 ~ 70cd / m 2 As a more suitable brightness range, the paint film 1 can maintain 30cd / m 2The above time reaches about 11 hours, and the paint film 2 can also be maintained for about 10 hours, and the paint film 3 can even be maintained for about 13 hours. After being maintained for a long time, its fluorescence will undergo a rapid extinguishing process. It can be seen that the tunnel paint of the present invention can produce a lasting, effective and soft fluorescent luminescence effect to improve the dark light environment in the tunnel, thereby improving the safety of vehicles driving in the tunnel. And based on the above data, the most effective coating method for the tunnel paint of the present invention is the coating method of method C, because it can more effectively combine the energy storage luminescent composite material and the silicate layer, so as to have a longer luminescent afterglow time, and the light is relatively soft, but it can also be seen that the silicate layer will actually suppress the luminous brightness of the energy storage luminescent composite material to a certain extent, but for the actual use scenario of the tunnel paint, it is actually not harmful, and is even beneficial, and the fluorescence it produces is softer.

[0098] In addition, the paint film has good water resistance, alkali resistance, temperature change resistance, wear resistance and high temperature resistance, which can meet the basic protection needs of tunnel paint for the tunnel matrix. At the same time, due to the good physical and chemical properties of the paint film, the paint film loss is small in extreme weather, ensuring good luminous performance.

[0099] Example 2

[0100] A method for preparing an inorganic system tunnel paint,

[0101] The method comprises:

[0102] 1) Preparation of phosphate layer material: 5 g aluminum phosphate, 0.1 mL defoamer SPJ-301, 0.1 mL dispersant WL-302, 0.1 mL CB-903 thickener, and 10 mL ethanol were mixed evenly;

[0103] 2) Preparation of energy storage luminescent composite material: 10 g of calcium aluminate and 0.75 g of yttrium fluoride were mixed and ground to a particle size of 1 μm, and then 1 g of graphene was added and kept at 1200° C. for 6 h;

[0104] 3) Preparation of inorganic polymer layer material: 12 g potassium silicate and 2.4 g titanium dioxide with a particle size of 1 μm were dispersed in a 3 mol / L acetic acid aqueous solution, and the pH value of the system was adjusted to 4 with a 3 mol / L acetic acid aqueous solution, and 1 mL dibutyltin dilaurate was added and mixed evenly;

[0105] 4) Forming tunnel paint by any of the following three methods:

[0106] Method A: uniformly distributing the phosphate layer material, the energy storage luminescent composite material and the inorganic polymer layer material, and drying and curing them at about 18° C. to form a paint film 1;

[0107] Method B: Evenly distribute the phosphate layer material and dry and solidify it at about 18°C, take the energy storage luminescent composite material and the inorganic polymer layer material and mix them evenly, evenly distribute them on the dry phosphate layer, and dry and solidify them at about 18°C ​​to form a paint film 2;

[0108] Method C: Evenly mix the phosphate layer material and the energy storage luminescent composite material, evenly distribute them and dry and solidify them at about 18° C. After drying, evenly distribute the inorganic polymer layer material, dry and solidify them at about 18° C. to form a paint film 3;

[0109] Step 4) The coating amount of the phosphate layer material is controlled so that the paving thickness is 4 μm, the coating amount of the energy storage luminescent composite material is controlled so that the paving thickness is 5 μm, and the coating amount of the inorganic polymer layer material is controlled so that the paving thickness is 6 μm. The paint film prepared in this example is tested for performance in the same manner as in Example 1, and the test results are as follows.

[0110]

[0111] According to the results in the table, as the Y 3+ As the ion concentration increases, the crystal structure changes from partially disordered stacking to ordered. Due to the change in the crystal structure, Y 3+ The emission band of the ions moves to the short wavelength, making the energy storage luminescent composite material have better color rendering and enhanced initial brightness. As the concentration of doped ions increases, more emission centers are formed inside the material, the energy absorbed by the doped ions increases, the interaction is enhanced, and the afterglow time is prolonged.

[0112] Example 3

[0113] A method for preparing an inorganic system tunnel paint,

[0114] The method comprises:

[0115] 1) Preparation of phosphate layer material: 5 g aluminum phosphate, 0.1 mL defoamer SPJ-301, 0.1 mL dispersant WL-302, 0.1 mL CB-903 thickener, and 10 mL ethanol were mixed evenly;

[0116] 2) Preparation of energy storage luminescent composite material: 10 g of calcium aluminate and 1.0 g of yttrium fluoride were mixed and ground to a particle size of 1 μm, and then 1 g of graphene was added, and the mixture was kept at a constant temperature of 1200° C. for 6 h;

[0117] 3) Preparation of inorganic polymer layer material: 12 g potassium silicate and 2.4 g titanium dioxide with a particle size of 1 μm were dispersed in a 3 mol / L acetic acid aqueous solution, and the pH value of the system was adjusted to 4 with a 3 mol / L acetic acid aqueous solution, and 1 mL dibutyltin dilaurate was added and mixed evenly;

[0118] 4) Forming tunnel paint by any of the following three methods:

[0119] Method A: uniformly distributing the phosphate layer material, the energy storage luminescent composite material and the inorganic polymer layer material, and drying and curing them at about 18° C. to form a paint film 1;

[0120] Method B: Evenly distribute the phosphate layer material and dry and solidify it at about 18°C, take the energy storage luminescent composite material and the inorganic polymer layer material and mix them evenly, evenly distribute them on the dry phosphate layer, and dry and solidify them at about 18°C ​​to form a paint film 2;

[0121] Method C: Evenly mix the phosphate layer material and the energy storage luminescent composite material, evenly distribute them and dry and solidify them at about 18° C. After drying, evenly distribute the inorganic polymer layer material, dry and solidify them at about 18° C. to form a paint film 3;

[0122] Step 4) The coating amount of the phosphate layer material is controlled so that the flat thickness is 4 μm, the coating amount of the energy storage luminescent composite material is controlled so that the flat thickness is 5 μm, and the coating amount of the inorganic polymer layer material is controlled so that the flat thickness is 6 μm.

[0123] The paint film prepared in this example was subjected to the same performance test as in Example 1, and the test results are as follows.

[0124]

[0125] According to the results in the table, when the doping ion concentration is further increased and reaches the supersaturated state, the ions in the excited state interact with each other, forming a new energy loss mechanism, and concentration quenching occurs. Therefore, the afterglow time and initial brightness of the paint film in this example are reduced to a certain extent, but for paint film 3, due to the higher effectiveness of the combination of its energy storage luminescent composite material and the silicate layer, it is relatively less affected.

[0126] Combined with the results in the tables of Examples 1 to 3, compared to method A, the energy storage luminescent composite material of method B is evenly distributed in the inorganic polymer layer. Affected by the catalyst, although it exhibits excellent luminescent performance, a large amount of energy storage luminescent composite material is exposed, resulting in a slightly shorter service life of the tunnel paint and a relatively short afterglow time. In addition, the antistatic performance of the inorganic polymer layer covered with particulate matter is much lower than that of the layered inorganic polymer material, and static electricity accumulates rapidly, increasing the risk of fire. In method C, the prepared paint film presents a mixed topological structure at the microscopic level, and the energy storage luminescent composite material settles between the phosphate layer and the coated substrate, agglomerates, and makes the coordination effectiveness of the energy storage luminescent composite material and the phosphate layer stronger, and the paint film exhibits a longer afterglow time.

[0127] Comparative Example 1

[0128] A method for preparing an inorganic system tunnel paint,

[0129] The method comprises:

[0130] 1) Preparation of energy storage luminescent composite material: 10 g of calcium aluminate and 0.75 g of yttrium fluoride were mixed and ground to a particle size of 1 μm, and then 1 g of graphene was added, and the mixture was kept at 1200° C. for 6 h;

[0131] 2) Preparation of inorganic polymer layer material: 12 g potassium silicate and 2.4 g titanium dioxide with a particle size of 1 μm were dispersed in a 3 mol / L acetic acid aqueous solution, and the pH value of the system was adjusted to 4 with a 3 mol / L acetic acid aqueous solution, and 1 mL dibutyltin dilaurate was added and mixed evenly;

[0132] 3) Forming tunnel paint by any of the following two methods:

[0133] Method B: the energy storage luminescent composite material and the inorganic polymer layer material are mixed evenly and evenly distributed, and dried and cured at about 18° C. to form a paint film 2;

[0134] Method C: uniformly distributing the energy storage luminescent composite material, and then uniformly distributing the inorganic polymer layer material, and drying and curing at about 18° C. to form a paint film 3;

[0135] Step 3) The coating amount of the energy storage luminescent composite material is controlled so that its flat thickness is 5 μm, and the coating amount of the inorganic polymer layer material is controlled so that its flat thickness is 6 μm.

[0136] The paint film prepared in this example was subjected to the same performance test as in Example 1, and the test results are as follows.

[0137]

[0138]

[0139] According to the results in the table, the paint film has poor temperature resistance and high temperature resistance, and has peeling, cracking and other phenomena. The reason is that phosphate contains P=O double bonds, which provide a pair of free electrons and can form a coupling with calcium aluminate. However, there is no bonding in the paint film of this example, resulting in the density and bonding force of the paint film of this example being much lower than the paint film of Example 2, and the mechanical properties are significantly reduced. In addition, the protective effect of the inorganic polymer layer on the energy storage luminescent composite material is weakened, resulting in the paint film afterglow time being much less than the required time. The heat source is brought close to the center of the paint film of this example until it touches, and the partition effect of the paint film of this example on the coated substrate is significantly deteriorated.

[0140] The current density of the paint film of Example 2 and this example was characterized. The corrosion current density of the paint film of Example 2 was 14.2 μA / cm 2 The corrosion current density of the paint film in this example is 18.9μA / cm 2 It can be seen that the corrosion resistance of the paint film without a phosphate layer deteriorates and the corrosion rate is fast.

[0141] Comparative Example 2

[0142] A method for preparing an inorganic system tunnel paint,

[0143] The method comprises:

[0144] 1) Preparation of phosphate layer material: 5 g aluminum phosphate, 0.1 mL defoamer SPJ-301, 0.1 mL dispersant WL-302, 0.1 mL CB-903 thickener, and 10 mL ethanol were mixed evenly;

[0145] 2) Preparation of energy storage luminescent composite material: 10 g of calcium aluminate and 0.75 g of yttrium fluoride were mixed and ground to a particle size of 4 μm, and then 1 g of graphene was added, and the mixture was kept at 1200° C. for 6 h;

[0146] 3) Preparation of inorganic polymer layer material: 12 g potassium silicate and 2.4 g titanium dioxide with a particle size of 1 μm were dispersed in a 3 mol / L acetic acid aqueous solution, and the pH value of the system was adjusted to 4 with a 3 mol / L acetic acid aqueous solution, and 1 mL dibutyltin dilaurate was added and mixed evenly;

[0147] 4) Forming tunnel paint by any of the following three methods:

[0148] Method A: uniformly distributing the phosphate layer material, the energy storage luminescent composite material and the inorganic polymer layer material, and drying and curing them at about 18° C. to form a paint film 1;

[0149] Method B: Evenly distribute the phosphate layer material and dry and solidify it at about 18°C, take the energy storage luminescent composite material and the inorganic polymer layer material and mix them evenly, evenly distribute them on the dry phosphate layer, and dry and solidify them at about 18°C ​​to form a paint film 2;

[0150] Method C: Evenly mix the phosphate layer material and the energy storage luminescent composite material, evenly distribute them and dry and solidify them at about 18° C. After drying, evenly distribute the inorganic polymer layer material, dry and solidify them at about 18° C. to form a paint film 3;

[0151] Step 4) The coating amount of the phosphate layer material is controlled so that the flat thickness is 4 μm, the coating amount of the energy storage luminescent composite material is controlled so that the flat thickness is 5 μm, and the coating amount of the inorganic polymer layer material is controlled so that the flat thickness is 6 μm.

[0152] The paint film prepared in this example was subjected to the same performance test as in Example 1, and the test results are as follows.

[0153]

[0154]

[0155] Energy storage luminescent composite materials are an important component of coating luminescence, which directly affects the luminescent properties of the paint film. The chelate obtained by yttrium element excitation has a wide range of light excitation wavelengths, a narrow range of emitted light wavelengths, high initial luminescence brightness, good particle dispersion, and long afterglow time. When the paint film is irradiated with bright light and excited by the light of this wavelength, the electrons with a certain energy difference in the crystal jump to the orbit of a higher energy level, and the energy of the light of this wavelength is transferred to the excited electrons, that is, the light of this wavelength is absorbed and energy storage occurs. However, the electrons in the high-energy orbit are a metastable state, releasing the energy of the light of this wavelength and jumping back to the low-energy orbit, thereby emitting light. According to the results in the table, the energy storage luminescent composite material with too large a particle size affects the uniformity of the tunnel paint and has a negative impact on the surface gloss of the paint film, which is not conducive to light output. It was found through experiments that when the particle size of the energy storage luminescent composite material is too large, the initial brightness of the paint film decreases by more than 10%. At the same time, the large particle size powder has poor dispersibility, resulting in precipitation, which leads to poor wear resistance of the paint film. However, when the energy storage luminescent composite material is ground too finely, the scattering cross section increases, and the grinding process easily causes surface damage and defects. It is also easy to aggregate and cause aggregation quenching during use, so the actual fluorescence effect is significantly reduced. For example, after calcium aluminate and yttrium fluoride are mixed and ground to 0.5 μm, the initial brightness of the paint film 3 is only about 42.71 cd / m 2 , but the afterglow time is relatively less affected and can still maintain a 14h afterglow time.

[0156] Comparative Example 3

[0157] A method for preparing an inorganic system tunnel paint,

[0158] The method comprises:

[0159] 1) Preparation of phosphate layer material: 5 g aluminum phosphate, 0.1 mL defoamer SPJ-301, 0.1 mL dispersant WL-302, 0.1 mL CB-903 thickener, and 10 mL ethanol were mixed evenly;

[0160] 2) Preparation of energy storage luminescent composite material: 10 g of calcium aluminate and 0.75 g of yttrium fluoride were mixed and ground to a particle size of 1 μm, and then 1 g of graphene was added and kept at 1200° C. for 6 h;

[0161] 3) Forming tunnel paint by any of the following two methods:

[0162] Method A: uniformly distributing the phosphate layer material and the energy storage luminescent composite material, respectively, and drying and curing at about 18° C. to form a paint film 1;

[0163] Method C: Mix the phosphate layer material and the energy storage luminescent composite material evenly, distribute them evenly and dry and cure them at about 18° C., and dry and cure them at about 18° C. to form a paint film 3;

[0164] In step 3), the coating amount of the phosphate layer material is controlled so that the flat thickness is 4 μm, and the coating amount of the energy storage luminescent composite material is controlled so that the flat thickness is 5 μm.

[0165] The paint film prepared in this example was subjected to the same performance test as in Example 1, and the test results are as follows.

[0166]

[0167] During the bonding process, the silica sol is catalyzed by dibutyltin dilaurate, combined with semiconductor metal oxides, and grows together to form silicon-oxygen tetrahedrons. Silicates can produce highly active Si(OH)4 in an acidic environment, further forming hydroxyl groups with high activation energy, bonding, adsorption and polycondensation to form hydrated silica. Metal oxides provide a larger area to disperse the impact force, thereby improving the mechanical properties of the paint film. However, in this example, the hydroxyl content is low, the paint film curing time is extended, the internal bonding strength is insufficient, the brittleness is large, and the toughness is poor. When subjected to a certain external load, holes and cracks are prone to appear, it is easy to be damaged, and the service life is short. Combined with the test results of comparative example 1 and the paint film of this example, the inorganic polymer layer needs to be used in conjunction with the phosphate layer and the energy storage luminescent composite material. However, from the above data results, it can also be seen that without the inorganic polymer layer, the phosphate layer has a greater impact on the brightness, and although the inorganic polymer layer does not have a direct effect of extending the afterglow time, due to the relatively high exposure of the energy storage luminescent composite material, the afterglow time is also shortened accordingly.

[0168] Comparative Example 4

[0169] A method for preparing an inorganic system tunnel paint,

[0170] The method comprises:

[0171] 1) Preparation of phosphate layer material: 5 g aluminum phosphate, 0.1 mL defoamer SPJ-301, 0.1 mL dispersant WL-302, 0.1 mL CB-903 thickener, and 10 mL ethanol were mixed evenly;

[0172] 2) Preparation of energy storage luminescent composite material: 10 g of calcium aluminate and 0.75 g of yttrium fluoride were mixed and ground to a particle size of 1 μm, and then 1 g of graphene was added and kept at 1200° C. for 6 h;

[0173] 3) Preparation of inorganic polymer layer material: 12 g potassium silicate and 6 g titanium dioxide with a particle size of 1 μm were dispersed in a 3 mol / L acetic acid aqueous solution, and the pH value of the system was adjusted to 4 with a 3 mol / L acetic acid aqueous solution, and 1 mL dibutyltin dilaurate was added and mixed evenly;

[0174] 4) Forming tunnel paint by any of the following three methods:

[0175] Method A: uniformly distributing the phosphate layer material, the energy storage luminescent composite material and the inorganic polymer layer material, and drying and curing them at about 18° C. to form a paint film 1;

[0176] Method B: Evenly distribute the phosphate layer material and dry and solidify it at about 18°C, take the energy storage luminescent composite material and the inorganic polymer layer material and mix them evenly, evenly distribute them on the dry phosphate layer, and dry and solidify them at about 18°C ​​to form a paint film 2;

[0177] Method C: Evenly mix the phosphate layer material and the energy storage luminescent composite material, evenly distribute them and dry and solidify them at about 18° C. After drying, evenly distribute the inorganic polymer layer material, dry and solidify them at about 18° C. to form a paint film 3;

[0178] Step 4) The coating amount of the phosphate layer material is controlled so that the flat thickness is 4 μm, the coating amount of the energy storage luminescent composite material is controlled so that the flat thickness is 5 μm, and the coating amount of the inorganic polymer layer material is controlled so that the flat thickness is 6 μm.

[0179] The paint film prepared in this example was subjected to the same performance test as in Example 1, and the test results are as follows.

[0180]

[0181] The increase in the amount of titanium dioxide can enhance the effect of incident light, so that the paint film absorbs light more strongly, that is, the luminous intensity of the paint film is enhanced. However, in this case, excessive semiconductors are used, which enhances the absorption of incident light, reduces the path length of fluorescent emission, and even forms electron capture recombination centers to capture excited electrons in fluorescent materials, thereby reducing the afterglow time of the paint film. According to the results in the table, the afterglow time of the paint film in this case is greatly shortened, which is difficult to meet the requirements.

[0182] Comparative Example 5

[0183] A method for preparing an inorganic system tunnel paint,

[0184] The method comprises:

[0185] 1) Preparation of phosphate layer material: 5 g aluminum phosphate, 0.1 mL defoamer SPJ-301, 0.1 mL dispersant WL-302, 0.1 mL CB-903 thickener, and 10 mL ethanol were mixed evenly;

[0186] 2) Preparation of energy storage luminescent composite material: 10 g of calcium aluminate and 0.75 g of yttrium fluoride were mixed and ground to a particle size of 1 μm, and then 1 g of graphene was added and kept at 1200° C. for 6 h;

[0187] 3) Preparation of inorganic polymer layer material: 12 g potassium silicate and 2.4 g titanium dioxide with a particle size of 1 μm were dispersed in a 3 mol / L acetic acid aqueous solution and the pH value of the system was adjusted to 4 with the 3 mol / L acetic acid aqueous solution;

[0188] 4) Forming tunnel paint by any of the following three methods:

[0189] Method A: uniformly distributing the phosphate layer material, the energy storage luminescent composite material and the inorganic polymer layer material, and drying and curing them at about 18° C. to form a paint film 1;

[0190] Method B: Evenly distribute the phosphate layer material and dry and solidify it at about 18°C, take the energy storage luminescent composite material and the inorganic polymer layer material and mix them evenly, evenly distribute them on the dry phosphate layer, and dry and solidify them at about 18°C ​​to form a paint film 2;

[0191] Method C: Evenly mix the phosphate layer material and the energy storage luminescent composite material, evenly distribute them and dry and solidify them at about 18° C. After drying, evenly distribute the inorganic polymer layer material, dry and solidify them at about 18° C. to form a paint film 3;

[0192] Step 4) The coating amount of the phosphate layer material is controlled so that the flat thickness is 4 μm, the coating amount of the energy storage luminescent composite material is controlled so that the flat thickness is 5 μm, and the coating amount of the inorganic polymer layer material is controlled so that the flat thickness is 6 μm.

[0193] The paint film prepared in this example was subjected to the same performance test as in Example 1, and the test results are as follows.

[0194]

[0195] According to the results in the table, the effect of dibutyltin dilaurate on the initial brightness is relatively small, but the effect on the afterglow time is relatively significant, the energy storage luminescent composite material fails in a short time, and the afterglow time is short. This is because dibutyltin dilaurate can actually inhibit the ability of titanium dioxide to capture electrons excited in the fluorescent material to a certain extent, resulting in a phenomenon similar to that of Comparative Example 4.

[0196] Comparative Example 6

[0197] A method for preparing an inorganic system tunnel paint,

[0198] The method comprises:

[0199] 1) Preparation of phosphate layer material: 5 g aluminum phosphate, 0.1 mL defoamer SPJ-301, 0.1 mL dispersant WL-302, 0.1 mL CB-903 thickener, and 10 mL ethanol were mixed evenly;

[0200] 2) Preparation of energy storage luminescent composite material: 10 g of calcium aluminate and 0.75 g of yttrium fluoride were mixed and ground to a particle size of 1 μm, and then 1 g of graphene was added and kept at 1200° C. for 6 h;

[0201] 3) Preparation of inorganic polymer layer material: 12 g potassium silicate and 2.4 g titanium dioxide with a particle size of 1 μm were dispersed in a 3 mol / L acetic acid aqueous solution, and the pH value of the system was adjusted to 4 with a 3 mol / L acetic acid aqueous solution, and 1 mL dibutyltin dilaurate was added and mixed evenly;

[0202] 4) Forming tunnel paint by any of the following three methods:

[0203] Method A: uniformly distributing the phosphate layer material, the energy storage luminescent composite material and the inorganic polymer layer material, and thermally curing them at 45° C. to form a paint film 1;

[0204] Method B: Evenly distribute the phosphate layer material, heat cure at 45°C, take the energy storage luminescent composite material and the inorganic polymer layer material and mix them evenly, evenly distribute them on the dry phosphate layer, and heat cure at 45°C to form a paint film 2;

[0205] Method C: Evenly mix the phosphate layer material and the energy storage luminescent composite material, evenly distribute them and heat cure them at 45°C, evenly distribute the inorganic polymer layer material after drying, and heat cure them at 45°C to form a paint film 3;

[0206] Step 4) The coating amount of the phosphate layer material is controlled so that the paving thickness is 4 μm, the coating amount of the energy storage luminescent composite material is controlled so that the paving thickness is 5 μm, and the coating amount of the inorganic polymer layer material is controlled so that the paving thickness is 6 μm. The paint film prepared in this example is tested for performance in the same manner as in Example 1, and the test results are as follows.

[0207]

[0208]

[0209] The electrochemical transfer resistance of the paint film of Example 2 and this example was characterized. After characterization, the resistance of the paint film of this example was 1.67×10 5 Ω·cm 2 Compared with the paint film of Example 2, it decreased by 17.2%, the antistatic effect of the paint film was deteriorated, and the probability of fire caused by accumulated static electricity in the paint film increased significantly. According to the results in the table, the performance of the paint film in this example, such as temperature change resistance, was deteriorated. The reason was that the curing temperature required for thermal curing was high, and the higher the temperature, the faster the drying speed, and obvious cracks and peeling appeared.

[0210] In addition, it can be seen from the above results that the use of a higher curing temperature will significantly shorten the initial brightness and afterglow time of the paint film, especially for paint film 3. This is because the temperature affects the curing order or law between the layers of materials, resulting in the influence of the internal component distribution of the material, which in turn affects the uniformity and porosity of the coating. The microstructure of the coating has an effect on the scattering, absorption and transmission of fluorescence, thereby affecting the luminescence performance. Especially for paint film 3, due to the higher thermal curing temperature, the silicate layer may be analyzed, resulting in the energy storage composite luminescent material being "pushed" into the inorganic polymer layer, resulting in a change in the distribution position of the energy storage luminescent composite material. And from the perspective of subsequent multiple tests, controlling the curing temperature to 15-25°C can maintain a relatively optimal curing effect. When the curing temperature is higher than 25°C (single factor variable test with a gradient of 5°C), the initial brightness and afterglow time begin to decrease, and when it is lower than 15°C, the above situation also occurs accordingly.

Claims

1. An inorganic system tunnel paint, characterized in that: The inorganic system tunnel paint comprises a phosphate layer material, an energy storage luminescent composite material and an inorganic polymer layer material; The preparation method of the inorganic system tunnel paint comprises: 1) The preparation method of the phosphate layer material: phosphate, an additive and a solvent are mixed uniformly; 2) The preparation method of the energy storage luminescent composite material: aluminate and fluoride are mixed evenly, then ground and sieved, and a reducing agent is added to perform microwave sintering; 3) The preparation method of the inorganic polymer layer material is as follows: silicate and metal oxide are dispersed in an acid solution, and the amount of the acid solution is controlled to adjust the pH value to a weakly acidic condition, and then an auxiliary agent is added and mixed uniformly; The phosphate layer material, the energy storage luminescent composite material and the inorganic polymer layer material are prepared and stored in independent bags; 4) Forming tunnel paint by any of the following three methods: Method A: Evenly distribute the phosphate layer material, the energy storage luminescent composite material and the inorganic polymer layer material, and dry and solidify them at 15-25°C to form a paint film; Method B: Evenly distribute the phosphate layer material and dry and solidify it at 15-25°C. Take the energy storage luminescent composite material and the inorganic polymer layer material and mix them evenly, evenly distribute them on the dry phosphate layer, and dry and solidify them at 15-25°C to form a paint film; Method C: Mix the phosphate layer material and the energy storage luminescent composite material evenly, distribute them evenly and dry and cure them at 15-25°C, evenly distribute the inorganic polymer layer material after drying, and dry and cure them at 15-25°C to form a paint film; In the preparation method of the phosphate layer material: The phosphate is aluminum phosphate and / or zirconium phosphate and / or magnesium phosphate and / or aluminum chromium phosphate; The auxiliary agent is a defoamer and / or a dispersant and / or a thickener, and its dosage is 0.01-0.1 mL / g phosphate; The solvent is ethanol, and its usage is 1-2 mL / g phosphate; In the preparation method of the energy storage luminescent composite material: The aluminate is calcium aluminate; The fluoride is yttrium fluoride, and its dosage is 0.05-0.1 g / g aluminate; The reducing agent is graphene, and its usage is 0.1-0.2 g / g aluminate; The grinding is to grind the mixed materials to a particle size of 1 to 3 μm; The microwave sintering is carried out at a constant temperature of 1200-1300°C for 4-6 hours; In the preparation method of the inorganic polymer layer material: The silicate is potassium silicate and / or lithium silicate and / or ammonium silicate; The metal oxide is titanium dioxide and / or cuprous oxide and / or zinc oxide and / or tin dioxide and / or aluminum oxide, and its particle size is 1 to 3 μm, and its dosage is 0.2 to 0.4 g / g silicate; The acid solution is an aqueous solution of acetic acid, and its concentration is 1 to 3 mol / L; The auxiliary agent is dibutyltin dilaurate, and the dosage thereof is 0.05-0.1 mL / g silicate.

2. An inorganic system tunnel paint according to claim 1, characterized in that: In the preparation method of the inorganic polymer layer material: The pH value of the weakly acidic condition is 4 to 5.5.