Anticorrosive powder coating for fire-fighting pipeline and preparation method thereof
Through anticorrosion powder coatings combined with epoxy components and polyurethane components, combined with electrostatic spraying technology and filler composition, the problems of adhesion and impact resistance of anticorrosion coatings on galvanized steel pipes are solved, and long-lasting protection of fire-fighting pipes is achieved and performance improvement.
Patent Information
- Application Number
- CN202410817974.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-06-24
AI Technical Summary
The anticorrosion coating formed by the existing epoxy powder coating FBE on galvanized steel pipes has poor adhesion, and the heat and cold impact resistance needs to be improved, which affects the service life of the fire-fighting pipeline.
Anticorrosion powder coatings that combine epoxy components and polyurethane components are used to form a anticorrosion coating with strong binding force and galvanized steel pipes through a specific electrostatic spraying process, containing filler compositions such as calcium carbonate, kaolin, etc., to improve the anticorrosion coating. Resistant to hot and cold impact toughness and weather resistance.
It significantly improves the anti-corrosion coating's anti-cold impact toughness, hydrolysis resistance, heat resistance and corrosion resistance, extends the service life of fire-fighting pipes, and simplifies the production process for industrial manufacturing.
Smart Images

Figure BDA0004908268680000171 
Figure BDA0004908268680000172 
Figure BDA0004908268680000181
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of pipeline powder coating preparation, and in particular to an anti-corrosion powder coating for fire protection pipelines and a preparation method thereof. Background Art
[0002] Steel pipes used in water, oil, gas and other fields are susceptible to corrosion from the external environment and therefore require surface anti-corrosion treatment. After anti-corrosion treatment to form an anti-corrosion coating, it can effectively prevent or slow down chemical or electrochemical reactions on the surface of the steel pipe during transportation and use, thereby improving the service life of the steel pipe. The quality and performance of the anti-corrosion coating determine the stability and service life of the steel pipe, which requires the anti-corrosion coating formed by the anti-corrosion coating to have good heat resistance, impact resistance, permeability resistance, insulation, and good adhesion to metals.
[0003] Thermosetting heavy-duty anti-corrosion epoxy powder coating, also known as fusion-bonded epoxy powder coating FBE, has good adhesion to metal and has good heat resistance, permeability resistance, insulation and certain impact resistance. It is the current mainstream anti-corrosion powder coating for conveying steel pipes. Fusion-bonded epoxy FBE is a solid coating that is transported and dispersed using air as a carrier. It is applied to the surface of preheated steel products, and after melting, leveling and curing, a uniform anti-corrosion coating is formed on the surface of steel products. The fusion-bonded epoxy powder particles uniformly contain various components, and a continuous, stable and uniform anti-corrosion coating is formed on the surface of steel products through coating operations. There is no pollution from the three wastes during the coating process, and it is a green and environmentally friendly coating.
[0004] At present, although the existing epoxy powder coating FBE has good adhesion, heat resistance, permeability resistance and insulation, the fire-fighting pipes are galvanized steel pipes. The anti-corrosion coating formed by the epoxy powder coating FBE on the galvanized steel pipes has poor water adhesion to the surface of the galvanized steel pipes, which affects its service life. In addition, the hot and cold impact resistance of the formed anti-corrosion coating needs to be further improved.
[0005] In view of the problems existing in the epoxy powder coating FBE in the above-mentioned prior art, the applicant provides an anti-corrosion powder coating for fire protection pipes and a preparation method thereof. Summary of the invention
[0006] In order to solve the above technical problems, the present application provides an anti-corrosion powder coating for fire protection pipes and a preparation method thereof.
[0007] The present application provides an anti-corrosion powder coating for fire protection pipes, which is achieved through the following technical solutions:
[0008] An anticorrosive powder coating for fire-fighting pipes, comprising an epoxy component, a polyurethane component, and a filler composition, wherein the mass ratio of the epoxy component to the polyurethane component is (60-68):(32-40); the filler composition accounts for 28-36wt% of the total mass of the anticorrosive powder coating for fire-fighting pipes;
[0009] The epoxy component comprises the following raw materials in parts by weight: 80-100 parts of an epoxy resin composition, 5-15 parts of bisphenol A epoxy acrylate, 8-15 parts of a curing agent composition, 0.5-2 parts of a curing accelerator, 1-3 parts of a leveling agent, 0.5-1 parts of an anti-aging agent, and 0.5-4 parts of a hyperbranched polyester HB-20;
[0010] The polyurethane component comprises the following raw materials in parts by weight: 25-40 parts of an aliphatic diisocyanate composition, 10-25 parts of a chain extender, 40-80 parts of a polyol, 0.05-0.12 parts of a catalyst, 0.05-0.5 parts of an initiator, 0.5-2 parts of a crosslinking agent, 0.5-2 parts of a leveling agent, and 0.5-1 parts of an anti-aging agent;
[0011] The filler composition includes at least one of calcium carbonate, kaolin, feldspar powder, barite, chopped glass fiber, alumina, white carbon black, aluminum nitride, titanium nitride, titanium oxynitride, flake graphite powder, graphene, carbon nanotubes, and nano-carbon fibers.
[0012] Preferably, the epoxy resin composition is Hexion Epikote 828 epoxy resin, Dow bisphenol A solid epoxy resin DER8230-W, Hexion bisphenol A type solid epoxy resin Epikote 1002F, Hexion bisphenol A type solid epoxy resin Epikote The invention relates to a novel epoxy resin composition comprising at least one of phthalic anhydride, maleic anhydride and dicyandiamide and at least one of 4,4'-(2,2,2-trifluoro-1-trifluoromethyl)ethylenebis(1,2-phthalic acid) and 4,4-(hexafluoroisopropylene)diphthalic anhydride; the curing accelerator is at least one of 2,4,6-tris(dimethylaminomethyl)phenol, N,N-dimethylethanolamine, resorcinol, 2-methylimidazole and 2-ethyl-4-methylimidazole; the leveling agent is at least one of BYK306 leveling agent and DOWSIL56 leveling agent.
[0013] Preferably, the preparation method of the epoxy acrylate is as follows: adding epoxy functional group-containing resin, polymerization inhibitor and antioxidant into a reaction kettle, heating to 96-98°C under nitrogen protection and a stirring speed of 200-280rpm, mixing the catalyst and acrylic resin evenly and loading them into a titration instrument, dripping the acrylic resin into the reaction kettle at a rate of 1-4g / min, and after the acrylic resin is dripped, controlling the system temperature at 104-108°C, continuing the reaction until the acid value of the system drops to 4-8mg / g, and cooling with water to room temperature to obtain the finished epoxy acrylate.
[0014] The present application adopts epoxy components, polyurethane components, and fillers to compound into an anti-corrosion powder coating, and the anti-corrosion coating for fire-fighting pipes prepared by a specific electrostatic spraying process has a strong bonding with the fire-fighting pipes, and has good resistance to cold and hot shock toughness, hydrolysis resistance, heat resistance, corrosion resistance and weather resistance, and provides long-lasting protection for fire-fighting pipes.
[0015] Preferably, the epoxy acrylate is made of epoxy functional group-containing resin, acrylic resin, inhibitor, catalyst, and antioxidant; the ratio of the molar amount of epoxy functional groups in the epoxy functional group-containing resin to the molar amount of carboxyl functional groups in the acrylic resin is 1:(1.04-1.08); the polymer resin of the epoxy matrix includes at least one of bisphenol A epoxy resin E51, bisphenol A epoxy resin E44, and 3-(perfluoro-n-hexyl)propylene oxide; the acrylic resin is at least one of acrylic acid, methacrylic acid, 2-(trifluoromethyl)acrylic acid, 4,4,4-trifluorobutenoic acid, and 2-methyl-4-trifluoromethylthiazole-5-carboxylic acid; the inhibitor is at least one of p-hydroxyanisole, 2,5-dimethylhydroquinone, and 2,6-di-tert-butyl-p-cresol; the catalyst is one of tetrabutylammonium bromide, trimethylbenzylammonium chloride, and chromium acetylacetonate.
[0016] Preferably, the epoxy component is made of the following raw materials in parts by mass: 50-60 parts of Hexion bisphenol A solid epoxy resin Epikote 1002F, 5-10 parts of polybutadiene epoxy resin with a molecular weight of 2000-5000, 5-6 parts of epoxy acrylate, 8-12 parts of maleic anhydride, 2-4 parts of dicyandiamide, 0.5-2 parts of 4,4-(hexafluoroisopropylene) diphthalic anhydride, 0.8-1.2 parts of 2,4,6-tris(dimethylaminomethyl)phenol, 0.4-0.8 parts of 2-ethyl-4-methylimidazole, 1.6-2.4 parts of BYK306 leveling agent, 0.6-0.8 parts of antioxidant 1010, 0.1-0.2 parts of antioxidant 168, and 1.2-1.6 parts of hyperbranched polyester HB-20.
[0017] By adopting the above technical scheme, introducing fluorine element into the three-dimensional network cross-linked structure formed by the epoxy composition can not only improve the heat resistance and weather resistance of the formed anti-corrosion coating, but also improve the easy cleaning performance of the surface of the anti-corrosion coating.
[0018] Preferably, the R value of the polyurethane component is 1.0-1.05, and the hard segment content is 38-48wt%; the aliphatic diisocyanate composition is at least one of IPDI, HDI, HMDI, HTDI, and TMDI; the chain extender is 1,6-hexanediol or 1,6-hexanediol combined with at least one of 1,4-butene diol, tetrafluorobutanediol, and 2,2-bis(4-hydroxycyclohexyl)hexafluoropropane; the polyol is a polycarbonate diol with a molecular weight of 1000-2000 combined with a palm oil-based polyol with a molecular weight of 2000-3000, a castor oil-based polyol with a molecular weight of 2000-3000, and a polyol with a molecular weight of 2000-2000. -3000 polytetrahydrofuran diol, adipic acid polyester diol with a molecular weight of 1000-3000, fluorinated adipic acid polyester diol with a molecular weight of 1000-3000, and a polyolefin polyol with a molecular weight of 2000-4500; the catalyst is at least one of an organic bismuth catalyst and an organic tin catalyst; the initiator is at least one of azobisisobutyronitrile and diisopropyl peroxide; the cross-linking agent is at least one of trimethylolpropane, glycerol, N,N,N',N'-tetrakis(2-hydroxyethyl)adipamide, and 3-aminopropyltrihydroxysilane; the leveling agent is at least one of BYK306 leveling agent and DOWSIL56 leveling agent.
[0019] Preferably, the R value of the polyurethane component is 1.02-1.04, and the hard segment content is 42-45wt%; the chain extender is composed of 1,6-hexanediol and 2,2-bis(4-hydroxycyclohexyl)hexafluoropropane in a molar ratio of (85-90):(10-15); the aliphatic diisocyanate composition is composed of isophorone diisocyanate IPDI and 4'-diisocyanate HMDI; the polyol is composed of polycarbonate diol with a molecular weight of 1000-2000, castor oil-based polyol with a molecular weight of 2000-3000, and polyolefin polyol with a molecular weight of 2000-4500; the catalyst is bismuth isooctanoate or stannous octoate; the initiator is azobisisobutyronitrile; and the crosslinking agent is N,N,N',N'-tetrakis(2-hydroxyethyl)adipamide or 3-aminopropyltrihydroxysilane.
[0020] By adopting the above technical solution, the thermal shock toughness and hydrolysis resistance of the formed anti-corrosion coating can be effectively improved.
[0021] Preferably, the filler composition is made of the following raw materials in percentage by mass: 0.5-2.0wt% of nano titanium nitride, 0.5-4wt% of titanium oxynitride, 1-5wt% of nano carbon fiber, 5-20wt% of white carbon black, 20-40wt% of barite powder, and the balance is ultrafine calcium carbonate.
[0022] By adopting the above technical scheme, the compactness, thermal shock toughness, hydrolysis resistance, heat resistance, corrosion resistance and weather resistance of the formed anti-corrosion coating can be effectively improved.
[0023] The present application provides a method for preparing an anti-corrosion powder coating for fire protection pipes, which is achieved by the following scheme:
[0024] A method for preparing an anticorrosive powder coating for a fire-fighting pipeline comprises the following steps:
[0025] Step 1: Modification of filler composition: Under nitrogen protection, the surface modifier and filler composition are put into a high-speed mixer and mixed at 400-800 rpm for 30-90 minutes;
[0026] Step 2, adding an acetone mixed solvent into a reaction kettle, controlling the rotation speed to 200-400rpm under nitrogen protection, adding accurately measured epoxy resin composition, polyurethane combination, defoaming agent, and surface-modified filler composition in step 1 into the reaction kettle, evacuating the kettle to a pressure of 0.04-0.08MPa after the feeding is completed, continuing to stir and defoam the mixture at 200-400rpm for 15-30min, the mass percentage of acetone mixed solvent in the obtained mixture is 40-60wt%, and after stirring and defoaming, adjusting the kettle pressure to 0.08-0.085MPa, heating to 55-60°C to remove the acetone mixed solvent in the mixture to obtain a semi-finished premixed resin material;
[0027] Step 3: under nitrogen protection, pour the semi-finished premixed resin material into a double-roll crusher for refinement, the double-roll spacing of the double-roll crusher is controlled to be 25-100 microns, the double-roll crushing temperature is controlled to be 0-10° C., and the finished premixed resin material is obtained after at least three double-roll crushings;
[0028] Step 4: Put the finished premixed resin material into a twin-screw extruder for fusion extrusion. The twin-screw extruder adopts a homogenizing section with a full 90° meshing screw, a plasticizing section temperature of 100-105°C, and a homogenizing section temperature of 118-122°C. The obtained extruded melt is cooled by a cooling roller to obtain a sheet, and the obtained sheet is input into a crushing roller for preliminary crushing to obtain a semi-finished powder coating;
[0029] Step 5: The semi-finished powder coating is ground by an ACM mill and then sieved to obtain a finished powder coating with a mesh size of ≤160.
[0030] The preparation method provided in this application is relatively simple, the investment in production equipment is relatively small, and it is easy to realize industrial production and manufacturing.
[0031] Preferably, the method further includes step six, using finished powder coating to electrostatically spray the pipeline, and the specific electrostatic spraying process is as follows: first, the steel pipe to be sprayed is surface cleaned, and the steel pipe that has completed the surface cleaning is heated to 200-220°C by a high-frequency induction coil and then enters the powder spraying workshop, the powder supply pressure is 0.05-0.06MPa, the spraying voltage is 65-70kV, the powder spraying amount is 120-150g / min, and the spraying distance is 180-240mm. After the electrostatic spraying process is completed, a 60-800 micron anti-corrosion film layer is formed on the fire-fighting pipeline, and the 95°C / 48h hot water adhesion is level 1-2; the test condition is 95°C / 25°C for 2000 cycles of cold and hot water circulation corrosion: there are no bubbles or detachment in the anti-corrosion coating.
[0032] The specific electrostatic spraying process provided in this application can ensure the quality and quality stability of the prepared anti-corrosion coating.
[0033] In summary, this application has the following advantages:
[0034] 1. This application has good resistance to cold and hot shock toughness, hydrolysis resistance, heat resistance, corrosion resistance and weather resistance, and can provide long-lasting protection for fire protection pipes.
[0035] 2. The preparation method of the anti-corrosion powder coating for fire-fighting pipes provided in this application is relatively simple, and the investment in production equipment is relatively small, which facilitates industrial production and manufacturing.
[0036] 3. The specific electrostatic spraying process provided in this application can ensure the quality and quality stability of the prepared anti-corrosion coating. DETAILED DESCRIPTION
[0037] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples and comparative examples.
[0038] Example
[0039] An anticorrosive powder coating for fire-fighting pipes includes an epoxy component, a polyurethane component, and a filler composition. The mass ratio of the epoxy component to the polyurethane component is (60-68):(32-40). Preferably, the mass ratio of the epoxy component to the polyurethane component is 65:35. The filler composition accounts for 28-36wt% of the total mass of the anticorrosive powder coating for fire-fighting pipes, and the preferred range value is 30-32wt%.
[0040] The epoxy component comprises the following raw materials in parts by weight: 60-80 parts of epoxy resin composition, 4-8 parts of epoxy acrylate, 8-20 parts of curing agent composition, 0.5-2 parts of curing accelerator, 1-3 parts of leveling agent, 0.5-1 parts of anti-aging agent and 0.5-2 parts of hyperbranched polyester HB-20.
[0041] Epoxy acrylate is made of epoxy functional group-containing resin, acrylic resin, polymerization inhibitor, catalyst, and antioxidant. The ratio of the molar amount of epoxy functional group in epoxy functional group-containing resin to the molar amount of carboxyl functional group in acrylic resin is 1: (1.04-1.08), preferably 1: (1.04-1.06). The polymer resin of epoxy matrix includes at least one of bisphenol A epoxy resin E51, bisphenol A epoxy resin E44, and 3-(perfluoro-n-hexyl) propylene oxide. Preferably, the polymer resin of epoxy matrix is composed of bisphenol A epoxy resin E44 and 3-(perfluoro-n-hexyl) propylene oxide in a molar ratio of (85-90): (10-15). The acrylic resin is at least one of acrylic acid, methacrylic acid, 2-(trifluoromethyl) acrylic acid, 4,4,4-trifluorobutylene acid, and 2-methyl-4-trifluoromethylthiazole-5-carboxylic acid. Preferably, the acrylic resin is composed of acrylic acid and 4,4,4-trifluorocrotonic acid in a molar ratio of (85-90):(10-15). The inhibitor is at least one of p-hydroxyanisole, 2,5-dimethylhydroquinone, and 2,6-di-tert-butyl-p-cresol. The inhibitor is preferably 2,5-dimethylhydroquinone. The catalyst is one of tetrabutylammonium bromide, trimethylbenzyl ammonium chloride, and chromium acetylacetonate. The catalyst is preferably tetrabutylammonium bromide.
[0042] The preparation method of epoxy acrylate is as follows: adding epoxy functional group-containing resin, polymerization inhibitor and antioxidant into a reaction kettle, heating to 96-98°C under nitrogen protection and a stirring speed of 200-280rpm, mixing the catalyst and acrylic resin evenly and loading them into a titration instrument, dripping the acrylic resin into the reaction kettle at 1-4g / min, and after the acrylic resin is dripped, controlling the system temperature at 104-108°C, continuing the reaction until the acid value of the system drops to 4-8mg / g, and cooling with water to room temperature to obtain the epoxy acrylate.
[0043] The epoxy resin composition is composed of at least one of Hexion Epikote 828 epoxy resin, Dow bisphenol A solid epoxy resin DER8230-W, Hexion bisphenol A type solid epoxy resin Epikote 1002F, Hexion bisphenol A type solid epoxy resin Epikote 1004F, Sinopec Baling Petrochemical epoxy resin CYD-014U and polybutadiene epoxy resin. Preferably, the epoxy resin composition is composed of Hexion bisphenol A type solid epoxy resin Epikote 1002F and polybutadiene epoxy resin.
[0044] The curing agent composition is at least one of phthalic anhydride, maleic anhydride, and dicyandiamide combined with at least one of 4,4'-(2,2,2-trifluoro-1-trifluoromethyl)ethylenebis(1,2-phthalic acid) and 4,4-(hexafluoroisopropylene) diphthalic anhydride. Preferably, the curing agent composition is composed of maleic anhydride, dicyandiamide, and 4,4-(hexafluoroisopropylene) diphthalic anhydride.
[0045] The curing accelerator is at least one of 2,4,6-tris(dimethylaminomethyl)phenol, N,N-dimethylethanolamine, resorcinol, 2-methylimidazole, and 2-ethyl-4-methylimidazole. Preferably, the curing accelerator is composed of 2,4,6-tris(dimethylaminomethyl)phenol and 0.4-0.8 parts of 2-ethyl-4-methylimidazole.
[0046] The leveling agent is at least one of BYK306 leveling agent and DOWSIL56 leveling agent.
[0047] The anti-aging agent is at least one of antioxidant 1010, antioxidant 1098, antioxidant BHT, antioxidant 168, UV-531, UV-P, UV-284, and UV-326.
[0048] The preferred formula is that the epoxy component includes the following raw materials in parts by mass: 50-60 parts of Hexion bisphenol A solid epoxy resin Epikote 1002F, 5-10 parts of polybutadiene epoxy resin with a molecular weight of 2000-5000, 5-6 parts of epoxy acrylate, 8-12 parts of maleic anhydride, 2-4 parts of dicyandiamide, 0.5-2 parts of 4,4-(hexafluoroisopropylene) diphthalic anhydride, 0.8-1.2 parts of 2,4,6-tris(dimethylaminomethyl)phenol, 0.4-0.8 parts of 2-ethyl-4-methylimidazole, 1.6-2.4 parts of BYK306 leveling agent, 0.6-0.8 parts of antioxidant 1010, 0.1-0.2 parts of antioxidant 168, and 1.2-1.6 parts of hyperbranched polyester HB-20.
[0049] The polyurethane component comprises the following raw materials in parts by weight: 25-40 parts of aliphatic diisocyanate composition, 10-25 parts of chain extender, 40-80 parts of polyol, 0.05-0.12 parts of catalyst, 0.05-0.5 parts of initiator, 0.5-2 parts of crosslinking agent, 0.5-2 parts of leveling agent, and 0.5-1 parts of anti-aging agent. The R value of the polyurethane component is 1.0-1.05, and the hard segment content is 38-48wt%. Preferably, the R value of the polyurethane component is 1.02-1.04, and the hard segment content is 42-45wt%.
[0050] The aliphatic diisocyanate composition is at least one of IPDI, HDI, HMDI, HTDI and TMDI. Preferably, the aliphatic diisocyanate composition is composed of isophorone diisocyanate IPDI and 4'-diisocyanate HMDI.
[0051] The chain extender is 1,6-hexanediol or 1,6-hexanediol combined with at least one of 1,4-butene glycol, tetrafluorobutanediol, and 2,2-bis(4-hydroxycyclohexyl)hexafluoropropane. Preferably, the chain extender is 1,6-hexanediol and 2,2-bis(4-hydroxycyclohexyl)hexafluoropropane in a molar ratio of (85-90):(10-15).
[0052] The polyol is composed of a polycarbonate diol with a molecular weight of 1000-2000, a palm oil-based polyol with a molecular weight of 2000-3000, a castor oil-based polyol with a molecular weight of 2000-3000, a polytetrahydrofuran diol with a molecular weight of 2000-3000, an adipic acid polyester diol with a molecular weight of 1000-3000, a fluorine-containing adipic acid polyester diol with a molecular weight of 1000-3000, and a polyolefin polyol with a molecular weight of 2000-4500.
[0053] Preferably, the polyol is composed of polycarbonate diol with a molecular weight of 1000-2000, castor oil-based polyol with a molecular weight of 2000-3000, and polyolefin polyol with a molecular weight of 2000-4500.
[0054] Preferably, the polyol is composed of polycarbonate diol with a molecular weight of 1000-2000, castor oil-based polyol with a molecular weight of 2000-3000, and hydroxyl-terminated methyl vinyl silicone oil with a molecular weight of 3000-5000.
[0055] The catalyst is at least one of an organic bismuth catalyst and an organic tin catalyst.
[0056] Preferably, the catalyst is bismuth isooctanoate or stannous octoate.
[0057] The initiator is at least one of azobisisobutyronitrile and dicumyl peroxide, preferably azobisisobutyronitrile.
[0058] The crosslinking agent is at least one of trimethylolpropane, glycerol, N,N,N',N'-tetrakis(2-hydroxyethyl)adipamide, and 3-aminopropyltrihydroxysilane. Preferably, the crosslinking agent is N,N,N',N'-tetrakis(2-hydroxyethyl)adipamide or 3-aminopropyltrihydroxysilane.
[0059] The leveling agent is at least one of BYK306 leveling agent and DOWSIL56 leveling agent.
[0060] The anti-aging agent is at least one of antioxidant 1010, antioxidant 1098, antioxidant BHT, antioxidant 168, UV-531, UV-P, UV-284, and UV-326.
[0061] The filler composition includes at least one of calcium carbonate, kaolin, feldspar powder, barite powder, chopped glass fiber, alumina, white carbon black, aluminum nitride, titanium nitride, titanium oxynitride, scalene graphite powder, graphene, carbon nanotubes, and nano-carbon fibers.
[0062] Preferably, the filler composition is made of the following raw materials in percentage by mass: 0.5-2.0wt% of nano titanium nitride, 0.5-4wt% of titanium oxynitride, 1-5wt% of nano carbon fiber, 5-20wt% of white carbon black, 20-40wt% of barite powder, and the balance is ultrafine calcium carbonate.
[0063] A method for preparing an anticorrosive powder coating for a fire-fighting pipeline comprises the following steps:
[0064] Step 1: Modification of filler composition: Under nitrogen protection, the surface modifier and filler composition are put into a high-speed mixer and mixed at 400-800 rpm for 30-90 minutes;
[0065] Step 2, adding an acetone mixed solvent into a reaction kettle, controlling the rotation speed to 200-400rpm under nitrogen protection, adding accurately measured epoxy resin composition, polyurethane combination, defoaming agent, and surface-modified filler composition in step 1 into the reaction kettle, evacuating the kettle to a pressure of 0.04-0.08MPa after the feeding is completed, continuing to stir and defoam the mixture at 200-400rpm for 15-30min, the mass percentage of acetone mixed solvent in the obtained mixture is 40-60wt%, and after stirring and defoaming, adjusting the kettle pressure to 0.08-0.085MPa, heating to 55-60°C to remove the acetone mixed solvent in the mixture to obtain a semi-finished premixed resin material;
[0066] Step 3: under nitrogen protection, pour the semi-finished premixed resin material into a double-roll crusher for refinement, the double-roll spacing of the double-roll crusher is controlled to be 25-100 microns, the double-roll crushing temperature is controlled to be 0-10° C., and the finished premixed resin material is obtained after at least three double-roll crushings;
[0067] Step 4: Put the finished premixed resin material into a twin-screw extruder for fusion extrusion. The twin-screw extruder adopts a homogenizing section with a full 90° meshing screw, a plasticizing section temperature of 100-105°C, and a homogenizing section temperature of 118-122°C. The obtained extruded melt is cooled by a cooling roller to obtain a sheet, and the obtained sheet is input into a crushing roller for preliminary crushing to obtain a semi-finished powder coating;
[0068] Step 5: The semi-finished powder coating is ground by an ACM mill and then sieved to obtain a finished powder coating with a mesh size of ≤160.
[0069] The finished powder coating prepared as above is used for electrostatic spraying of fire-fighting pipes. The specific electrostatic spraying process is as follows: first, the steel pipe to be sprayed is surface cleaned, and the steel pipe that has completed the surface cleaning is heated to 200-220°C by a frequency induction coil and then enters the powder spraying workshop. The powder supply pressure is 0.05-0.06MPa, the spraying voltage is 65-70kV, the powder spraying amount is 120-150g / min, and the spraying distance is 180-240mm. After the electrostatic spraying process is completed, a 60-800 micron anti-corrosion film layer is formed on the fire-fighting pipe, and the 95°C / 48h hot water adhesion is level 1-2; the test condition is 95°C / 25°C for 2000 cycles of cold and hot water cyclic corrosion: there are no bubbles or detachment in the anti-corrosion coating.
[0070] Preparation Example 1: Epoxy acrylate is made from 337.5 g of bisphenol A epoxy resin E51, 37.61 g of 3-(perfluoro-n-hexyl)propylene oxide, 64.85 g of acrylic acid, 14.57 g of 2-(trifluoromethyl)acrylic acid, 2 g of 2,6-di-tert-butyl-p-cresol, 3.6 g of tetrabutylammonium bromide, 3 g of antioxidant 1010, and 1 g of antioxidant 168.
[0071] Preparation method of epoxy acrylate: S1. 337.5g of bisphenol A epoxy resin E51, 37.61g of 3-(perfluoro-n-hexyl)propylene oxide, 2g of 2,6-di-tert-butyl-p-cresol, 3g of antioxidant 1010, and 1g of antioxidant 168 are added to a reactor. Under nitrogen protection and a stirring speed of 2400rpm, the temperature is raised to 97.5-98.0°C in an oil bath. 3.6g of tetrabutylammonium bromide, 64.85g of acrylic acid, and 14.57g of 2-(trifluoromethyl)acrylic acid are mixed uniformly to obtain a mixed acrylic acid liquid. The mixed acrylic acid liquid is charged into a titration instrument, and the mixed acrylic acid liquid is added dropwise to the reactor at a rate of 2g / min. After the mixed acrylic acid liquid is added dropwise, the system temperature is controlled at 104-105°C, and the reaction is continued until the acid value of the system drops to the range of 4-8mg / g, and then the system is cooled to room temperature in an ice-water bath to obtain a finished epoxy acrylate.
[0072] The difference between Preparation Example 2 and Preparation Example 1 is that the epoxy acrylate is made from 382.5 g of bisphenol A epoxy resin E44, 56.42 g of 3-(perfluoro-n-hexyl)propylene oxide, 68.87 g of methacrylic acid, 14.01 g of 2-(trifluoromethyl)acrylic acid, 21.01 g of 4,4,4-trifluorobutenoic acid, 2.4 g of 2,6-di-tert-butyl-p-cresol, 4 g of tetrabutylammonium bromide, 4 g of antioxidant 1010, and 1 g of antioxidant 168.
[0073] The difference between Preparation Example 3 and Preparation Example 1 is that epoxy acrylate is made from 396g of bisphenol A epoxy resin E44, 45.13g of 3-(perfluoro-n-hexyl)propylene oxide, 64.85g of acrylic acid, 38.01g of 2-methyl-4-trifluoromethylthiazole-5-carboxylic acid, 2.4g of 2,6-di-tert-butyl-p-cresol, 4g of tetrabutylammonium bromide, 4g of antioxidant 1010, and 1g of antioxidant 168.
[0074] The difference between Preparation Example 4 and Preparation Example 1 is that the epoxy acrylate is made from 414g of bisphenol A epoxy resin E44, 30.10g of 3-(perfluoro-n-hexyl)propylene oxide, 63.41g of acrylic acid, 11.2g of 2-(trifluoromethyl)acrylic acid, 16.90g of 2-methyl-4-trifluoromethylthiazole-5-carboxylic acid, 2.4g of 2,6-di-tert-butyl-p-cresol, 4g of tetrabutylammonium bromide, 4g of antioxidant 1010, and 1g of antioxidant 168.
[0075] The difference between Preparation Example 5 and Preparation Example 1 is that epoxy acrylate is made from 450g of bisphenol A epoxy resin E44, 57.65g of acrylic acid, 21.01g of 2-(trifluoromethyl)acrylic acid, 21.12g of 2-methyl-4-trifluoromethylthiazole-5-carboxylic acid, 2.4g of 2,6-di-tert-butyl-p-cresol, 4g of tetrabutylammonium bromide, 4g of antioxidant 1010, and 1g of antioxidant 168.
[0076] The difference between Preparation Example 6 and Preparation Example 1 is that epoxy acrylate is made from 450g of bisphenol A epoxy resin E44, 75.66g of acrylic acid, 2.4g of 2,6-di-tert-butyl-p-cresol, 4g of tetrabutylammonium bromide, 4g of antioxidant 1010, and 1g of antioxidant 168.
[0077] Example 1: An anticorrosive powder coating for fire protection pipes is prepared from 38.4 parts of an epoxy component, 25.6 parts of a polyurethane component and 36 parts of a filler composition.
[0078] The epoxy component is composed of 55 parts of Hansen bisphenol A type solid epoxy resin Epikote 1002F, 5 parts of polybutadiene epoxy resin (CAS: 129288-65-9, epoxy equivalent 220, brand: Shandong Xiju), 5 parts of epoxy acrylate in Preparation Example 1, 10 parts of maleic anhydride, 2 parts of dicyandiamide, 0.8 parts of 4,4-(hexafluoroisopropyl) diphthalic anhydride (CAS No. 1107-00-2), 0.8 parts of 2,4,6-tris(dimethylaminomethyl)phenol, 0.6 parts of 2-ethyl-4-methylimidazole, 1.5 parts of BYK306 leveling agent, 0.8 parts of antioxidant 1010, 0.2 parts of antioxidant 168, and 0.5 parts of hyperbranched polyester HB-20.
[0079] The polyurethane component is composed of 444.6 g of IPDI, 157.4 g of HMDI, 236.4 g of 1,6-hexanediol, 600 g of polycarbonate diol with a molecular weight of 2000 (Ube UH-VARB200, Mn2000), 240 g of castor oil-based polyol with a molecular weight of 2000 (Vantrus The mixture is composed of 160 g of polytetramethylene glycol (PolyTHF 2000) with a molecular weight of 2000 and 157.5 g of polyolefin polyol (Niss PB GI-3000 of Nippon Soda Co., Ltd., hydrogenated HTPB, number average molecular weight 3000), 0.42 g of bismuth isooctanoate, 0.28 g of stannous octoate, 4 g of azobisisobutyronitrile, 5 g of trimethylolpropane, 12 g of BYK306 leveling agent, 8 g of antioxidant 1098, 2 g of antioxidant BHT, 6 g of UV-531 and 4 g of UV-326.
[0080] The filler composition is prepared from 50 parts of ultrafine calcium carbonate (nano-activated calcium carbonate KY-5000, particle size 3 μm, brand, Sun Holy Fire), 30 parts of ultrafine barite powder (1250 mesh high-gloss barium sulfate, brand Hengyue), 16 parts of fumed silica (Cabot CAB-O-SIL M5, hydrophilic type), and 4 parts of nano-carbon fiber (VGCF-H powder, Showa Denko, Japan, fiber diameter 150 nm; fiber length 6 μm; aspect ratio 40).
[0081] A method for preparing an anticorrosive powder coating for a fire-fighting pipeline comprises the following steps:
[0082] Step 1: The filler composition needs to be surface modified before use: 50 parts of ultrafine calcium carbonate, 30 parts of ultrafine barite powder, 16 parts of fumed silica, and 4 parts of nano-carbon fiber are placed in a high-speed stirring kettle and dispersed at 360 rpm for 15 minutes to obtain a filler composition; 100 parts of the obtained filler composition and 2 parts of γ-glycidyloxypropyltrimethoxysilane KH-560 (CAS: 2530-83-8) and 3 parts of γ-aminopropyltriethoxysilane KH-550 (CAS: 919-30-2) are placed in a small laboratory kneader, and kneaded for 45 minutes to obtain a surface-modified filler composition;
[0083] At the same time, a polyurethane prepolymer was prepared: 444.6 g of IPDI and 157.4 g of HMDI were mixed evenly, and then the mixture was heated to 35° C., 8 g of antioxidant 1098, 2 g of antioxidant BHT, 6 g of UV-531, and 4 g of UV-326 were added and mixed evenly; 600 g of polycarbonate diol with a molecular weight of 2000 (Ube UH-VARB200, Mn2000) and 240 g of castor oil-based polyol with a molecular weight of 2000 (Vantrus) were added; Castor oil modified polyol D2000), 160g of polytetrahydrofuran diol with a molecular weight of 2000 (BASF PolyTHF 2000), 157.5g of polyolefin polyol (Niss PB GI-3000 of Japan Soda Co., Ltd., hydrogenated HTPB, number average molecular weight 3000), 0.42g of bismuth isooctanoate, stir evenly and heat to 80°C for reaction for 1h, then add 0.28g of stannous octoate and 165.2g of 1,6-hexanediol (the remaining 71.2g of 1,6-hexanediol is used as a chain extender for the second epoxy component / polyurethane component in step 2), react at 85°C for 2h to obtain a polyurethane prepolymer for standby use;
[0084] At the same time, prepare the epoxy component: 550g of Hansen bisphenol A type solid epoxy resin Epikote 1002F, 50g of polybutadiene epoxy resin with an epoxy equivalent of 220, 50g of epoxy acrylate in Preparation Example 1, 100g of maleic anhydride, 20g of dicyandiamide, 8g of 4,4-(hexafluoroisopropyl)phthalic anhydride, 8g of 2,4,6-tris(dimethylaminomethyl)phenol, 6g of 2-ethyl-4-methylimidazole, 16g of BYK306 leveling agent, 8g of antioxidant 1010, 2g of antioxidant 168, and 5g of hyperbranched polyester HB-20 are placed in a reaction kettle, and mixed evenly under nitrogen protection and at a low temperature of 4-8°C to obtain the finished epoxy component.
[0085] Step 2, add 1200g of acetone mixed solvent into the reactor, control the speed to 240rpm under nitrogen protection, weigh 384g of the finished epoxy component in step 1, 236.26g of polyurethane prepolymer, 8.74g of 1,6-hexanediol, 16g of BASF Efka PB 2001 defoamer, and 300g of the surface-modified filler composition in step 1 into the reactor, evacuate the reactor to a pressure of 0.06-0.065MPa after adding the materials, continue to stir and defoam the mixture at 240rpm for 30min, adjust the reactor pressure to 0.08-0.085MPa after the stirring and defoaming is completed, and heat to 60°C to remove the acetone mixed solvent in the mixture to obtain a semi-finished premixed resin material;
[0086] Step 3: under nitrogen protection, pour the semi-finished premixed resin material into a double-roll crusher for refinement treatment, the double-roll spacing of the double-roll crusher is controlled to be 50 μm, and the double-roll crushing temperature is controlled to be 10° C., that is, the surface temperature of the crushing roller of the double-roll crusher is 10° C. After three times of repeated double-roll crushing treatment, the finished premixed resin material is obtained;
[0087] Step 4: Put the finished premixed resin material into a twin-screw extruder for fusion extrusion. The twin-screw extruder adopts a homogenizing section with a full 90° meshing screw, a plasticizing section temperature of 105°C, and a homogenizing section temperature of 120°C. The obtained extruded melt is cooled by a cooling roller press to obtain a sheet. The obtained sheet is input into a double-roll crusher (double-roll spacing of 100 μm) for preliminary crushing to obtain a semi-finished powder coating;
[0088] Step 5: The semi-finished powder coating is ground by an ACM mill and then sieved to obtain a finished powder coating with a 325-mesh sieve.
[0089] The difference between Example 2 and Example 1 is that the anticorrosive powder coating for fire-fighting pipes is made of 45.5 parts of epoxy components, 24.5 parts of polyurethane components and 30 parts of filler composition.
[0090] The difference between Example 3 and Example 1 is that the anticorrosive powder coating for fire-fighting pipes is made of 48.9 parts of epoxy components, 23.1 parts of polyurethane components and 28 parts of filler composition.
[0091] The difference between Example 4 and Example 1 is that the epoxy component is composed of 60 parts of Hansen bisphenol A type solid epoxy resin Epikote 1002F, 5 parts of polybutadiene epoxy resin with an epoxy equivalent of 220, 5.5 parts of epoxy acrylate in Preparation Example 1, 10.6 parts of maleic anhydride, 2.4 parts of dicyandiamide, 1.6 parts of 4,4-(hexafluoroisopropyl)phthalic anhydride, 1 part of 2,4,6-tris(dimethylaminomethyl)phenol, 0.7 parts of 2-ethyl-4-methylimidazole, 2 parts of BYK306 leveling agent, 0.8 parts of antioxidant 1010, 0.2 parts of antioxidant 168, and 1 part of hyperbranched polyester HB-20.
[0092] The difference between Example 5 and Example 1 is that the epoxy component is composed of 63 parts of Hansen bisphenol A type solid epoxy resin Epikote 1002F, 7 parts of polybutadiene epoxy resin with an epoxy equivalent of 220, 5.5 parts of epoxy acrylate in Preparation Example 1, 11.2 parts of maleic anhydride, 2.5 parts of dicyandiamide, 1.8 parts of 4,4-(hexafluoroisopropyl)phthalic anhydride, 1 part of 2,4,6-tris(dimethylaminomethyl)phenol, 0.7 parts of 2-ethyl-4-methylimidazole, 2 parts of BYK306 leveling agent, 0.8 parts of antioxidant 1010, 0.2 parts of antioxidant 168, and 1 part of hyperbranched polyester HB-20.
[0093] The difference between Example 6 and Example 1 is that the epoxy component is composed of 70 parts of Hansen bisphenol A type solid epoxy resin Epikote 1002F, 10 parts of polybutadiene epoxy resin with an epoxy equivalent of 220, 6 parts of epoxy acrylate in Preparation Example 1, 12 parts of maleic anhydride, 3.2 parts of dicyandiamide, 2 parts of 4,4-(hexafluoroisopropyl)phthalic anhydride, 1.2 parts of 2,4,6-tris(dimethylaminomethyl)phenol, 0.8 parts of 2-ethyl-4-methylimidazole, 2.4 parts of BYK306 leveling agent, 1.2 parts of antioxidant 1010, 0.3 parts of antioxidant 168, and 2 parts of hyperbranched polyester HB-20.
[0094] The difference between Example 7 and Example 4 is that the epoxy component is composed of 60 parts of Hansen bisphenol A type solid epoxy resin Epikote 1002F, 5 parts of polybutadiene epoxy resin with an epoxy equivalent of 220, 5.5 parts of epoxy acrylate in Preparation Example 2, 10.6 parts of maleic anhydride, 2.4 parts of dicyandiamide, 1.6 parts of 4,4-(hexafluoroisopropyl)phthalic anhydride, 1 part of 2,4,6-tris(dimethylaminomethyl)phenol, 0.7 parts of 2-ethyl-4-methylimidazole, 2 parts of BYK306 leveling agent, 0.8 parts of antioxidant 1010, 0.2 parts of antioxidant 168, and 1 part of hyperbranched polyester HB-20.
[0095] The difference between Example 8 and Example 4 is that the epoxy component is composed of 60 parts of Hansen bisphenol A type solid epoxy resin Epikote 1002F, 5 parts of polybutadiene epoxy resin with an epoxy equivalent of 220, 5.5 parts of epoxy acrylate in Preparation Example 3, 10.6 parts of maleic anhydride, 2.4 parts of dicyandiamide, 1.6 parts of 4,4-(hexafluoroisopropyl)phthalic anhydride, 1 part of 2,4,6-tris(dimethylaminomethyl)phenol, 0.7 parts of 2-ethyl-4-methylimidazole, 2 parts of BYK306 leveling agent, 0.8 parts of antioxidant 1010, 0.2 parts of antioxidant 168, and 1 part of hyperbranched polyester HB-20.
[0096] The difference between Example 9 and Example 4 is that the epoxy component is composed of 60 parts of Hansen bisphenol A type solid epoxy resin Epikote 1002F, 5 parts of polybutadiene epoxy resin with an epoxy equivalent of 220, 5.5 parts of epoxy acrylate in Preparation Example 4, 10.6 parts of maleic anhydride, 2.4 parts of dicyandiamide, 1.6 parts of 4,4-(hexafluoroisopropyl)phthalic anhydride, 1 part of 2,4,6-tris(dimethylaminomethyl)phenol, 0.7 parts of 2-ethyl-4-methylimidazole, 2 parts of BYK306 leveling agent, 0.8 parts of antioxidant 1010, 0.2 parts of antioxidant 168, and 1 part of hyperbranched polyester HB-20.
[0097] The difference between Example 10 and Example 4 is that the epoxy component is composed of 60 parts of Hansen bisphenol A type solid epoxy resin Epikote 1002F, 5 parts of polybutadiene epoxy resin with an epoxy equivalent of 220, 5.5 parts of epoxy acrylate in Preparation Example 5, 10.6 parts of maleic anhydride, 2.4 parts of dicyandiamide, 1.6 parts of 4,4-(hexafluoroisopropyl)phthalic anhydride, 1 part of 2,4,6-tris(dimethylaminomethyl)phenol, 0.7 parts of 2-ethyl-4-methylimidazole, 2 parts of BYK306 leveling agent, 0.8 parts of antioxidant 1010, 0.2 parts of antioxidant 168, and 1 part of hyperbranched polyester HB-20.
[0098] The difference between Example 11 and Example 10 is that the epoxy component is composed of 55 parts of Dow bisphenol A solid epoxy resin DER8230-W, 5 parts of Hansen Epikote 828 epoxy resin, 5 parts of polybutadiene epoxy resin with an epoxy equivalent of 220, 5.5 parts of epoxy acrylate in Preparation Example 5, 10.6 parts of maleic anhydride, 2.4 parts of dicyandiamide, 1.6 parts of 4,4-(hexafluoroisopropyl)phthalic anhydride, 1 part of 2,4,6-tris(dimethylaminomethyl)phenol, 0.7 parts of 2-ethyl-4-methylimidazole, 2 parts of BYK306 leveling agent, 0.8 parts of antioxidant 1010, 0.2 parts of antioxidant 168, and 1 part of hyperbranched polyester HB-20.
[0099] The difference between Example 12 and Example 1 is that the polyurethane component is composed of 444.6 g of IPDI, 157.4 g of HMDI, 248.2 g of 1,6-hexanediol, 400 g of polycarbonate diol with a molecular weight of 2000 (UH-VARB200, Mn2000), 240 g of castor oil-based polyol with a molecular weight of 2000 ( The mixture is composed of 160 g of polytetramethylene glycol (PolyTHF 2000) with a molecular weight of 2000 and 157.5 g of polyolefin polyol (NissPB GI-3000 of Nippon Soda Co., Ltd., hydrogenated HTPB, number average molecular weight 3000), 0.4 g of bismuth isooctanoate, 0.25 g of stannous octoate, 3.8 g of azobisisobutyronitrile, 5.9 g of N,N,N',N'-tetrakis(2-hydroxyethyl)adipamide, 11.6 g of BYK306 leveling agent, 7.8 g of antioxidant 1098, 1.8 g of antioxidant BHT, 5.4 g of UV-531 and 3.6 g of UV-326.
[0100] The difference between Example 13 and Example 1 is that the polyurethane component is composed of 444.6 g of IPDI, 157.4 g of HMDI, 228.1 g of 1,6-hexanediol, 720 g of polycarbonate diol with a molecular weight of 2000 (Ube UH-VARB200, Mn2000), 240 g of castor oil-based polyol with a molecular weight of 2000 ( The mixture is composed of 200 g of polytetrahydrofuran diol (PolyTHF 2000) with a molecular weight of 2000 and 157.5 g of polyolefin polyol (Niss PB GI-3000 of Nippon Soda Co., Ltd., hydrogenated HTPB, number average molecular weight 3000), 0.45 g of bismuth isooctanoate, 0.3 g of stannous octoate, 4.2 g of azobisisobutyronitrile, 5.2 g of 3-aminopropyltrihydroxysilane, 12.8 g of BYK306 leveling agent, 8.6 g of antioxidant 1098, 2.4 g of antioxidant BHT, 6.4 g of UV-531 and 4.2 g of UV-326.
[0101] The difference between Example 14 and Example 1 is that the polyurethane component is composed of 444.6 g of IPDI, 157.4 g of HMDI, 218.6 g of 1,6-hexanediol, 13.22 g of 1,4-butene diol, 700 g of polycarbonate diol with a molecular weight of 2000 (Ube UH-VARB200, Mn2000), 240 g of castor oil-based polyol with a molecular weight of 2000 (Vantrus The invention comprises the following components: castor oil modified polyol D2000), 160 g of polytetramethylene glycol with a molecular weight of 2000 (BASF PolyTHF 2000), 0.40 g of bismuth isooctanoate, 0.28 g of stannous octoate, 4 g of azobisisobutyronitrile, 5 g of trimethylolpropane, 12 g of BYK306 leveling agent, 8 g of antioxidant 1098, 2 g of antioxidant BHT, 6 g of UV-531 and 4 g of UV-326.
[0102] The difference between Example 15 and Example 1 is that the polyurethane component is composed of 444.6 g of IPDI, 157.4 g of HMDI, 206.8 g of 1,6-hexanediol, 13.22 g of 1,4-butene diol, 16.2 g of tetrafluorobutanediol, 700 g of polycarbonate diol (UH-VARB200) with a molecular weight of 2000, 240 g of castor oil-based polyol ( The invention comprises the following components: castor oil modified polyol D2000), 160 g of polytetramethylene glycol (PolyTHF 2000) with a molecular weight of 2000, 0.40 g of bismuth isooctanoate, 0.28 g of stannous octoate, 4 g of azobisisobutyronitrile, 5 g of trimethylolpropane, 12 g of BYK306 leveling agent, 8 g of antioxidant 1098, 2 g of antioxidant BHT, 6 g of UV-531 and 4 g of UV-326.
[0103] The difference between Example 16 and Example 1 is that the polyurethane component is composed of 444.6 g of IPDI, 157.4 g of HMDI, 206.8 g of 1,6-hexanediol, 13.22 g of 1,4-butene diol, 34.9 g of 2,2-bis(4-hydroxycyclohexyl)hexafluoropropane, 700 g of polycarbonate diol (UH-VARB200) with a molecular weight of 2000, and 240 g of The composition comprises castor oil modified polyol D2000, 160 g of polytetrahydrofuran diol (PolyTHF 2000) with a molecular weight of 2000, 0.40 g of bismuth isooctanoate, 0.28 g of stannous octoate, 4 g of azobisisobutyronitrile, 5 g of trimethylolpropane, 12 g of BYK306 leveling agent, 8 g of antioxidant 1098, 2 g of antioxidant BHT, 6 g of UV-531 and 4 g of UV-326.
[0104] The difference between Example 17 and Example 1 is that the polyurethane component is composed of 444.6 g of IPDI, 157.4 g of HMDI, 206.8 g of 1,6-hexanediol, 13.22 g of 1,4-butene diol, 34.9 g of 2,2-bis(4-hydroxycyclohexyl)hexafluoropropane, 600 g of polycarbonate diol (UH-VARB200) with a molecular weight of 2000, and 240 g of The invention comprises castor oil modified polyol D2000, 160 g of polytetrahydrofuran diol (PolyTHF 2000) with a molecular weight of 2000, 175 g of polyolefin polyol (Niss PB GI-3000, hydrogenated HTPB, number average molecular weight of 3000), 0.45 g of bismuth isooctanoate, 0.30 g of stannous octoate, 4.5 g of azobisisobutyronitrile, 5.2 g of trimethylolpropane, 12.8 g of BYK306 leveling agent, 8.2 g of antioxidant 1098, 2.1 g of antioxidant BHT, 6.4 g of UV-531 and 4.2 g of UV-326.
[0105] The difference between Example 18 and Example 1 is that the polyurethane component is composed of 444.6 g of IPDI, 157.4 g of HMDI, 206.8 g of 1,6-hexanediol, 13.22 g of 1,4-butene diol, 34.9 g of 2,2-bis(4-hydroxycyclohexyl)hexafluoropropane, 500 g of polycarbonate diol (UH-VARB200) with a molecular weight of 2000, and 240 g of The invention comprises castor oil modified polyol D2000, 160 g of polytetrahydrofuran diol (PolyTHF 2000) with a molecular weight of 2000, 100 g of fluorinated adipic acid polyester diol with a molecular weight of 2000, 175 g of polyolefin polyol (Niss PB GI-3000, hydrogenated HTPB, number average molecular weight of 3000), 0.45 g of bismuth isooctanoate, 0.30 g of stannous octoate, 4.5 g of azobisisobutyronitrile, 5.2 g of trimethylolpropane, 12.8 g of BYK306 leveling agent, 8.2 g of antioxidant 1098, 2.1 g of antioxidant BHT, 6.4 g of UV-531 and 4.2 g of UV-326.
[0106] Preparation method of fluorinated adipic acid polyester diol with a molecular weight of 2000 (commissioned production): first, 2.0 mol of adipic acid, 0.24 mol of 2,2-bis(4-hydroxycyclohexyl)hexafluoropropane, 1.88 mol of 1,4-butanediol and 0.05 g of tetraisopropyl titanate catalyst are put into a reactor, mixed evenly and set aside; then the temperature is raised to 135°C, the esterification reaction is carried out until water is discharged, and then the temperature is raised to 228±1°C, and the acid value of the material is measured after the ester exchange reaction for 150 minutes. Regular testing was performed, with an interval of 15 minutes between two tests. When the acid value was greater than 20 mgKOH / g, the ester exchange reaction was continued for 10 minutes and the acid value was tested again. The above operation was repeated until the acid value was ≤ 20 mgKOH / g, and then vacuum was started until the gauge pressure was increased from 0.018 MPa to 0.098 MPa. After 15 minutes, the OH-value of the material was tested. The OH-value was controlled at 56 ± 3 mgKOH / g to obtain a fluorinated adipic acid-based polyester diol with a molecular weight of 2000.
[0107] The difference between Example 19 and Example 18 is that the polyurethane component is composed of 444.6 g of IPDI, 157.4 g of HMDI, 206.8 g of 1,6-hexanediol, 13.22 g of 1,4-butene diol, 34.9 g of 2,2-bis(4-hydroxycyclohexyl)hexafluoropropane, 520 g of polycarbonate diol (UH-VARB200) with a molecular weight of 2000, and 240 g of Castor oil modified polyol D2000, 160g of polytetrahydrofuran diol (PolyTHF 2000) with a molecular weight of 2000, 100g of fluorinated adipic acid polyester diol with a molecular weight of 2000, 86.4g of hydroxyl-terminated methyl vinyl silicone oil (purchased from Wuhan Huaxiang Kejie Biotechnology Co., Ltd., hydroxyl content 6±0.5% molar ratio, vinyl content 6±0.5% molar ratio, viscosity 25°C: ≤33mm 2 / s, water content ≤0.35%), 0.45g of bismuth isooctanoate, 0.30g of stannous octoate, 4.5g of azobisisobutyronitrile, 5.2g of trimethylolpropane, 12.8g of BYK306 leveling agent, 8.2g of antioxidant 1098, 2.1g of antioxidant BHT, 6.4g of UV-531, and 4.2g of UV-326.
[0108] The difference between Example 20 and Example 1 is that the filler composition is made of the following raw materials in the following mass percentages: 2wt% of nano-titanium nitride (average particle size 700nm, purchased from Wuhan Huaxiang Kejie Biotechnology Co., Ltd.), 4wt% of nano-carbon fiber, 20wt% of fumed silica CAB-O-SIL M5, 30wt% of ultrafine barite powder, and the balance is ultrafine calcium carbonate.
[0109] The difference between Example 21 and Example 1 is that the filler composition is made of the following raw materials in percentage by mass: 0.5wt% of nano titanium nitride, 2wt% of titanium oxynitride (nano titanium oxynitride, particle size 30nm, brand: Kemik), 4wt% of nano carbon fiber, 20wt% of white carbon black CAB-O-SIL M5, 30wt% of ultrafine barite powder, and the balance is ultrafine calcium carbonate.
[0110] The difference between Example 22 and Example 1 is that the filler composition is made of the following raw materials in the following mass percentages: 1wt% of nano-titanium nitride, 3wt% of titanium oxynitride, 3wt% of nano-carbon fiber, 20wt% of white carbon black CAB-O-SILM5, 30wt% of ultrafine barite powder, and the balance is ultrafine calcium carbonate.
[0111] The difference between Example 23 and Example 1 is that the filler composition is made of the following raw materials in the following mass percentages: 2.0wt% of nano-titanium nitride, 4wt% of titanium oxynitride, 3wt% of nano-carbon fibers, 20wt% of white carbon black CAB-O-SILM5, 30wt% of ultrafine barite powder, and the balance is ultrafine calcium carbonate.
[0112] The difference between Example 24 and Example 19 is that the epoxy component is composed of 60 parts of Hansen bisphenol A type solid epoxy resin Epikote 1002F, 5 parts of polybutadiene epoxy resin with an epoxy equivalent of 220, 5.5 parts of epoxy acrylate in Preparation Example 5, 10.6 parts of maleic anhydride, 2.4 parts of dicyandiamide, 1.6 parts of 4,4-(hexafluoroisopropyl)phthalic anhydride, 1 part of 2,4,6-tris(dimethylaminomethyl)phenol, 0.7 parts of 2-ethyl-4-methylimidazole, 2 parts of BYK306 leveling agent, 0.8 parts of antioxidant 1010, 0.2 parts of antioxidant 168, and 1 part of hyperbranched polyester HB-20. The filler composition is made of the following raw materials in percentage by mass: 1wt% of nano titanium nitride, 3wt% of titanium oxynitride, 3wt% of nano carbon fiber, 20wt% of white carbon black, 30wt% of barite powder, and the balance is nano calcium carbonate.
[0113] The difference between Comparative Example 1 and Example 1 is that the anticorrosive powder coating for fire-fighting pipes is made of 64 parts of epoxy components, 0 parts of polyurethane components and 36 parts of filler composition.
[0114] The difference between Comparative Example 2 and Example 1 is that the anticorrosive powder coating for fire-fighting pipes is made of 51.2 parts of epoxy components, 12.8 parts of polyurethane components and 36 parts of filler composition.
[0115] The difference between Comparative Example 3 and Example 1 is that the anticorrosive powder coating for fire-fighting pipes is made of 35.2 parts of epoxy components, 28.8 parts of polyurethane components and 36 parts of filler composition.
[0116] The difference between Comparative Example 4 and Example 1 is that the epoxy component is composed of 60 parts of Hansen bisphenol A type solid epoxy resin Epikote 1002F, 5 parts of epoxy acrylate in Preparation Example 1, 10 parts of maleic anhydride, 2.4 parts of dicyandiamide, 2 parts of dicyandiamide, 0.8 parts of 4,4-(hexafluoroisopropyl)phthalic anhydride, 0.8 parts of 2,4,6-tris(dimethylaminomethyl)phenol, 0.6 parts of 2-ethyl-4-methylimidazole, 1.5 parts of BYK306 leveling agent, 0.8 parts of antioxidant 1010, 0.2 parts of antioxidant 168, and 0.5 parts of hyperbranched polyester HB-20.
[0117] The difference between Comparative Example 5 and Example 1 is that the epoxy component is composed of 55 parts of Hansen bisphenol A type solid epoxy resin Epikote 1002F, 5 parts of polybutadiene epoxy resin with an epoxy equivalent of 220, 5 parts of epoxy acrylate in Preparation Example 1, 12.8 parts of maleic anhydride, 0.8 parts of 2,4,6-tris(dimethylaminomethyl)phenol, 0.6 parts of 2-ethyl-4-methylimidazole, 1.5 parts of BYK306 leveling agent, 0.8 parts of antioxidant 1010, 0.2 parts of antioxidant 168, and 0.5 parts of hyperbranched polyester HB-20.
[0118] The difference between Comparative Example 6 and Example 1 is that the epoxy component is composed of 55 parts of Hansen bisphenol A type solid epoxy resin Epikote 1002F, 5 parts of polybutadiene epoxy resin with an epoxy equivalent of 220, 5 parts of epoxy acrylate in Preparation Example 1, 10 parts of maleic anhydride, 2.4 parts of dicyandiamide, 2 parts of dicyandiamide, 0.8 parts of 4,4-(hexafluoroisopropyl)phthalic anhydride, 0.8 parts of 2,4,6-tris(dimethylaminomethyl)phenol, 0.6 parts of 2-ethyl-4-methylimidazole, 1.5 parts of BYK306 leveling agent, 0.8 parts of antioxidant 1010, 0.2 parts of antioxidant 168, and 0 parts of hyperbranched polyester HB-20.
[0119] The difference between Comparative Example 7 and Example 1 is that the epoxy component is composed of 55 parts of Hansen bisphenol A type solid epoxy resin Epikote 1002F, 5 parts of polybutadiene epoxy resin with an epoxy equivalent of 220, 5 parts of epoxy acrylate in Preparation Example 1, 10 parts of maleic anhydride, 2.4 parts of dicyandiamide, 2 parts of dicyandiamide, 0.8 parts of 4,4-(hexafluoroisopropyl)phthalic anhydride, 0.8 parts of 2,4,6-tris(dimethylaminomethyl)phenol, 0.6 parts of 2-ethyl-4-methylimidazole, 1.5 parts of BYK306 leveling agent, 0.8 parts of antioxidant 1010, 0.2 parts of antioxidant 168, and 0.2 parts of hyperbranched polyester HB-20.
[0120] The difference between Comparative Example 8 and Example 1 is that the epoxy component is composed of 55 parts of Hansen bisphenol A type solid epoxy resin Epikote 1002F, 5 parts of polybutadiene epoxy resin with an epoxy equivalent of 220, 5 parts of epoxy acrylate in Preparation Example 1, 10 parts of maleic anhydride, 2.4 parts of dicyandiamide, 2 parts of dicyandiamide, 0.8 parts of 4,4-(hexafluoroisopropyl)phthalic anhydride, 0.8 parts of 2,4,6-tris(dimethylaminomethyl)phenol, 0.6 parts of 2-ethyl-4-methylimidazole, 1.5 parts of BYK306 leveling agent, 0.8 parts of antioxidant 1010, 0.2 parts of antioxidant 168, and 2.5 parts of hyperbranched polyester HB-20.
[0121] The difference between Comparative Example 9 and Example 4 is that the epoxy component is composed of 60 parts of Hansen bisphenol A type solid epoxy resin Epikote 1002F, 5 parts of polybutadiene epoxy resin with an epoxy equivalent of 220, 5.5 parts of epoxy acrylate in Preparation Example 6, 10.6 parts of maleic anhydride, 2.4 parts of dicyandiamide, 1.6 parts of 4,4-(hexafluoroisopropyl)phthalic anhydride, 1 part of 2,4,6-tris(dimethylaminomethyl)phenol, 0.7 parts of 2-ethyl-4-methylimidazole, 2 parts of BYK306 leveling agent, 0.8 parts of antioxidant 1010, 0.2 parts of antioxidant 168, and 1 part of hyperbranched polyester HB-20.
[0122] The difference between Comparative Example 10 and Example 4 is that the epoxy component is composed of 65.1 parts of Hansen bisphenol A type solid epoxy resin Epikote 1002F, 5.4 parts of polybutadiene epoxy resin with an epoxy equivalent of 220, 2.4 parts of dicyandiamide, 1.6 parts of 4,4-(hexafluoroisopropyl)phthalic anhydride, 1 part of 2,4,6-tris(dimethylaminomethyl)phenol, 0.7 parts of 2-ethyl-4-methylimidazole, 2 parts of BYK306 leveling agent, 0.8 parts of antioxidant 1010, 0.2 parts of antioxidant 168, and 1 part of hyperbranched polyester HB-20.
[0123] The difference between Comparative Example 11 and Example 1 is that the polyurethane component is composed of 444.6 g of IPDI, 157.4 g of HMDI, 260 g of 1,6-hexanediol, 400 g of polycarbonate diol with a molecular weight of 2000 (UH-VARB200, Mn2000), 160 g of castor oil-based polyol with a molecular weight of 2000 ( The mixture is composed of 100 g of polytetramethylene glycol (PolyTHF 2000) with a molecular weight of 2000 and 87.5 g of polyolefin polyol (Niss PBGI-3000 of Nippon Soda Co., Ltd., hydrogenated HTPB, number average molecular weight 3000), 0.36 g of bismuth isooctanoate, 0.24 g of stannous octoate, 3.5 g of azobisisobutyronitrile, 4.6 g of N,N,N',N'-tetrakis(2-hydroxyethyl)adipamide, 10.8 g of BYK306 leveling agent, 7.5 g of antioxidant 1098, 1.5 g of antioxidant BHT, 5.2 g of UV-531 and 3.2 g of UV-326.
[0124] The difference between Comparative Example 12 and Example 1 is that the filler composition consists of 18 parts of ultrafine barite powder and 18 parts of ultrafine barite powder.
[0125] Study on the electrostatic spraying process of the above-mentioned anti-corrosion powder coating for fire protection pipelines:
[0126] Electrostatic spraying process A is as follows: first, the surface of the DN100 galvanized fire-fighting pipe to be sprayed is cleaned, and the surface oil of the galvanized fire-fighting pipe is removed by using a surfactant aqueous solution (containing 3wt% emulsifier L-548), and then wiped with an acetone aqueous solution (acetone / deionized water mixed in a volume ratio of 1:4), and then dried at 60°C after wiping. Finally, it is heated to 218°C by a frequency induction coil and then shot blasted for rust removal. The rust removal quality should meet the Sa5 / 2 level requirements specified in GB / T 8923; enter the powder spraying workshop to spray the anti-corrosion powder coating for the fire-fighting pipe in Example 1, the powder supply pressure is 0.05MPa, the spraying voltage is 70kV, the powder spraying amount is 125g / min, and the spraying distance is 200mm. After completing the electrostatic spraying process, a 500-micron anti-corrosion film layer is formed on the fire-fighting pipe.
[0127] The difference between electrostatic spraying process B and electrostatic spraying process A is as follows: enter the powder spraying workshop to spray the anti-corrosion powder coating for the fire-fighting pipe in Example 1, the powder supply pressure is 0.05MPa, the spraying voltage is 60kV, the powder spraying amount is 125g / min, the spraying distance is 200mm, and after completing the electrostatic spraying process, a 500-micron anti-corrosion film layer is formed on the fire-fighting pipe.
[0128] The difference between electrostatic spraying process C and electrostatic spraying process A is as follows: enter the powder spraying workshop to spray the anti-corrosion powder coating for the fire-fighting pipe in Example 1, the powder supply pressure is 0.06MPa, the spraying voltage is 70kV, the powder spraying amount is 125g / min, the spraying distance is 200mm, and after completing the electrostatic spraying process, a 500-micron anti-corrosion film layer is formed on the fire-fighting pipe.
[0129] The difference between electrostatic spraying process D and electrostatic spraying process A is as follows: enter the powder spraying workshop to spray the anti-corrosion powder coating for the fire-fighting pipe in Example 1, the powder supply pressure is 0.05MPa, the spraying voltage is 70kV, the powder spraying amount is 150g / min, the spraying distance is 200mm, and after completing the electrostatic spraying process, a 500-micron anti-corrosion film layer is formed on the fire-fighting pipe.
[0130] The difference between electrostatic spraying process E and electrostatic spraying process A is as follows: enter the powder spraying workshop to spray the anti-corrosion powder coating for the fire-fighting pipe in Example 1, the powder supply pressure is 0.05MPa, the spraying voltage is 70kV, the powder spraying amount is 125g / min, and the spraying distance is 240mm. After completing the electrostatic spraying process, a 500-micron anti-corrosion film layer is formed on the fire-fighting pipe.
[0131] The difference between electrostatic spraying process F and electrostatic spraying process A is as follows: first, the surface of the DN100 galvanized fire protection pipe to be sprayed is cleaned, and the surface oil of the galvanized fire protection pipe is removed by using a surfactant aqueous solution (containing 3wt% emulsifier L-548), and then wiped with an acetone aqueous solution (acetone / deionized water volume ratio of 1:4). After wiping, it is dried at 60°C, and finally heated to 200°C by a high-frequency induction coil for shot blasting and rust removal. The rust removal quality should meet the Sa5 / 2 level requirements specified in GB / T 8923.
[0132] The difference between electrostatic spraying process G and electrostatic spraying process A is as follows: first, the surface of the DN100 galvanized fire-fighting pipe to be sprayed is cleaned, and the surface oil of the galvanized fire-fighting pipe is removed with a surfactant aqueous solution (containing 3wt% emulsifier L-548) and then wiped with an acetone aqueous solution (acetone / deionized water mixed in a volume ratio of 1:4). After wiping, it is dried at 60°C, and finally heated to 210°C by a high-frequency induction coil for shot blasting and rust removal. The rust removal quality should meet the Sa5 / 2 level requirements specified in GB / T 8923.
[0133] Performance test: 1. Neutral salt spray resistance and salt water resistance tests are measured in accordance with GB / T 1771-2007. 2. Bending toughness test method: According to the requirements of "SY / T 0315-2013 Technical Specifications for Fusion Bonded Epoxy Powder External Coatings of Steel Pipelines", the formed anti-corrosion coating is subjected to bending test at -30℃ / 3°. 3. 30d cathodic stripping performance test is carried out in accordance with the requirements of "SY / T0315-2013 Technical Specifications for Fusion Bonded Epoxy Powder External Coatings of Steel Pipelines", the test conditions are 70±2℃ / 1.5V, and the qualified standard is the final stripping ([(70±2℃) / 1.5V] / mm) result <18mm. 4. Hot water adhesion: Tested in accordance with CJ / T120-2016, test conditions: 95℃ hot water constant temperature for 48h. 5. Impact resistance: Tested in accordance with GB / T1732-2020 coating impact resistance determination method, test standard ≥50cm. 6. Hot and cold water cycle corrosion: refer to the test method in BSEN877-1999 for testing. The test conditions are 95℃ / 25℃ cycle for 2000 cycles. One cycle of alternating hot and cold water is 93℃ hot water for 1min + drainage for 1min + 25℃ cold water for 1min + drainage for 1min. Observe whether there is any peeling or bubbles on the surface.
[0134] Table 1: Test parameters of anti-corrosion coatings made by electrostatic spraying AG process for anti-corrosion powder coatings for fire protection pipes
[0135]
[0136] Combined with Table 1, it can be seen that the comprehensive performance and energy consumption of the anti-corrosion coating prepared by the electrostatic spraying process A are better. The anti-corrosion coating experimental samples 1-24 and the anti-corrosion coating comparative samples 1-12 were prepared by using the electrostatic spraying process A in combination with the anti-corrosion powder coating for fire protection pipes in Examples 1-24 and Comparative Examples 1-12, and performance tests were performed. The test parameters are shown in Table 2:
[0137] Table 2: Test parameters of anticorrosive powder coatings for fire protection pipes in Examples 1-24 and Comparative Examples 1-12
[0138]
[0139]
[0140] It can be seen from the combination of Examples 1-3 and Comparative Examples 1-3 and Table 2 that the appropriate addition of the polyurethane component can improve the anti-cold and hot shock toughness, impact resistance and adhesion performance of the anti-corrosion coating to the galvanized fire-fighting pipe. In the pilot experiment, it was found that the increase in the amount of the filler composition required the addition of more polyurethane components to improve the overall anti-cold and hot shock toughness, impact resistance and adhesion performance of the galvanized fire-fighting pipe. When the amount of the filler composition added>36wt%, the amount of the polyurethane component added must be above 26wt%, but the anti-cold and hot shock toughness of the anti-corrosion coating finally formed had a small amount of bubbles and the hot water adhesion dropped to level 2. Preferably, the mass ratio of the epoxy component to the polyurethane component is (60-68): (32-40). Preferably, the filler composition accounts for 28-36wt% of the total mass of the anti-corrosion powder coating for fire-fighting pipes.
[0141] Combining Examples 1-6 and Comparative Examples 4-8 with Table 2, it can be seen that the addition of polybutadiene epoxy resin can improve the impact resistance of the anti-corrosion coating. And by comparing Example 1 with Comparative Example 5, it can be seen that the curing agent composition formed by compounding 4,4'-(2,2,2-trifluoro-1-trifluoromethyl)ethylenebis(1,2-phthalic acid), dicyandiamide and maleic anhydride can improve the salt water resistance of the anti-corrosion coating.
[0142] Combining Example 1 and Comparative Examples 6-7 with Table 1, it can be seen that the addition of hyperbranched polyester HB-20 can improve the adhesion performance of the interface between the anti-corrosion coating and the galvanized steel pipe, and excessive addition will increase the overall cross-linking density and lead to a decrease in impact resistance.
[0143] It can be seen from Example 4 and Comparative Examples 9-10 and Table 1 that the anti-corrosion coating prepared using the epoxy acrylate in Preparation Examples 1-5 of the present application has relatively good adhesion performance with the galvanized steel pipe interface and better corrosion resistance.
[0144] Combining Example 1, Examples 12-19 and Comparative Example 11 and Table 1, it can be seen that the adhesion performance and impact resistance of the anti-corrosion coating prepared by the polyurethane components in Examples 1 and Examples 12-18 and the galvanized steel pipe interface are relatively good. In Comparative Example 11, at a high amount of filler composition added, the high hard segment content of the polyurethane component affects the impact resistance. In the experimental pilot stage, Example 19 and Example 18 found that the polyurethane molecular chain network structure containing a hydroxyl-terminated methyl vinyl silicone oil segment structure can improve the glass transition temperature Tg of the formed anti-corrosion coating, that is, the glass transition temperature Tg of the anti-corrosion coating of Example 19 is greater than the glass transition temperature Tg of the anti-corrosion coating of Example 18, and the anti-cold and hot impact toughness, hydrolysis resistance, heat resistance, corrosion resistance, and weather resistance of the anti-corrosion coating of Example 19 also meet the standards.
[0145] It can be seen from Example 1 and Examples 20-24 and Comparative Example 12 and Table 1 that the addition of nano-carbon fibers can improve the impact resistance and salt corrosion resistance of the formed anti-corrosion coating. The addition amount of nano-carbon fibers should be 3-5wt% of the filler composition. Too much addition will make the production cost high.
[0146] From Example 1 and Examples 20-24 and Comparative Example 12 and Table 1, it can be seen that the addition of nano-titanium nitride and / or titanium oxynitride plays a role in toughening and strengthening, and can reduce the amount of nano-carbon fiber added. On the premise of ensuring that the comprehensive performance of the anti-corrosion coating meets the standards, the production cost of the filler composition can be optimized, and the anti-corrosion coating can be given good surface cleanability.
[0147] In summary, the anti-corrosion coating for fire-fighting pipes prepared by compounding an epoxy component, a polyurethane component, and a filler combination and combining it with a specific electrostatic spraying process contains an IPN structure and has excellent adhesion performance with galvanized fire-fighting pipes, and has good resistance to cold and hot shock toughness, hydrolysis resistance, heat resistance, corrosion resistance and weather resistance, and can provide long-lasting protection for fire-fighting pipes.
[0148] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. An anticorrosive powder coating for fire protection pipes, characterized in that: The anti-corrosion powder coating for fire-fighting pipes comprises an epoxy component, a polyurethane component and a filler composition, wherein the mass ratio of the epoxy component to the polyurethane component is (60-68):(32-40); the filler composition accounts for 28-36wt% of the total mass of the anti-corrosion powder coating for fire-fighting pipes; The epoxy component comprises the following raw materials in parts by weight: 60-80 parts of an epoxy resin composition, 4-8 parts of epoxy acrylate, 8-20 parts of a curing agent composition, 0.5-2 parts of a curing accelerator, 1-3 parts of a leveling agent, 0.5-1 parts of an anti-aging agent, and 0.5-2 parts of a hyperbranched polyester HB-20; The epoxy resin composition is composed of at least one of Hexion Epikote 828 epoxy resin, Dow bisphenol A solid epoxy resin DER8230-W, Hexion bisphenol A solid epoxy resin Epikote 1002F, Hexion bisphenol A solid epoxy resin Epikote 1004F, Sinopec Baling Petrochemical epoxy resin CYD-014U and polybutadiene epoxy resin with a molecular weight of 2000-5000; the curing agent composition is phthalic anhydride, maleic anhydride, dicyandiamide At least one of the amines is combined with at least one of 4,4'-(2,2,2-trifluoro-1-trifluoromethyl)ethylenebis(1,2-phthalic acid) and 4,4-(hexafluoroisopropylene)diphthalic anhydride; the curing accelerator is at least one of 2,4,6-tris(dimethylaminomethyl)phenol, N,N-dimethylethanolamine, resorcinol, 2-methylimidazole, and 2-ethyl-4-methylimidazole; the leveling agent is at least one of BYK306 leveling agent and DOWSIL56 leveling agent; The epoxy acrylate is made of epoxy functional group-containing resin, acrylic resin, polymerization inhibitor, catalyst and antioxidant; the ratio of the molar amount of epoxy functional group in the epoxy functional group-containing resin to the molar amount of carboxyl functional group in the acrylic resin is 1:(1.04-1.08); the epoxy functional group-containing resin includes at least one of bisphenol A epoxy resin E51, bisphenol A epoxy resin E44 and 3-(perfluoro-n-hexyl)propylene oxide; the acrylic resin is at least one of acrylic acid, methacrylic acid, 2-(trifluoromethyl)acrylic acid, 4,4,4-trifluorobutenoic acid and 2-methyl-4-trifluoromethylthiazole-5-carboxylic acid; the polymerization inhibitor is at least one of p-hydroxyanisole, 2,5-dimethylhydroquinone and 2,6-di-tert-butyl-p-cresol; the catalyst is one of tetrabutylammonium bromide, trimethylbenzylammonium chloride and chromium acetylacetonate; The polyurethane component comprises the following raw materials in parts by weight: 25-40 parts of an aliphatic diisocyanate composition, 10-25 parts of a chain extender, 40-80 parts of a polyol, 0.05-0.12 parts of a catalyst, 0.05-0.5 parts of an initiator, 0.5-2 parts of a crosslinking agent, 0.5-2 parts of a leveling agent, and 0.5-1 parts of an anti-aging agent; The filler composition is made of the following raw materials in percentage by mass: 0.5-2.0 wt% of nano titanium nitride, 0.5-4 wt% of titanium oxynitride, 1-5 wt% of nano carbon fiber, 5-20 wt% of white carbon black, 20-40 wt% of barite powder, and the balance is nano calcium carbonate.
2. The anticorrosive powder coating for fire protection pipes according to claim 1, characterized in that: The preparation method of epoxy acrylate is as follows: adding epoxy functional group-containing resin, polymerization inhibitor and antioxidant into a reaction kettle, heating to 96-98°C under nitrogen protection and a stirring speed of 200-280rpm, mixing a catalyst and an acrylic resin evenly and loading them into a titration instrument, dripping the acrylic resin into the reaction kettle at a rate of 1-4g / min, and after the acrylic resin is dripped, controlling the system temperature at 104-108°C, continuing the reaction until the acid value of the system drops to 4-8mg / g, and cooling with water to room temperature to obtain the finished epoxy acrylate.
3. The anticorrosive powder coating for fire protection pipes according to claim 2, characterized in that: The epoxy component includes the following raw materials in parts by weight: 50-60 parts of Hansen bisphenol A solid epoxy resin Epikote1002F, 5-10 parts of polybutadiene epoxy resin with a molecular weight of 2000-5000, 5-6 parts of epoxy acrylate, 8-12 parts of maleic anhydride, 2-4 parts of dicyandiamide, 0.5-2 parts of 4,4-(hexafluoroisopropylene) diphthalic anhydride, 0.8-1.2 parts of 2,4,6-tris(dimethylaminomethyl)phenol, 0.4-0.8 parts of 2-ethyl-4-methylimidazole, 1.6-2.4 parts of BYK306 leveling agent, 0.6-0.8 parts of anti-aging agent 1010, 0.1-0.2 parts of anti-aging agent 168, and 1.2-1.6 parts of hyperbranched polyester HB-20.
4. The anticorrosive powder coating for fire protection pipes according to claim 1, characterized in that: The R value of the polyurethane component is 1.0-1.05, and the hard segment content is 38-48wt%; the aliphatic diisocyanate composition is at least one of IPDI, HDI, HMDI, HTDI, and TMDI; the chain extender is 1,6-hexanediol or 1,6-hexanediol combined with at least one of 1,4-butene diol, tetrafluorobutanediol, and 2,2-bis(4-hydroxycyclohexyl)hexafluoropropane; the polyol is a polycarbonate diol with a molecular weight of 1000-2000 combined with a palm oil-based polyol with a molecular weight of 2000-3000, a castor oil-based polyol with a molecular weight of 2000-3000, and a polyol with a molecular weight of 2000-3000. The invention relates to a polytetramethyleneimine glycol having a molecular weight of 1000-3000, adipic acid polyester diol having a molecular weight of 1000-3000, a fluorinated adipic acid polyester diol having a molecular weight of 1000-3000, and a polyolefin polyol having a molecular weight of 2000-4500; the catalyst is at least one of an organic bismuth catalyst and an organic tin catalyst; the initiator is at least one of azobisisobutyronitrile and diisopropyl peroxide; the cross-linking agent is at least one of trimethylolpropane, glycerol, N,N,N',N'-tetrakis(2-hydroxyethyl)adipamide and 3-aminopropyltrihydroxysilane; the leveling agent is at least one of BYK306 leveling agent and DOWSIL56 leveling agent.
5. The anticorrosive powder coating for fire protection pipes according to claim 4, characterized in that: The R value of the polyurethane component is 1.02-1.04, and the hard segment content is 42-45wt%; the chain extender is composed of 1,6-hexanediol and 2,2-bis(4-hydroxycyclohexyl)hexafluoropropane in a molar ratio of (85-90):(10-15); the aliphatic diisocyanate composition is composed of isophorone diisocyanate IPDI and 4,4'-dicyclohexylmethane diisocyanate HMDI; the polyol is composed of polycarbonate diol with a molecular weight of 1000-2000, castor oil-based polyol with a molecular weight of 2000-3000, and polyolefin polyol with a molecular weight of 2000-4500; the catalyst is bismuth isooctanoate or stannous octoate; the initiator is azobisisobutyronitrile; and the crosslinking agent is N,N,N',N'-tetrakis(2-hydroxyethyl)adipamide or 3-aminopropyltrihydroxysilane.
6. A method for preparing an anticorrosive powder coating for fire protection pipes according to any one of claims 1 to 5, characterized in that: The following steps are involved: Step 1: Modification of filler composition: Under nitrogen protection, the surface modifier and filler composition are put into a high-speed mixer and mixed at 400-800 rpm for 30-90 minutes; Step 2, adding an acetone mixed solvent into a reactor, controlling the rotation speed to 200-400rpm under nitrogen protection, adding accurately measured epoxy resin composition, polyurethane combination, defoaming agent, and surface-modified filler composition in step 1 into the reactor, evacuating the reactor to a pressure of 0.04-0.08MPa after the feeding is completed, continuing to stir and defoam the mixture at 200-400rpm for 15-30min, the mass percentage of acetone mixed solvent in the obtained mixture is 40-60wt%, and after stirring and defoaming, adjusting the reactor pressure to 0.08-0.085MPa, heating to 55-60°C to remove the acetone mixed solvent in the mixture to obtain a semi-finished premixed resin material; Step 3: under nitrogen protection, pour the semi-finished premixed resin material into a double-roll crusher for refinement, the double-roll spacing of the double-roll crusher is controlled to be 25-100 microns, the double-roll crushing temperature is controlled to be 0-10°C, and the finished premixed resin material is obtained after at least three double-roll crushings; Step 4: put the finished premixed resin material into a twin-screw extruder for fusion extrusion, the twin-screw extruder adopts a homogenizing section with a full 90° meshing screw, a plasticizing section temperature of 100-105°C, and a homogenizing section temperature of 118-122°C, the obtained extruded melt is cooled by a cooling roller to obtain a sheet, and the obtained sheet is input into a crushing roller for preliminary crushing to obtain a semi-finished powder coating; Step 5: The semi-finished powder coating is ground by an ACM mill and then sieved to obtain a finished powder coating with a mesh size of ≤160.
7. The method for preparing an anticorrosive powder coating for fire protection pipes according to claim 6, characterized in that: It also includes step six, using finished powder coating to electrostatically spray the pipeline, and the specific electrostatic spraying process is as follows: first, the steel pipe to be sprayed is surface cleaned, and the steel pipe that has completed the surface cleaning is heated to 200-220°C by a high-frequency induction coil and then enters the powder spraying workshop, the powder supply pressure is 0.05-0.06MPa, the spraying voltage is 65-70kV, the powder spraying amount is 120-150g / min, and the spraying distance is 180-240mm. After the electrostatic spraying process is completed, a 60-800 micron anti-corrosion film layer is formed on the fire-fighting pipeline, and the 95°C / 48h hot water adhesion is level 1-2; the test condition is 95°C / 25°C for 2000 cycles of cold and hot water circulation corrosion: there are no bubbles or detachment in the anti-corrosion coating.