A bio-based polylactic acid tape and preparation method thereof
Biaxially stretched polylactic acid film is prepared through a three-layer co-extrusion process and coated with polylactic acid adhesive, which solves the environmental pollution problem of traditional tapes and achieves a bio-based polylactic acid tape with high biodegradability and excellent physical properties, suitable for a variety of applications field.
Patent Information
- Application Number
- CN202411086145.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-08-08
AI Technical Summary
Traditional tapes use petroleum-based materials, which leads to a high risk of environmental pollution. There are few studies on polylactic acid as an adhesive material, and there is a lack of reports on tapes with bio-based polylactic acid as the main component.
A three-layer co-extrusion process is used to prepare a biaxially stretched polylactic acid film as the tape base material, and polylactic acid adhesive is coated on it. Polylactic acid-grafted polyether silicone oil is used as a release agent, and the grafting rate is increased through gamma ray irradiation. Reduces viscosity and migration capabilities to create a highly biodegradable tape.
The high biodegradability and excellent physical properties of the tape are achieved, reducing the risk of environmental pollution and being suitable for a wider range of application fields, such as electronics, medical and express packaging.
Smart Images

Figure CN118599441B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of bio-based adhesive material preparation, and more specifically, relates to a bio-based polylactic acid tape and a preparation method thereof. Background Art
[0002] Traditional adhesive tapes are usually made of petroleum-based materials, which have certain environmental pollution risks. Therefore, researchers are committed to developing a bio-based tape to improve the biodegradability of the tape and thus reduce the risk of environmental pollution.
[0003] In recent years, great progress has been made in the application of polylactic acid in the production of biaxially oriented polylactic acid (BOPLA) films as tape substrates, while coating adhesives are still mainly acrylic materials. Although research on acrylic adhesives partially replaced by bio-based monomers has also been carried out, research on polylactic acid as an adhesive material is relatively rare, and there is currently no report on tapes with both the tape substrate and adhesive using bio-based polylactic acid as the main component. Summary of the invention
[0004] The purpose of the present invention is to provide a bio-based polylactic acid tape and a preparation method thereof, wherein the tape substrate and adhesive of the tape are both based on bio-based polylactic acid as the main component, so that the tape has a high biodegradability rate, thereby reducing the risk of environmental pollution. At the same time, the prepared polylactic acid tape has excellent physical properties and appearance, making it suitable for a wider range of applications.
[0005] To achieve the above-mentioned object, the first aspect of the present invention provides a bio-based polylactic acid tape, comprising a tape substrate and a polylactic acid adhesive layer coated on the surface of the tape substrate;
[0006] The tape substrate comprises an inner layer, an intermediate layer and an outer surface layer stacked in sequence; the inner layer contains polylactic acid, an opening agent and a lubricant; the intermediate layer contains only polylactic acid; the outer surface layer contains polylactic acid, an opening agent, a lubricant and a release agent;
[0007] The polylactic acid adhesive layer is coated on the inner layer.
[0008] Furthermore, the release agent is polylactic acid grafted polyether silicone oil; the polyether silicone oil is a polyether silicone oil containing epoxy functional groups, and its viscosity is 100~400 mPa.S.
[0009] Furthermore, the polylactic acid grafted polyether silicone oil is prepared by the following method: polylactic acid, polyether silicone oil and a catalyst are uniformly mixed, and then extruded and granulated by a twin-screw extruder.
[0010] Furthermore, the method further comprises the step of irradiating the polylactic acid grafted polyether silicone oil after extrusion and granulation, wherein the irradiation conditions are: 50 KGy absorbed dose, and γ-ray irradiation for 15 to 20 hours.
[0011] Furthermore, the mass ratio of polyether silicone oil to polylactic acid is 3-5:95-97, the catalyst is BIBP (di-tert-butyl peroxide isopropylbenzene), the amount of the catalyst added is 0.1-0.3wt%, and the operating temperature of the twin-screw extruder is 150-220°C.
[0012] Furthermore, in the inner layer, the net contents of the opening agent and the lubricant are 250-500 ppm and 1000-3000 ppm respectively; in the outer surface layer, the net contents of the opening agent, the lubricant and the release agent are 250-1000 ppm, 10000-20000 ppm and 3000-5000 ppm respectively.
[0013] Furthermore, the polylactic acid adhesive layer has two glass transition temperatures of -40 to -30°C and 35 to 45°C.
[0014] Furthermore, the polylactic acid adhesive layer is prepared using caprolactone and lactide as raw materials, and the molar ratio of caprolactone to lactide is 20-75:25-80.
[0015] Furthermore, the weight average molecular weight of the polylactic acid in the inner layer, the middle layer and the outer surface layer is greater than 200,000, the polydispersity index is less than 1.6, and the melting point is 155-180°C.
[0016] A second aspect of the present invention provides a method for preparing a bio-based polylactic acid tape, comprising the following steps:
[0017] The raw materials of the inner layer, the middle layer and the outer surface layer are melted and co-extruded to obtain a cast sheet;
[0018] The cast sheet is longitudinally stretched and transversely stretched to obtain a polylactic acid film;
[0019] The polylactic acid film is unwound and coated by a coating machine, the polylactic acid film is used as a tape substrate, a polylactic acid adhesive is coated on the inner layer thereof, and the film is slit after being rolled up to obtain a bio-based polylactic acid tape.
[0020] Compared with the prior art, the present invention has the following technical effects:
[0021] The tape substrate and adhesive of the bio-based polylactic acid tape of the present invention are both based on bio-based polylactic acid as the main component, which can be naturally biodegraded, has a high biodegradability rate, and reduces the risk of environmental pollution. At the same time, the polylactic acid tape of the present invention has excellent physical properties and appearance, making it suitable for a wider range of application fields.
[0022] The method for preparing a bio-based polylactic acid tape of the present invention prepares a biaxially stretched polylactic acid film with single-side release by a three-layer co-extrusion method, and then obtains the bio-based polylactic acid tape by coating a polylactic acid adhesive on the polylactic acid film. The method of the present invention can effectively utilize bio-based materials to prepare high-quality polylactic acid tapes, and the prepared tapes have excellent physical properties and biodegradability, and can be widely used in the fields of electronics, medical treatment, and express packaging. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0024] Figure 1 This is a comparison chart of the relative decomposition rates of the bio-based polylactic acid tape prepared in Example 9 of the present invention and microcrystalline cellulose. DETAILED DESCRIPTION
[0025] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0026] The terms used in the embodiments of the present invention are only for the purpose of describing specific embodiments, and are not intended to limit the present invention. The singular forms "a", "said" and "the" used in the embodiments of the present invention and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0027] The weight of the relevant components mentioned in the description of the embodiments of the present invention may not only refer to the specific content of each component, but also indicate the weight ratio between the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the description of the embodiments of the present invention, it is within the scope disclosed in the description of the embodiments of the present invention. Specifically, the mass described in the description of the embodiments of the present invention may be a mass unit known in the chemical industry such as µg, mg, g, kg, etc.
[0028] The embodiment of the present invention provides a bio-based polylactic acid tape and a preparation method thereof, wherein the bio-based polylactic acid tape comprises a tape substrate and a polylactic acid adhesive layer coated on the surface of the tape substrate. The tape substrate comprises an inner layer, an intermediate layer and an outer surface layer stacked in sequence; the inner layer contains polylactic acid, an opening agent and a lubricant; the intermediate layer contains only polylactic acid; the outer surface layer contains polylactic acid, an opening agent, a lubricant and a release agent; and the polylactic acid adhesive layer is coated on the inner layer.
[0029] The tape substrate of the embodiment of the present invention is composed of an inner layer, an intermediate layer and an outer surface layer stacked in sequence, and the outer surface layer contains a release agent, so that a release surface is formed on the surface of the outer surface layer, so that the tape substrate of the embodiment of the present invention does not need to be brushed with a release agent on its surface when in use, which can simplify the process of applying the release agent.
[0030] The tape substrate and adhesive of the bio-based polylactic acid tape of the embodiment of the present invention both use bio-based polylactic acid as the main component, are naturally biodegradable, have a high biodegradability rate, and reduce the risk of environmental pollution.
[0031] During the storage of the tape, the release agent used conventionally will gradually migrate from the outer surface layer to the adhesive layer in contact with it, which will cause a certain amount of release agent to be contained in the adhesive layer. The migration of the release agent to the adhesive layer will affect the adhesive properties of the tape, resulting in a decrease in the peel strength of the tape when used. On the other hand, if the release agent in the outer surface layer is missing, the adhesive surface and the back of the winding tape are prone to adhesion, which increases the release force of the tape and is not conducive to the slitting and use of the tape.
[0032] Therefore, the release agent used in the embodiment of the present invention is a homemade polylactic acid grafted polyether silicone oil, and the polyether silicone oil is a polyether silicone oil containing epoxy functional groups, and its viscosity is 100-400 mPa.S. By grafting the polyether silicone oil onto the polylactic acid, the migration ability of the polyether silicone oil on the outer surface layer is reduced, thereby improving the bonding performance of the adhesive layer of the prepared tape and reducing the release force of the tape.
[0033] The polylactic acid grafted polyether silicone oil of the embodiment of the present invention is prepared by the following method: polylactic acid, polyether silicone oil, and catalyst are mixed in a certain proportion and then extruded and granulated by a twin-screw extruder. The temperature of the grafting reaction of polyether silicone oil and polylactic acid is 150~220 ℃, so the working temperature of the twin-screw extruder is set to 150~220 ℃ in the embodiment of the present invention. The catalyst is commercially available BIBP, which has a half-life of 1 min at 182 ℃. Specifically, the mass ratio of polyether silicone oil to polylactic acid can be 3~5:95~97, and the amount of catalyst added can be 0.1~0.3wt%.
[0034] In addition, the inventors of the present invention unexpectedly discovered that placing the polylactic acid grafted polyether silicone oil prepared by the twin-screw reactive extrusion method under irradiation conditions can further improve the grafting rate of the polyether silicone oil on the polylactic acid. The higher the grafting rate, the lower the migration ability of the polylactic acid grafted polyether silicone oil in the outer surface layer, which is more conducive to improving the bonding performance of the adhesive layer of the tape, and makes the release force of the tape smaller, and the adhesive surface and the back of the tape are less likely to be adhered, which is more convenient to use. The preferred irradiation conditions are: 50 KGy absorbed dose, γ-ray irradiation for 15 to 20 hours, for example, irradiation for 17 hours.
[0035] In the embodiment of the present invention, the tape substrate is prepared by a three-layer co-extrusion process and a biaxial stretching process. In the inner layer of the tape substrate, the net contents of the opening agent and the lubricant are 250-500 ppm and 1000-3000 ppm respectively; in the outer surface layer of the tape substrate, the net contents of the opening agent, the lubricant and the release agent are 250-1000 ppm, 10000-20000 ppm and 3000-5000 ppm respectively. By controlling the content of each component in the inner layer and the outer surface layer of the tape substrate, and selecting polylactic acid with a weight average molecular weight greater than 200,000, a polydispersity index less than 1.6 and a melting point of 155-180 ° C as the main component of each layer, the film stability requirements of asynchronous stretching (3 times longitudinal stretching and 4 times transverse stretching) or synchronous stretching (4 times longitudinal stretching and 3 times transverse stretching) are met, and finally the tape substrate has excellent physical properties and appearance, making it suitable for a wider range of applications. In addition, polylactic acid raw materials with different melting points can be matched to have different crystallinity, and the optical and mechanical properties of the biaxially stretched film can be balanced by adjusting the crystallinity.
[0036] In the three-layer co-extrusion process, the flow rate of the raw material melt is controlled to be 3-4 g / 10 min (190 ° C) to ensure the stability of the three-layer composite melt during the three-layer co-extrusion. The moisture content of the raw material melt is an important factor affecting the stability of processing and product quality. The embodiment of the present invention controls the moisture content of the raw material melt to be less than 300 ppm, and the moisture content can be achieved through pre-drying or online drying system.
[0037] The polylactic acid adhesive layer of the embodiment of the present invention has two glass transition temperatures of -40~-30 ℃ and 35~45 ℃ to realize the pressure-sensitive properties of the material. The polylactic acid adhesive layer of the embodiment of the present invention is made of caprolactone and lactide as raw materials, and two copolymers with glass transition temperatures of -40~-30 ℃ and 35~45 ℃ are prepared respectively, and then the two copolymers are melt-blended as pressure-sensitive adhesives. In these two copolymers, the molar ratio of caprolactone and lactide is 20~75:25~80. The copolymer has excellent fluidity after melting, which can meet the requirements of uniform coating and stability. The peel strength of the copolymer of the embodiment of the present invention is greater than 1200 g / 25 mm, the initial ring adhesion is greater than 5.5 N, and the lasting adhesion is greater than 24 hours.
[0038] A bio-based polylactic acid tape and a preparation method thereof according to an embodiment of the present invention are illustrated below through a plurality of specific embodiments.
[0039] Example 1
[0040] Embodiment 1 of the present invention provides a tape substrate (biaxially oriented polylactic acid film, i.e., BOPLA release film) and a preparation method thereof, comprising the following steps:
[0041] (1) Prepared by abc three-layer co-extrusion method: a layer (inner layer) is mainly made of polylactic acid, and the net contents of the anti-blocking agent and the lubricant in the a layer are 250 ppm and 1500 ppm respectively; b layer (middle layer) is made of pure polylactic acid raw material, which can be commercially available Fengyuan 801 (FY801) or Fengyuan 802 (FY802) etc.; c layer (outer surface layer) is mainly made of polylactic acid, and the net contents of the anti-blocking agent, the lubricant and the release agent in the c layer are 500 ppm, 20000 ppm and 3000 ppm respectively. The anti-blocking agent used is D 50 The particle size of the polymethylsilsesquioxane used is 4.5 um, the lubricant used is polymethylsiloxane with a molecular weight of 500,000, and the release agent used is homemade polylactic acid grafted polyether silicone oil.
[0042] The mass ratio of the abc three-layer co-extruded melt is controlled to be 10:80:10 by the melt pumps of the three extruders respectively, and the pressure after the pump is maintained at 2-3 MPa by adjusting the melt temperature and flow rate; vacuum adsorption or electrostatic attachment is selected to make the melt fit closely with the quenching roller to achieve the effect of rapid cooling, and the optimal cold roller temperature is 25-35 ℃; the cast sheet with a thickness of 200-350 um generated by quenching is preheated to 60-65 ℃ through infrared auxiliary heating.
[0043] (2) Preparation by biaxial stretching process: Biaxial stretching is performed on the cast sheet preheated in step (1), and a longitudinal stretching ratio of 3 times is achieved by setting the speed ratio of two or three longitudinal stretching rollers and the pressure roller; the longitudinally stretched sheet produces a 25% to 30% shrinkage, and a 4-fold transverse stretching is achieved by adjusting the width ratio of the transverse stretching inlet and outlet. The transverse stretching preheating temperature is 70 to 78 °C, and the stretching section temperature is 75 to 85 °C. The film at the transverse stretching outlet is wound up after being trimmed with the assistance of a small pressure roller, and the production line speed is 45 to 150 m / min.
[0044] Among them, the homemade polylactic acid grafted polyether silicone oil was prepared according to the following method: polyether silicone oil with an epoxy value of 0.086 mol / 100 g and a viscosity of 100 mPa.S was selected as the raw material, and the mass ratio of the polylactic acid FY801 was 3:97, and 0.2wt% of the catalyst BIBP was added at the same time, and the ingredients were 150 kg. After the ingredients were mixed in a high mixing pot for 5 minutes, they were automatically fed to a 65-type twin-screw extruder with a length-to-diameter ratio of 52:1 through a loss-in-weight scale. The processing temperatures of the extruder feeding section, plasticizing section, mixing section, and compression section were set to 150 ℃, 180 ℃, 175 ℃, and 170 ℃, respectively. The water-cooled strands were cut into pellets and dried at 40 ℃ for 24 hours to obtain a homemade release agent (polylactic acid grafted polyether silicone oil).
[0045] Example 2
[0046] Example 2 of the present invention provides a tape substrate (biaxially oriented polylactic acid film, i.e., BOPLA release film) and a preparation method thereof, which is different from Example 1 in that the net content of the anti-blocking agent in the c layer is 1000 ppm, and other process conditions are the same.
[0047] Example 3
[0048] Example 3 of the present invention provides a tape substrate (biaxially oriented polylactic acid film, i.e., BOPLA release film) and a preparation method thereof, which is different from Example 1 in that the net content of the anti-blocking agent in the c layer is 1500 ppm, and other process conditions are the same.
[0049] Examples 1-3 of the present invention investigate the effect of the content of the antiblocking agent in the c layer on the performance of the BOPLA release film. The performance of the BOPLA release films prepared in Examples 1-3 of the present invention are tested, and the test results are shown in Table 1 below.
[0050] Table 1 Effect of antiblocking agent on the performance of BOPLA release film
[0051] Example Net content of opening agent / ppm Haze / % Static friction coefficient Dynamic friction coefficient Release force (g / 25 mm) 1 500 2 0.30 0.23 475 2 1000 2.6 0.33 0.24 500 3 1500 2.7 0.4 0.25 550
[0052] As can be seen from Table 1, the content of the opening agent has a certain effect on the haze of the film. In the range of 500-1500 ppm, the optical properties of the film meet the technical requirement of the haze of the tape being less than 3%. When the content of the lubricant is 20000 ppm, the dynamic friction coefficient of all films is less than 0.3, showing good slip performance. The release force of the film prepared in Example 1 with a better content of the opening agent, lubricant, and release agent is 475 g / 25mm.
[0053] Example 4
[0054] Example 4 of the present invention provides a tape substrate (biaxially oriented polylactic acid film, i.e., BOPLA release film) and a preparation method thereof, which is different from Example 1 in that the net contents of the opening agent, the slip agent, and the release agent in the c layer are 250 ppm, 1600 ppm, and 1500 ppm, respectively, and the other process conditions are the same.
[0055] Example 5
[0056] Example 5 of the present invention provides a tape substrate (biaxially oriented polylactic acid film, i.e., BOPLA release film) and a preparation method thereof, which is different from Example 4 in that the net content of the lubricant in the c layer is 8000 ppm, and other process conditions are the same.
[0057] Example 6
[0058] Example 6 of the present invention provides a tape substrate (biaxially oriented polylactic acid film, i.e., BOPLA release film) and a preparation method thereof, which is different from Example 4 in that the net content of the lubricant in the c layer is 16000 ppm, and other process conditions are the same.
[0059] Examples 4-6 of the present invention investigate the effect of the content of the lubricant in the c layer on the performance of the BOPLA release film. The performance of the BOPLA release film prepared in Examples 4-6 of the present invention is tested, and the test results are shown in Table 2 below.
[0060] Table 2 Effect of lubricant on the performance of BOPLA release film
[0061] Example Net content of lubricant / ppm Haze / % Static friction coefficient Dynamic friction coefficient Release force (g / 25mm) 4 1600 0.9 0.55 0.46 625 5 8000 1.6 0.47 0.4 575 6 16000 2.3 0.4 0.35 529
[0062] As can be seen from Table 2, the content of the lubricant has a great influence on the haze. The haze of Example 4 is less than 1%, showing excellent optical properties. To meet better slip performance (lower dynamic friction coefficient), the content of the lubricant should be above 16000 ppm. At this time, the release force of Example 6 is also at a relatively low level.
[0063] Example 7
[0064] Example 7 of the present invention provides a tape substrate (biaxially oriented polylactic acid film, i.e., BOPLA release film) and a preparation method thereof, which is different from Example 1 in that: the homemade polylactic acid grafted polyether silicone oil used is further irradiated after being extruded, pelletized and dried by a twin-screw extruder, and the irradiation conditions are: 50 KGy absorbed dose, γ-ray irradiation for 17 hours.
[0065] In Example 1 and Example 7 of the present invention, the effects of release agents (polylactic acid grafted polyether silicone oil) prepared by different preparation methods in the c layer on the performance of the BOPLA release film are investigated. The performance of the BOPLA release films prepared in Example 1 and Example 7 of the present invention are tested, and the test results are shown in Table 3 below.
[0066] Table 3 Effect of release agent on the performance of BOPLA release film
[0067] Example Irradiation time / h Haze / % Static friction coefficient Dynamic friction coefficient Release force (g / 25 mm) 1 0 2 0.30 0.23 475 7 17 1.8 0.25 0.21 465
[0068] It can be seen from Table 3 that compared with Example 1, the haze, friction coefficient, release force, etc. of the film prepared in Example 7 are improved. This may be because irradiation promotes the grafting reaction of polyether silicone oil on polylactic acid, making the release agent with a higher grafting rate less likely to migrate in the outer surface layer of the BOPLA release film.
[0069] Example 8
[0070] The BOPLA release film prepared in Example 1 was stored in a high humidity environment (temperature 30°C, relative humidity 80%) for 45 days, and then its mechanical properties were tested. At the same time, the BOPLA release film prepared in this example was stored in a conventional storage environment (temperature 23°C, relative humidity 50%) for 45 days and its mechanical properties were tested. The test results are shown in Table 4 below.
[0071] Table 4 Effect of storage method on the mechanical properties of BOPLA release film
[0072] Test direction Storage Maximum strength / MPa Elongation at break / % Elastic modulus / MPa Vertical conventional 135 145 3084 High humidity 118 134 3078 Horizontal conventional 146 125 3159 High humidity 126 118 3134
[0073] It can be seen from Table 4 above that the BOPLA release film prepared in Example 1 can still exhibit excellent mechanical properties even after being stored in a high humidity environment for 45 days.
[0074] Example 9
[0075] Embodiment 9 of the present invention provides a bio-based polylactic acid tape and a preparation method thereof, comprising the following steps:
[0076] (1) Preparation of polylactic acid adhesive: Two copolymers with glass transition temperatures of 38.3 °C and -37.5 °C were synthesized according to the molar ratio of caprolactone to lactide of 20:80 and 75:25, respectively, and used as polylactic acid pressure-sensitive adhesive after melt blending.
[0077] The specific synthesis process of the two copolymers is as follows:
[0078] 1) Weigh 2280 g of caprolactone and 11520 g of L-lactide in a molar ratio of 20:80, add them to a reactor that has been dehydrated, add 0.5% of the total mass of isosorbide as an initiator, use a double-row gas distributor to evacuate the reactor and fill it with nitrogen. After three treatments, seal the reactor and start heating. After the initiator and monomer are fully mixed and the lactide is completely melted, use a syringe to take a stannous chloride catalyst solution and inject it into the reactor through the liquid feed port. The amount of stannous chloride catalyst added accounts for 0.2% of the total mass of the system. At 140 ° C, react for 24 hours, discharge the material through the melt pump at the bottom of the reactor, cool it with ice water and cut it into pellets, and dry it at 40 ° C for 24 hours to obtain a copolymer with a glass transition temperature of 38.3 ° C.
[0079] 2) Weigh 8550 g of caprolactone and 3600 g of L-lactide in a molar ratio of 75:25, add them to the reactor after dewatering, add 0.5% of the total mass of isosorbide as initiator, use a double-row gas distributor to evacuate the reactor and fill it with nitrogen, after three times of treatment, seal the reactor and start heating, after the initiator and monomer are fully mixed and the lactide is completely melted, use a syringe to take the stannous chloride catalyst solution, inject it into the reactor through the liquid feed port, and the amount of stannous chloride catalyst added is 0.2% of the total mass of the system. At 140 ° C, react for 24 hours, discharge the material through the melt pump at the bottom of the reactor, cool it with ice water and cut it into pellets, and dry it at 40 ° C for 24 hours to obtain a copolymer with a glass transition temperature of -37.5 ° C.
[0080] (2) Using the BOPLA release film prepared in Example 1 as the tape substrate, the pressure-sensitive adhesive (i.e., polylactic acid adhesive) prepared in step (1) is added to a coating machine and heated to an appropriate temperature to make the pressure-sensitive adhesive liquid. The pressure-sensitive adhesive prepared in step (1) is coated on layer a of the tape substrate with a thickness of 30 um, unwound and coated by a coating machine, and then slit after winding to obtain bio-based polylactic acid tapes of different widths.
[0081] The bonding performance of the bio-based polylactic acid tape prepared in this example was compared with that of the commercial BOPP tape, and the results are shown in Table 5 below.
[0082] Table 5
[0083] sample Peel strength (g / 25 mm) Ring initial adhesion / N Holding force / h Release force (g / 25 mm) Example 9 1270 6.5 ≥24 475 BOPP tape 847 9.3 ≥24 538
[0084] It can be seen from Table 5 that the bonding performance of the bio-based polylactic acid tape prepared in this embodiment reaches or even exceeds that of the commercial BOPP tape. Under the social development demand of carbon reduction and environmental protection, the bio-based polylactic acid tape of this embodiment has promotion and application value.
[0085] According to GB / T 19277.1-2011 standard, a composting test was conducted on the bio-based polylactic acid tape prepared in this embodiment, and it was found that its relative decomposition rate reached 93.9% after 180 days, demonstrating its excellent biodegradability.
[0086] Figure 1 is a comparative test data diagram of the relative decomposition rate of the bio-based polylactic acid tape and microcrystalline cellulose prepared in this embodiment, from Figure 1 It can be seen that the degradation rate of bio-based polylactic acid tape is slower than that of microcrystalline cellulose within 50 days, while the relative decomposition rate at 180 days is higher than that of microcrystalline cellulose.
[0087] The relevant test standards in Examples 1 to 9 of the present invention are as follows:
[0088] GB / T 2410-2008 Determination of light transmittance and haze of transparent plastics
[0089] GB / T 10006-2021 Determination of friction coefficient of plastic films and sheets
[0090] GB / T 1040.3-2006 Determination of tensile properties of plastics Part 3: Test conditions for films and sheets
[0091] GB / T 2792 Test method for peel strength of adhesive tape
[0092] GB / T 4851-2014 Test method for adhesive tape holding property
[0093] GB / T 4852-2002 Test method for initial tack of pressure-sensitive adhesive tapes (rolling ball method).
[0094] The above embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the present invention. It should be pointed out that, for a person of ordinary skill in the art, several modifications and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the present invention patent shall be subject to the attached claims.
Claims
1. A bio-based polylactic acid tape, characterized in that: It comprises a tape substrate and a polylactic acid adhesive layer coated on the surface of the tape substrate; The adhesive tape substrate comprises an inner layer, an intermediate layer and an outer surface layer stacked in sequence; the inner layer contains polylactic acid, an opening agent and a lubricant; the intermediate layer contains only polylactic acid; the outer surface layer contains polylactic acid, an opening agent, a lubricant and a release agent; in the inner layer, the net contents of the opening agent and the lubricant are 250-500 ppm and 1000-3000 ppm respectively; in the outer surface layer, the net contents of the opening agent, the lubricant and the release agent are 250-1000 ppm, 10000-20000 ppm and 3000-5000 ppm respectively; The polylactic acid adhesive layer is coated on the inner layer; The release agent is polylactic acid grafted polyether silicone oil; the polyether silicone oil is polyether silicone oil containing epoxy functional groups, and its viscosity is 100-400 mPa.S; the mass ratio of polyether silicone oil to polylactic acid is 3-5:95-97; The polylactic acid adhesive layer has two glass transition temperatures of -40 to -30°C and 35 to 45°C.
2. A bio-based polylactic acid tape as claimed in claim 1, characterized in that: The polylactic acid grafted polyether silicone oil is prepared by the following method: polylactic acid, polyether silicone oil and BIBP are mixed and then extruded and granulated by a twin-screw extruder.
3. A bio-based polylactic acid tape as claimed in claim 2, characterized in that: The method also includes a step of irradiating the extruded and granulated polylactic acid grafted polyether silicone oil, wherein the irradiation conditions are: 50 KGy absorbed dose, and γ-ray irradiation for 15 to 20 hours.
4. A bio-based polylactic acid tape as claimed in claim 2, characterized in that: The addition amount of the BIBP is 0.1-0.3 wt %, and the working temperature of the twin-screw extruder is 150-220 ° C.
5. The bio-based polylactic acid tape according to claim 1, characterized in that: The polylactic acid adhesive layer is prepared from caprolactone and lactide as raw materials, and the molar ratio of caprolactone to lactide is 20-75:25-80.
6. A bio-based polylactic acid tape according to any one of claims 1 to 5, characterized in that: The weight average molecular weight of the polylactic acid in the inner layer, the middle layer and the outer surface layer is greater than 200,000, the polydispersity index is less than 1.6, and the melting point is 155-180°C.
7. A method for preparing a bio-based polylactic acid tape according to any one of claims 1 to 6, characterized in that: The following steps are involved: The raw materials of the inner layer, the middle layer and the outer surface layer are melted and co-extruded to obtain a cast sheet; The cast sheet is longitudinally stretched and transversely stretched to obtain a polylactic acid film; The polylactic acid film is unwound and coated by a coating machine, the polylactic acid film is used as a tape substrate, a polylactic acid adhesive is coated on the inner layer thereof, and the film is slit after being rolled up to obtain a bio-based polylactic acid tape.
Citation Information
Patent Citations
Two-way stretching polylactic acid film capable of resisting anti-adhesion of glue and preparation method of two-way stretching polylactic acid film
CN115366515A
Self-adhesive polylactic acid adhesive and application thereof
CN116855213A
Laminate containing a substrate and a release agent and method of its preparation
EP0254050A2
Self-adhesive sheet or tape for surface protection
JP1990252782A