A sintered R-Fe-B permanent magnet and its preparation method and application
By introducing Zr-B needle-shaped phase and high vacuum low-temperature diffusion treatment into NdFeB permanent magnets, the problem of degradation of magnetic performance of NdFeB permanent magnets at high temperatures is solved, and the grain size consistency and magnetic performance improvement are achieved , extends the high temperature resistance of the motor.
Patent Information
- Application Number
- CN202411075746.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-07
AI Technical Summary
The problem of the degradation of magnetic properties of existing neodymium iron boron permanent magnets at high temperatures is mainly due to the difference in grain size, poor magnetic properties, squareness and poor mechanical properties.
By introducing Zr-B needle-like phase into the sintered R-Fe-B permanent magnet, combined with high vacuum low-temperature diffusion treatment, the grain size consistency is controlled, and a slender diffusion channel is formed, which promotes the penetration of heavy rare earth elements into the interior and inhibits the penetration of heavy rare earth elements. The main phase grains grow.
The magnetic performance and grain size consistency of sintered R-Fe-B permanent magnet is improved, the high temperature resistance of the magnet is extended, and the stability of the motor efficiency is ensured.
Smart Images

Figure CN118609934B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of rare earth permanent magnet material preparation, and in particular relates to a sintered R-Fe-B permanent magnet prepared by grain boundary diffusion, and a preparation method and application thereof. Background Art
[0002] Improving energy utilization efficiency is a key way to effectively solve energy problems. According to statistics, in the industrial sector, motors have always accounted for a high proportion of electrical energy consumption. Therefore, improving the efficiency of motors is of great significance to saving power resources. Compared with traditional motors, permanent magnet motors have higher motor efficiency. Permanent magnet motors have been widely used in many industrial fields such as electric vehicles and elevators. Sintered NdFeB permanent magnet motors have the advantages of high efficiency, low noise and small size, making them the preferred material for manufacturing high-efficiency permanent magnet motors. However, during the operation of the motor, the Nd-Fe-B magnets will be subjected to high temperatures caused by eddy currents, causing the performance of the magnets to decrease with the increase in temperature, ultimately resulting in reduced motor efficiency and increased energy consumption. Improving the intrinsic coercive force of NdFeB magnets can improve the high temperature resistance of the magnets, increase the power density and torque density of the motor, and ensure that the motor efficiency does not decay.
[0003] There are many ways to improve the intrinsic coercivity of NdFeB magnets, among which grain refinement and heavy rare earth grain boundary diffusion technology are currently the most effective and easiest to implement methods. Further diffusion treatment using the grain-refined magnet as the substrate can significantly improve the coercivity of the magnet. However, the grain refinement causes an increase in the number of grains per unit volume, which increases the penetration barrier of heavy rare earth elements. In order to obtain a better diffusion effect and ensure that the surface and center of the magnet have the same heavy rare earth elements, a longer diffusion time is required to achieve the diffusion of the diffusion source elements into the interior of the magnet. Under high temperature during the diffusion process, the atoms in the boundary layer of the main phase of the magnet grains are in a high energy state and are in contact with the high concentration of rare earth elements in the thermally activated state in the grain boundary phase for a long time, and the main phase grains will grow spontaneously and inevitably. In particular, the abnormal growth of the surface grains of the magnet that first come into contact with the heavy rare earth diffusion source will reduce the diffusion channel, hinder the diffusion source from diffusing deeper into the magnet, and make the core main phase grains less exposed to the diffusion source elements while still maintaining the original grain size and performance, resulting in a large difference in grain size between the surface and core main phases of the magnet, leading to poor magnetic properties, squareness and mechanical properties of the magnet. Summary of the invention
[0004] To solve the above shortcomings, the technical solution of the present invention is as follows:
[0005] A sintered R-Fe-B permanent magnet, wherein the main phase grains of the surface layer of the sintered R-Fe-B permanent magnet are recorded as surface grains, the size of the surface grains is D1, the main phase grains of the core along the easy magnetization direction of the sintered R-Fe-B permanent magnet are recorded as core grains, the size of the core grains is Dn, and 0<D1-Dn≤0.34, for example, 0.3, 0.2, 0.1; wherein n is an integer greater than 1, for example, 2, 3, 4, 5...
[0006] In the present invention, the surface layer of the sintered R-Fe-B permanent magnet refers to the area at a depth of 0-0.3 mm from the outer surface of the permanent magnet in the easy magnetization direction of the sintered R-Fe-B permanent magnet, and the size D1 of the surface grains refers to the average size of the main phase grains in the surface layer; the core of the sintered R-Fe-B permanent magnet refers to the area from 0.3 mm from the outer surface of the permanent magnet to the center point of the permanent magnet geometry in the easy magnetization direction of the sintered R-Fe-B permanent magnet, and the size Dn of the core grains refers to the average size of the main phase grains in the core; the areas corresponding to the surface layer and the core are as follows Figure 2 In the present invention, the easy magnetization direction of the sintered R-Fe-B permanent magnet refers to the thickness direction, and the average size of the main phase grains refers to the average value of the sizes of multiple (at least 6 or more) main phase grains in the corresponding area.
[0007] According to a preferred embodiment of the present invention, in the core, the average size of the core grains close to the surface of the permanent magnet is larger, and the average size of the core grains close to the center point of the permanent magnet geometric body is smaller.
[0008] According to an embodiment of the present invention, the core can also be divided into multiple parts along the easy magnetization direction of the sintered R-Fe-B permanent magnet; for example, it is evenly divided into a first core, a second core and a third core, the first core, the second core and the third core have the same thickness, the first core is close to the surface of the permanent magnet, and the third core is close to the center point of the permanent magnet geometry. Preferably, the average size of the first core grains in the first core is D2, the average size of the second core grains in the second core is D3, and the average size of the third core grains in the third core is D4. Preferably, D4≤D3≤D2. Further, 0<D1-D2≤0.34, and 0<D1-D3≤0.34, and 0<D1-D4≤0.34.
[0009] According to the embodiment of the present invention, the thickness of the sintered R—Fe—B permanent magnet is not specifically limited, and a thickness known in the art, such as 3.0 mm or 3.1 mm, can be selected.
[0010] According to an exemplary solution of the present invention, the thickness of the sintered R-Fe-B permanent magnet is 3mm, and along the easy magnetization direction of the sintered R-Fe-B permanent magnet, the core includes: a first core, a second core and a third core in sequence. Preferably, the first core refers to the area from 0.3mm to 0.7mm from the surface of the permanent magnet, and the average size of the first core grains corresponding to this area is D2; the second core refers to the area from 0.7mm to 1.1mm from the surface of the permanent magnet, and the average size of the second core grains corresponding to this area is D3; the third core refers to the area from 1.1mm to 1.5mm from the surface of the permanent magnet, and the average size of the third core grains corresponding to this area is D4. Further, D1-D2≤0.34, and D1-D3≤0.34, and D1-D4≤0.34.
[0011] According to an embodiment of the present invention, the sintered R-Fe-B permanent magnet includes a main phase and a grain boundary phase, wherein the grain boundary phase includes a Zr-B phase, and the Zr-B phase has a needle-like structure, such as Figure 1 Preferably, the length of the needle-shaped Zr-B phase is 20nm-1000nm, for example, 100nm, 500nm. Preferably, the needle-shaped Zr-B phase is uniformly dispersed in the grain boundary phase, changing the grain boundary state.
[0012] According to an embodiment of the present invention, the magnetic properties of the sintered R-Fe-B permanent magnet are as follows:
[0013] (1) Br is not less than 1.41T, for example, 1.419T, 1.420T, 1.421T;
[0014] (2) Hcj is not less than 1900KA / m, for example, 1910KA / m, 1920KA / m, 1930KA / m, 1940KA / m, 1950KA / m, 1960KA / m, 1970KA / m, 1980KA / m, 1990KA / m.
[0015] According to an embodiment of the present invention, the raw material of the sintered R-Fe-B permanent magnet contains Zr and B. Preferably, the mass contents of Zr and B in the raw material are respectively recorded as [Zr] and [B], and satisfy 0.13≤[Zr] / [B]≤0.55, and the mass content of Zr in the raw material is not less than 0.15wt%, so as to ensure that a needle-shaped Zr-B phase can be formed in the grain boundary phase, thereby realizing the change of the grain boundary phase.
[0016] According to an embodiment of the present invention, the raw material for sintering the R-Fe-B permanent magnet comprises:
[0017] R is selected from at least one or more of Sm, La, Ce, Y, Nd, Pr, Ho, Gd, Dy, and Tb, and the mass content of Re is not less than 28wt% and not more than 35wt%;
[0018] M1 is selected from at least one or more of Co, Ga, Cu, Al, Nb, Zr, and Ti, and the mass content of M1 is not less than 0.5wt% and not more than 5wt%;
[0019] The content of B is not less than 0.95wt% and not more than 1.3wt%;
[0020] The content of Zr is not less than 0.15wt%, preferably not less than 0.15wt% and not more than 0.5wt%, for example, 0.45wt%;
[0021] The rest is Fe and inevitable impurity elements.
[0022] The present invention also provides a method for preparing the sintered R-Fe-B permanent magnet, the method comprising:
[0023] (1) The raw materials are mixed according to the corresponding mass ratio to prepare NdFeB alloy quick-solidification sheets, which are then crushed to obtain magnetic powder of target particle size;
[0024] (2) The obtained magnetic powder is pressed and cold isostatically pressed to obtain a green body;
[0025] (3) subjecting the green body to sintering and aging treatment to obtain a sintered NdFeB matrix;
[0026] (4) The sintered NdFeB matrix is then subjected to high temperature diffusion treatment to obtain the sintered R-Fe-B permanent magnet.
[0027] According to an embodiment of the present invention, in step (1), the raw material refers to the raw material for sintering R—Fe—B permanent magnets as described above.
[0028] According to an embodiment of the present invention, in step (1), the NdFeB alloy quick-setting sheet is prepared by a method known in the art, such as quick-setting belt spinning technology. Exemplarily, the method for preparing the NdFeB alloy quick-setting sheet is as follows: the raw material is heated to 1300-1600°C by electromagnetic induction to melt, and then the alloy melt is poured on a rapid cooling roller (preferably a polished rapid cooling roller), and then falls into a water cooling barrel for further cooling to obtain a NdFeB alloy quick-setting sheet.
[0029] According to an embodiment of the present invention, in step (1), the crushing step specifically includes: subjecting the NdFeB alloy quick-solidified thin sheet to hydrogen explosion to obtain a coarse crushed powder, and then subjecting the NdFeB alloy quick-solidified thin sheet to high-energy ball milling or air flow milling to obtain magnetic powder. Preferably, a lubricant can also be added during crushing, and the lubricant can be a lubricant known in the art, which is not specifically limited in the present invention. Furthermore, the amount of lubricant added is 0.1~1wt% of the magnetic powder, for example, 0.1~0.5wt%.
[0030] Exemplarily, in step (1), the pulverizing step is as follows: the NdFeB alloy quick-solidified thin sheet is first subjected to hydrogen explosion to obtain a coarse pulverized powder, and then ground and pulverized by a jet mill to obtain magnetic powder of a target particle size; optionally, after obtaining the magnetic powder of the target particle size, 0.1 to 0.5 wt% of a lubricant can be added to the mixture, for example, the mixture is mixed for 0.1 to 5 hours to uniformly mix the magnetic powder.
[0031] In the present invention, the hydrogen explosion, high-energy ball milling process and air flow milling process can be carried out using process conditions known in the art, as long as the magnetic powder can be obtained.
[0032] According to an embodiment of the present invention, in step (1), the target particle size of the magnetic powder is 1-8 μm, for example, 5 μm.
[0033] According to an embodiment of the present invention, in step (2), the pressing and molding comprises: pressing and molding the magnetic powder in an orientation manner in a magnetic field. Preferably, the magnetic field can be a magnetic field known in the art, for example, a magnetic field strength of 2T.
[0034] According to an embodiment of the present invention, in step (2), the cold isostatic pressing can be performed using cold isostatic pressing conditions known in the art, which are not specifically limited in the present invention.
[0035] According to an embodiment of the present invention, in step (3), the sintering treatment comprises: placing the green body in a vacuum environment and sintering it at a high temperature of 1055° C. to 1090° C.
[0036] According to an embodiment of the present invention, in step (3), the aging treatment refers to tempering treatment at a temperature below 1000° C. after sintering, which can be carried out under conditions known in the art, such as tempering at 910° C. and 520° C. for 4 hours respectively.
[0037] According to an embodiment of the present invention, in step (4), the sintered NdFeB substrate may be firstly machined to process the sintered NdFeB substrate into R—Fe—B black sheets of target size.
[0038] According to an embodiment of the present invention, in step (4), the sintered NdFeB matrix (such as R-Fe-B black sheet) may be cleaned first, and methods known in the art may be used for cleaning, such as acid pickling with a volume concentration of 1% to 5% to remove oxide impurities and oil stains on the surface of the sintered NdFeB matrix (such as R-Fe-B black sheet).
[0039] According to the embodiment of the present invention, in step (4), the high temperature diffusion treatment specifically comprises: coating the surface of the sintered NdFeB matrix (such as R-Fe-B black sheet) with heavy rare earth elements so that the heavy rare earth elements are evenly distributed on the surface of the sintered NdFeB matrix (such as R-Fe-B black sheet); performing two-stage heat treatment diffusion in a vacuum atmosphere, wherein the temperature range of the first stage heat treatment is 790°C. 930°C (preferably not higher than 900°C, for example 800°C, 850°C, 900°C), the temperature range of the secondary heat treatment is 440°C 530°C (preferably not higher than 520°C, such as 450°C, 500°C, 520°C), vacuum degree 10 2 10 4 The inventors found that when the two-stage heat treatment diffusion of the present invention is used, a lower vacuum degree is used to reduce the temperature during diffusion, so the Zr-B phase will not dissolve during the diffusion stage.
[0040] According to an embodiment of the present invention, the heavy rare earth element is provided by a diffusion source. Preferably, the diffusion source comprises heavy rare earth powder particles, an antioxidant and an organic solvent. Preferably, the diffusion source is coated on the surface of a sintered NdFeB matrix (such as R-Fe-B black sheet) in the form of a slurry. Preferably, the heavy rare earth powder particles comprise at least one or more mixtures of dysprosium, dysprosium hydride, dysprosium oxide, dysprosium fluoride, terbium, terbium hydride, terbium oxide, and terbium fluoride.
[0041] According to an embodiment of the present invention, the average particle size of the heavy rare earth powder particles is 2-100 μm (eg, 10 μm, 50 μm) and D90 / D10 is 1.2-5.1 (eg, 2, 3, 4).
[0042] The inventors found that in order to prevent the Zr element from dissolving in the Nd-rich phase at a higher temperature and alloying with other trace elements, thereby failing to achieve magnetic isolation and failing to inhibit the growth of the main phase grains, it is necessary to diffuse at a lower diffusion temperature to ensure that the Zr-B phase in the grain boundary phase of the permanent magnet after diffusion is not dissolved, and forms a slender tube with the main phase grains, thereby enhancing the capillary force and promoting the diffusion source to penetrate into the permanent magnet. For this purpose, the diffusion process adopts a high vacuum degree (≥10 -2Pa) to achieve a relatively low diffusion temperature; at the same time, the average particle size range of the powder particles in the diffusion source meets 2-100μm and the D90 / D10 range is 1.2-5.1, ensuring that the diffusion source is melted synchronously during the diffusion process, maximizing the concentration difference between the magnet surface and the internal diffusion source, increasing the diffusion driving force, promoting the diffusion source to penetrate into the permanent magnet, shortening the diffusion time, ensuring the magnetic properties while suppressing the abnormal growth of surface grains.
[0043] The present invention also provides a sintered R—Fe—B permanent magnet prepared by the above preparation method, and the sintered R—Fe—B permanent magnet has the meaning as described above.
[0044] The present invention also provides the use of the sintered R—Fe—B permanent magnet, preferably used in a motor.
[0045] Beneficial effects:
[0046] Compared with conventional fine-grained diffusion magnets, the needle-shaped Zr-B phase formed by Zr and B in the raw material of the permanent magnet of the present invention is distributed in the grain boundary phase, and the grain boundary state is changed. A relatively long and narrow channel is formed between the needle-shaped Zr-B phase and the main phase particles, which reduces diffusion obstacles, enhances the capillary force, accelerates the transfer of heavy rare earth elements in the diffusion source to the interior of the permanent magnet, reduces the accumulation of heavy rare earth elements in the grain boundary phase, and inhibits the growth of the main phase grains. The present invention improves the consistency of the grain size of the main phase in the sintered R-Fe-B permanent magnet, thereby improving the magnetic properties of the sintered R-Fe-B permanent magnet. In addition, the melting point of the grain boundary phase is reduced by adopting the low-temperature diffusion treatment conditions of high vacuum degree; the large particles with concentrated particle size distribution are synchronously melted by the diffusion source particles at a relatively low temperature, which promotes the diffusion source elements to form a larger concentration difference on the surface and inside of the magnet, further accelerates the diffusion of heavy rare earth elements into the interior of the magnet, reduces the accumulation of the diffusion source in the grain boundary phase, inhibits the growth of grains, and ensures the consistency of the grain size of the main phase in the permanent magnet after the fine-grained magnet is diffused. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Figure 1 This is the TEM of the sintered Nd—Fe—B permanent magnet obtained in Example 1.
[0048] Figure 2 Schematic diagram of the corresponding areas of the surface and core of the sintered R-Fe-B permanent magnet.
[0049] Figure 3 Schematic diagram of the main phase grains corresponding to different regions along the thickness direction in the cross section of the sintered R-Fe-B permanent magnet.
[0050] Figure 4 Schematic diagram of the sampling points of surface grains.
[0051] Figure 5TEM of the sintered Nd—Fe—B permanent magnet obtained in Comparative Example 1-6. DETAILED DESCRIPTION
[0052] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.
[0053] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.
[0054] Example 1
[0055] A method for preparing a high-performance sintered Nd-Fe-B permanent magnet, the steps are as follows:
[0056] (1) The raw materials required for the Nd-Fe-B alloy were melted in an argon atmosphere at 1400°C according to the target ratio and kept for 15 minutes to ensure the homogenization of the raw materials. Then, the raw materials were poured onto the surface of a rotating quenching roller to obtain a Nd-Fe-B alloy quick-solidification sheet with a thickness of about 0.3 mm. Among them, in the Nd-Fe-B alloy, Nd accounts for 31.3wt%, B accounts for 1.0wt%, Zr accounts for 0.45wt%, Al accounts for 0.10wt%, Ga accounts for 0.2wt%, and Co accounts for 1.0wt%; the rest is Fe and unavoidable impurities;
[0057] (2) The Nd-Fe-B alloy quick-solidified thin slices in step (1) are coarsely crushed in a hydrogen explosion furnace and discharged under argon protection to reduce oxidation of the coarse powder. The coarse powder after hydrogen explosion is directly jet milled to obtain magnetic powder with a particle size of 1-8μm and an average particle size of 2.8μm;
[0058] (3) adding 0.15 wt% of antioxidant fatty acid ester to the magnetic powder obtained in step (2), and continuously stirring mechanically for 4 h until the magnetic powder is evenly dispersed;
[0059] (4) Pressing the magnetic powder obtained in step (3) into a green body in a vacuum environment with a magnetic field strength of 2T and in a magnetic field orientation direction, and cold isostatically pressing the green body at 170 MPa to obtain a green body;
[0060] (5) The green body of step (4) is placed in a vacuum sintering furnace, sintered at 1065°C for 3 h, and then tempered at 910°C and 520°C for 4 h to obtain a sintered Nd-Fe-B substrate.
[0061] (6) The sintered Nd-Fe-B permanent magnet obtained in step (5) is machined into a black sheet with a thickness of 3.1 mm, a length of 35 mm, and a width of 21 mm, wherein the thickness direction is the direction in which the magnet is easily magnetized. The black sheet is degreased and decontaminated with 3% dilute nitric acid and then dried.
[0062] (7) The cleaned black sheet obtained in step (6) is coated with heavy rare earth elements in an atmospheric environment, and a slurry containing a Dy diffusion source is coated on two large surfaces of the black sheet, with a coating amount of 0.7% of the weight of the black sheet. The weight ratio of Dy powder particles to fatty acid ester and organic solvent in the slurry is 80:15:5, the average particle size of the Dy powder is 4.7 μm, and D90 / D10=3.1.
[0063] (8) The black sheet coated with heavy rare earth obtained in step (7) is placed on a 2×10 -3 Two-stage heat treatment diffusion is carried out in a Pa vacuum atmosphere. The temperature of the first heat treatment is 870°C for 6 hours, and the temperature of the second heat treatment is 460°C for 4 hours to obtain a sintered Nd-Fe-B permanent magnet.
[0064] This embodiment adopts a heat treatment temperature lower than the conventional two-stage heat treatment diffusion (900°C and 520°C), which inhibits the dissolution of the Zr element in the Nd-rich phase and alloying with other trace elements, ensuring the formation of the Zr-B phase in the grain boundary phase.
[0065] Performance test: a sample piece with a thickness of 3mm, a length of 7mm and a width of 7mm was processed from the center of the diffused black sheet. After saturation magnetization with a pulse magnetic field of 5T, a NIM-10000 measuring instrument was used to test the demagnetization curve of the obtained magnet at 20℃.
[0066] Magnet grain (i.e. main phase grain of permanent magnet) size test: grind off 0.05mm uniformly in all directions of the diffused magnet to remove the Dy diffusion source that has not penetrated into the magnet from the surface. Select the positions of 0.3mm, 0.7mm, 1.1mm and 1.4mm from the outer surface of the permanent magnet respectively, and cut it perpendicular to the easy magnetization direction (the thickness direction of the permanent magnet, also indicating the orientation direction). The cutting positions are as follows: Figure 3 As shown by the middle dotted line, the main phase grains in different cross sections corresponding to the test dotted lines; in the present invention, D1 is the size of the magnet grains in the area 0.3mm away from the outer surface in the cross section, D2 is the size of the magnet grains in the area 0.7mm away from the outer surface of the permanent magnet (recorded as the second core), D3 is the size of the magnet grains in the area 1.1mm away from the permanent magnet surface (recorded as the third core), and D4 is the size of the magnet grains in the area 1.5mm away from the permanent magnet surface (recorded as the fourth core). The above D1, D2, D3 and D4 all refer to the average value of the magnet grains measured at any 6 points in the corresponding cross section; as Figure 4 These are the 6 sampling points of D1.
[0067] Comparative Example 1-1
[0068] The preparation method of Comparative Example 1-1 is substantially the same as that of Example 1, except that: the Zr content in the Nd-Fe-B alloy in step (1) of Example 1 is changed to 0.10% while other contents remain unchanged, to obtain a Nd-Fe-B alloy quick-solidification sheet having a thickness of about 0.3 mm;
[0069] The rest is the same as in Example 1, and a sintered Nd-Fe-B permanent magnet is obtained.
[0070] According to the method described in Example 1, the magnetic properties of the sintered Nd-Fe-B permanent magnet obtained in this example at 20°C and the grain size at various locations were tested.
[0071] Comparative Example 1-2
[0072] The preparation method of Comparative Example 1-2 is basically the same as that of Example 1, except that the Zr element is not included in the formula for preparing the quick-setting sheet in step (1) of Example 1, and the other parts are consistent;
[0073] The rest is the same as in Example 1, and a sintered Nd-Fe-B permanent magnet is obtained.
[0074] According to the method described in Example 1, the magnetic properties of the sintered Nd-Fe-B permanent magnet obtained in this example at 20°C and the grain size at various locations were tested.
[0075] Comparative Examples 1-3
[0076] The preparation methods of Comparative Examples 1-3 are basically the same as those of Example 1, except that: the black sheet coated with heavy rare earth in step (8) of Example 1 is placed in a vacuum of 5×10 -2 Two-stage heat treatment diffusion is carried out in the atmosphere of Pa;
[0077] The rest is the same as in Example 1, and a sintered Nd-Fe-B permanent magnet is obtained.
[0078] According to the method described in Example 1, the magnetic properties of the sintered Nd-Fe-B permanent magnet obtained in this example at 20°C and the grain size at various locations were tested.
[0079] Comparative Examples 1-4
[0080] The preparation methods of Comparative Examples 1-4 are substantially the same as those of Example 1, except that: the average particle size of the Dy powder used in the slurry containing heavy rare earth Dy in step (7) of Example 1 is 1.8 μm, and the particle size distribution is D90 / D10=5.5;
[0081] The rest is the same as in Example 1, and a sintered Nd-Fe-B permanent magnet is obtained.
[0082] According to the method described in Example 1, the magnetic properties of the sintered Nd-Fe-B permanent magnet obtained in this example at 20°C and the grain size at various locations were tested.
[0083] Comparative Examples 1-5
[0084] The preparation methods of Comparative Examples 1-5 are basically the same as those of Example 1, except that: the Zr content in the Nd-Fe-B alloy in step (1) of Example 1 is 0.1%, and the black sheet coated with heavy rare earth in step (8) of Example 1 is placed in a vacuum of 2×10 -2 Two-stage heat treatment diffusion is carried out in the atmosphere of Pa; the average particle size of the diffusion source Dy powder used is still 4.7μm;
[0085] The rest is the same as in Example 1, and a sintered Nd-Fe-B permanent magnet is obtained.
[0086] According to the method described in Example 1, the magnetic properties of the sintered Nd-Fe-B permanent magnet obtained in this example at 20°C and the grain size at various locations were tested.
[0087] Comparative Examples 1-6
[0088] The preparation methods of Comparative Examples 1-6 are basically the same as those of Example 1, except that: the Zr content in the Nd-Fe-B alloy in step (1) of Example 1 is 0.1%, and the black sheet coated with heavy rare earth in step (8) of Example 1 is placed in a vacuum of 2×10 -2 Two-stage heat treatment diffusion was carried out in the atmosphere of Pa, the first stage heat treatment temperature was 900℃, the time was 6h, the second stage heat treatment temperature was 520℃, the time was 4h. The average particle size of the diffusion source Dy powder used was still 1.8μm;
[0089] The rest is the same as in Example 1, and a sintered Nd-Fe-B permanent magnet is obtained.
[0090] According to the method described in Example 1, the magnetic properties of the sintered Nd-Fe-B permanent magnet obtained in this example at 20°C and the grain size at various locations were tested.
[0091] Comparative Examples 1-7
[0092] The preparation methods of Comparative Examples 1-7 are basically the same as those of Example 1, except that: there is no heavy rare earth element coating process in step (7) of Example 1, no diffusion source heavy rare earth element diffusion, and the black sheet obtained in step (6) is directly coated on a 2×10 -3 Two-stage heat treatment diffusion was carried out in a Pa vacuum atmosphere, with the first stage heat treatment temperature at 860°C for 6 h and the second stage heat treatment temperature at 460°C for 4 h;
[0093] The rest is the same as in Example 1, and a sintered Nd-Fe-B permanent magnet is obtained.
[0094] According to the method described in Example 1, the magnetic properties of the sintered Nd-Fe-B permanent magnet obtained in this example at 20°C and the grain size at various locations were tested.
[0095] Example 2
[0096] The preparation method of Example 2 is basically the same as that of Example 1, except that: the Zr content in the Nd-Fe-B alloy in step (1) of Example 1 is 0.25%, and the black sheet coated with heavy rare earth in step (8) of Example 1 is placed in a vacuum of 2×10 - 3 Two-stage heat treatment diffusion is carried out in an atmosphere of Pa. The average particle size of the diffusion source Dy powder used is 11 μm, where D90 / D10=3.4;
[0097] The rest is the same as in Example 1, and a sintered Nd-Fe-B permanent magnet is obtained.
[0098] According to the method described in Example 1, the magnetic properties of the sintered Nd-Fe-B permanent magnet obtained in this example at 20°C were tested.
[0099] Example 3
[0100] The preparation method of Example 3 is basically the same as that of Example 1, except that: the Zr content in the Nd-Fe-B alloy in step (1) of Example 1 is 0.25%, and the black sheet coated with heavy rare earth in step (8) of Example 1 is placed in a vacuum of 2×10 - 4 Two-stage heat treatment diffusion is carried out in the atmosphere of Pa. The average particle size of the diffusion source Dy powder used is still 54μm, where D90 / D10=3.2;
[0101] The rest is the same as in Example 1, and a sintered Nd-Fe-B permanent magnet is obtained.
[0102] According to the method described in Example 1, the magnetic properties of the sintered Nd-Fe-B permanent magnet obtained in this example at 20°C were tested.
[0103] Example 4
[0104] The preparation method of Example 4 is basically the same as that of Example 1, except that: the Zr content in the Nd-Fe-B alloy in step (1) of Example 1 is 0.55%, and the black sheet coated with heavy rare earth in step (8) of Example 1 is placed in a vacuum of 2×10 - 4 Two-stage heat treatment diffusion is carried out in the atmosphere of Pa. The average particle size of the diffusion source Dy powder used is still 54μm, where D90 / D10=3.1;
[0105] The rest is the same as in Example 1, and a sintered Nd-Fe-B permanent magnet is obtained.
[0106] According to the method described in Example 1, the magnetic properties of the sintered Nd-Fe-B permanent magnet obtained in this example at 20°C were tested.
[0107] Example 1 and Comparative Examples 1-6 used TEM to analyze the grain boundary phase, and it can be observed that:
[0108] Figure 1 This is the TEM of the sintered Nd—Fe—B permanent magnet obtained in Example 1. The white area in the grain boundary in the figure is the Zr—B phase. It can be seen that a needle-shaped Zr—B phase is formed in the grain boundary phase of the sintered Nd—Fe—B permanent magnet prepared in this example, and the Zr—B phase is evenly and completely distributed in the grain boundary phase.
[0109] Figure 5 TEM of the sintered Nd-Fe-B permanent magnet obtained in Comparative Example 1-6. Figure 5 It can be seen that Zr-B is discretely distributed in the grain boundary phase, and the Zr-B phase does not form an elongated needle-like structure.
[0110] The magnetic properties of the sintered Nd—Fe—B permanent magnets of the above-mentioned embodiments and comparative examples at 20° C. and the grain sizes at various locations are recorded in Table 1.
[0111] Table 1
[0112]
[0113] It can be seen from the above table that in the sintered Nd-Fe-B permanent magnets prepared in Examples 1 to 4 of the present invention, D1-Dn≤0.34, Dn refers to D2, D3, and D4; while in the sintered Nd-Fe-B permanent magnets prepared in Comparative Examples 1 to 6, D1-Dn are all greater than 0.34. The comparison between the embodiments and the comparative examples shows that when the D1-Dn of the diffused product is less than 0.34 and greater than 0, the product has high grain size consistency and better magnetic properties.
[0114] The inventors believe that although the traditional diffusion process can greatly improve the magnetic properties of the permanent magnet during the diffusion process, at a higher diffusion temperature, the atoms in the boundary layer of the main phase grains in the permanent magnet are in a high-energy state. After long-term contact with the high-concentration rare earth elements and other elements in the thermally activated state in the grain boundary phase, the main phase grains, especially the surface grains, will spontaneously and inevitably grow, and the growth of the surface grains will affect the further improvement of the magnetic properties.
[0115] The sintered R-Fe-B permanent magnet prepared by the present invention can control the excessive growth of surface grains, so that the grain size corresponding to different positions in the sintered R-Fe-B permanent magnet is uniform, that is, 0<D1-Dn≤0.34. This is because: (1) The Zr element content is the basis for ensuring the formation of a larger needle-shaped Zr-B phase; the needle-shaped Zr-B phase changes the state of the grain boundary phase to ensure that the diffusion source elements quickly enter the interior of the magnet during the diffusion process, reducing the contact time between the diffusion source elements and the surface grains in the magnet to inhibit grain growth; (2) The high diffusion vacuum degree enables the elements in the diffusion source to complete the diffusion at a relatively low temperature, ensuring that the Zr-B phase in the grain boundary phase is not dissolved; (3) The particle size and distribution uniformity of the diffusion source powder enable it to melt at a lower diffusion temperature and realize the synchronous diffusion of the diffusion source, maximizing the concentration difference inside and outside the magnet, thereby shortening the diffusion time. It can be seen that the Zr content, diffusion vacuum and diffusion source particle size and distribution work together to prevent the diffusion source elements from being blocked from diffusing into the magnet, causing the magnet surface grains to be in contact with the diffusion source for a long time at high temperature, resulting in abnormal growth of the magnet grains. Specifically:
[0116] By comparing Comparative Examples 1-1, 1-2, 1-3, and 1-4, it can be seen that: if the needle-shaped Zr-B phase cannot be formed, the diffusion vacuum degree is low, and the diffusion source particle size is abnormal and the distribution is not concentrated, the diffusion source elements will be hindered from diffusing into the interior of the magnet, making it difficult for the diffusion source elements to penetrate into the magnet. The main phase grains on the surface of the magnet and the diffusion source elements and elements in the grain boundary phase undergo a long period of mass and heat transfer at high temperature, which ultimately leads to different degrees of growth of grains at different positions of the magnet, and a more obvious decrease in the Hcj@20℃ of the magnet.
[0117] By comparing Comparative Examples 1-5 with Example 1, it can be seen that when any two of the three factors, namely, the Zr element content, the diffusion vacuum degree and the diffusion source grain size, change, the magnet performance decreases more significantly, and the grains at different positions of the magnet grow larger and have greater size differences.
[0118] Therefore, the inventors believe that the synergistic effect of Zr element content, diffusion vacuum and diffusion source grain size is the key to preparing high-performance magnets with uniform grain size.
[0119] Comparing Comparative Examples 1-6 with Example 1, it can be seen that the Zr element content and the secondary low-temperature diffusion process affect the formation of the needle-shaped Zr-B phase, thereby affecting the diffusion rate of the diffusion source elements into the interior of the magnet and ultimately causing the magnet grain size to be consistent.
[0120] It can be seen from Example 2, Example 3, and Example 4 that when the Zr element content, diffusion vacuum degree, and diffusion source particle size and distribution vary within the scope of the present invention, there is no obvious effect on the formation of needle-shaped ZrB phase in the grain boundary, which effectively ensures the rapid diffusion of the diffusion source into the interior of the magnet, inhibits the abnormal growth of the magnet grains, and has little effect on the magnet performance and grain size, all of which have a small fluctuation range.
[0121] The above is a description of the exemplary embodiments of the present invention. However, the protection scope of the present application is not limited to the above embodiments. Any modification, equivalent substitution, improvement, etc. made by those skilled in the art within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A sintered R-Fe-B permanent magnet, characterized in that: The main phase grains of the surface layer of the sintered R-Fe-B permanent magnet are recorded as surface grains, and the size of the surface grains is D1. The main phase grains of the core along the easy magnetization direction of the sintered R-Fe-B permanent magnet are recorded as core grains, and the size of the core grains is Dn, and 0<D1-Dn≤0.34; wherein n is an integer greater than 1; the easy magnetization direction of the sintered R-Fe-B permanent magnet refers to the thickness direction; The sintered R-Fe-B permanent magnet includes a main phase and a grain boundary phase, wherein the grain boundary phase includes a Zr-B phase, and the Zr-B phase has a needle-like structure; the length of the needle-like Zr-B phase is 20nm-1000nm, and the needle-like Zr-B phase is uniformly dispersed in the grain boundary phase, thereby changing the grain boundary state; The raw material of the sintered R-Fe-B permanent magnet contains Zr element and B element; the mass contents of the Zr element and the B element in the raw material are respectively recorded as [Zr] and [B], and satisfy 0.13≤[Zr] / [B]≤0.55, and the mass content of the Zr element in the raw material is not less than 0.15wt%.
2. The sintered R-Fe-B permanent magnet according to claim 1, characterized in that: The magnetic properties of the sintered R-Fe-B permanent magnet are as follows: (1) Br is not less than 1.41T; (2) Hcj is not less than 1900KA / m.
3. The sintered R-Fe-B permanent magnet according to claim 1, characterized in that: The raw materials for the sintered R-Fe-B permanent magnet include: R is selected from at least one or more of Sm, La, Ce, Y, Nd, Pr, Ho, Gd, Dy, and Tb, and the mass content of Re is not less than 28wt% and not more than 35wt%; M1 is selected from at least one or more of Co, Ga, Cu, Al, Nb, Zr and Ti, and the mass content of M1 is not less than 0.5wt% and not more than 5wt%; The content of B is not less than 0.95wt% and not more than 1.3wt%; The content of Zr is not less than 0.15wt%; The rest is Fe and inevitable impurity elements.
4. The sintered R-Fe-B permanent magnet according to claim 1, characterized in that: The sintered R-Fe-B permanent magnet is obtained by subjecting a sintered NdFeB matrix to a high-temperature diffusion treatment; The high temperature diffusion treatment specifically includes: coating the surface of the sintered NdFeB substrate with heavy rare earth elements so that the heavy rare earth elements are evenly distributed on the surface of the sintered NdFeB substrate; performing two-stage heat treatment diffusion in a vacuum atmosphere, wherein the temperature range of the first heat treatment is 790°C-900°C but not including 900°C, the temperature range of the second heat treatment is 440°C-530°C, and the vacuum degree is 10 -2 -10 -4 Pa; The heavy rare earth element is provided by a diffusion source; the diffusion source comprises heavy rare earth powder particles, an antioxidant and an organic solvent; The heavy rare earth powder particles include at least one or more of dysprosium, dysprosium hydride, dysprosium oxide, dysprosium fluoride, terbium, terbium hydride, terbium oxide, and terbium fluoride; The heavy rare earth powder particles have an average particle size of 2-100 μm and a D90 / D10 of 1.2-5.
1.
5. The method for preparing a sintered R-Fe-B permanent magnet according to any one of claims 1 to 4, characterized in that: The preparation method comprises: (1) The raw materials are mixed according to the corresponding mass ratio to prepare NdFeB alloy quick-solidification sheets, which are then crushed to obtain magnetic powder of target particle size; (2) The obtained magnetic powder is pressed and cold isostatically pressed to obtain a green body; (3) subjecting the green body to sintering and aging treatment to obtain a sintered NdFeB matrix; (4) The sintered NdFeB matrix is then subjected to high temperature diffusion treatment to obtain the sintered R-Fe-B permanent magnet.
6. The preparation method according to claim 5, characterized in that: In step (1), the pulverizing step specifically comprises: subjecting the NdFeB alloy quick-solidified thin slice to hydrogen explosion to obtain coarse pulverized powder, and then subjecting the powder to high-energy ball milling or air flow milling to obtain magnetic powder; And / or, in step (1), the target particle size of the magnetic powder is 1-8 μm.
7. The preparation method according to claim 5, characterized in that: In step (2), the pressing and molding comprises: pressing and molding the magnetic powder in an orientation manner in a magnetic field; And / or, in step (3), the sintering process comprises: placing the green body in a vacuum environment and sintering it at a high temperature of 1055°C-1090°C; And / or, in step (3), the aging treatment refers to a tempering treatment at a temperature below 1000° C. after sintering.
8. The preparation method according to claim 5, characterized in that: In step (4), the high temperature diffusion treatment specifically includes: coating the surface of the sintered NdFeB substrate with heavy rare earth elements so that the heavy rare earth elements are evenly distributed on the surface of the sintered NdFeB substrate; performing two-stage heat treatment diffusion in a vacuum atmosphere, wherein the temperature range of the first heat treatment is 790°C-900°C but not including 900°C, the temperature range of the second heat treatment is 440°C-530°C, and the vacuum degree is 10 -2 -10 -4 Pa.
9. The preparation method according to claim 8, characterized in that: The heavy rare earth element is provided by a diffusion source; The diffusion source includes heavy rare earth powder particles, an antioxidant and an organic solvent; The heavy rare earth powder particles include at least one or more of dysprosium, dysprosium hydride, dysprosium oxide, dysprosium fluoride, terbium, terbium hydride, terbium oxide, and terbium fluoride; The heavy rare earth powder particles have an average particle size of 2-100 μm and a D90 / D10 of 1.2-5.
1.
10. Use of the sintered R-Fe-B permanent magnet according to any one of claims 1 to 4 in a motor.