Organic solar cell and method for preparing the same

Through layer-by-layer spin coating technology, the formation of ternary active layers in organic solar cells is solved, and the problems of high cost and poor performance of traditional processes are achieved, efficient and low-cost photovoltaic performance improvement is achieved, and it is suitable for industrial production.

CN118613127BActive Publication Date: 2024-11-05SHENZHEN TECH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411074961.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-05
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

The preparation process of traditional ternary active layers is costly and has poor photovoltaic performance. It is impossible to select appropriate solvents based on each component characteristic, which limits the performance of material performance.

Method used

By spin-coating the phosphonic acid-based material on the conductive substrate to form an anode interface modification layer, spin-coating the donor and acceptor solution layer by layer to form binary and ternary active layers, and spin-coating the cathode interface modification layer on the ternary active layer The material forms a metal electrode to control the component ratio and solvent selection of the ternary active layer.

Benefits of technology

The optimization process of organic solar cells is simplified, the preparation cost is reduced, it is suitable for industrial production, significantly improves photovoltaic performance, and is suitable for large-scale preparation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118613127B_ABST
    Figure CN118613127B_ABST
Patent Text Reader

Abstract

The invention discloses an organic solar cell and a preparation method thereof, and relates to the field of battery technology. The method comprises: spin coating a phosphonic acid-based material solution on a conductive substrate to form an anode interface modification layer on the surface of the conductive substrate; spin coating a donor solution on the surface of the anode interface modification layer to form a donor layer on the surface of the anode interface modification layer; spin coating a first acceptor solution on the surface of the donor layer to swell the first acceptor solution into the donor layer to form a binary active layer; spin coating a second acceptor solution on the surface of the binary active layer to swell the second acceptor solution into the binary active layer to form a ternary active layer; spin coating a cathode interface modification layer material solution on the ternary active layer to form a cathode interface modification layer on the surface of the ternary active layer; and forming a metal electrode on the surface of the cathode interface modification layer. The present application aims to solve the problem that the cost of the ternary active layer of an organic solar cell is high and the photovoltaic performance is poor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of battery technology, and in particular to a method for preparing an organic solar cell and an organic solar cell. Background Art

[0002] With the development of new organic semiconductor materials, the photoelectric conversion efficiency of organic solar cells has reached nearly 20%, showing excellent industrialization prospects. The ternary active layer plays a vital role in the performance of organic solar cells.

[0003] The traditional preparation process of the ternary active layer is to directly add different amounts of the third component (donor or acceptor) to the precursor solution, and determine the optimal doping ratio through a complex screening process, which significantly increases the manufacturing time and processing costs. Since the ternary active layer is prepared by dissolving three different components together or dissolving them two by two, the ternary active layer cannot select a suitable processing solvent according to the characteristics of each component, which limits the performance of the material and affects the photovoltaic performance of the prepared ternary active layer. Summary of the invention

[0004] The present invention provides a method for preparing an organic solar cell and an organic solar cell, aiming to solve the problems of high cost and poor photovoltaic performance of a ternary active layer of an organic solar cell.

[0005] In a first aspect, the present invention provides a method for preparing an organic solar cell, the method comprising:

[0006] Providing a conductive substrate, and spin coating a phosphonic acid-based material solution on the conductive substrate to form an anode interface modification layer on the surface of the conductive substrate;

[0007] Preparing a donor solution, and spin-coating the donor solution on the surface of the anode interface modification layer to form a donor layer on the surface of the anode interface modification layer;

[0008] preparing a first receptor solution, and spin coating the first receptor solution on the surface of the donor layer, so that the first receptor solution swells into the donor layer to form a binary active layer;

[0009] preparing a second receptor solution, and spin coating the second receptor solution on the surface of the binary active layer, so that the second receptor solution swells into the binary active layer to form a ternary active layer;

[0010] Preparing a cathode interface modification layer material solution, and spin-coating the cathode interface modification layer material solution on the ternary active layer to form a cathode interface modification layer on the surface of the ternary active layer;

[0011] A metal electrode is formed on the surface of the cathode interface modification layer.

[0012] In a second aspect, the present invention provides an organic solar cell, which is prepared by using the above-mentioned method for preparing an organic solar cell.

[0013] The present application provides a method for preparing an organic solar cell and a solar cell. The method comprises the following steps: providing a conductive substrate, and spin-coating a phosphonic acid-based material solution on the conductive substrate to form an anode interface modification layer on the surface of the conductive substrate; preparing a donor solution, and spin-coating the donor solution on the surface of the anode interface modification layer to form a donor layer on the surface of the anode interface modification layer; preparing a first receptor solution, and spin-coating the first receptor solution on the surface of the donor layer to allow the first receptor solution to swell into the donor layer to form a binary active layer; preparing a second receptor solution, and spin-coating the second receptor solution on the surface of the binary active layer to allow the second receptor solution to swell into the binary active layer to form a ternary active layer; preparing a cathode interface modification layer material solution, and spin-coating the cathode interface modification layer material solution on the ternary active layer to form a cathode interface modification layer on the surface of the ternary active layer; and forming a metal electrode on the surface of the cathode interface modification layer. In this way, the ratio of the three components in the ternary active layer can be controlled, which not only determines the corresponding solvent according to the material properties of each component, but also simplifies the complex optimization process of organic solar cells. It is suitable for industrial production casting. In industry, low-cost coating technology can be used to prepare the ternary active layer, which is conducive to large-scale preparation and has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying any creative work.

[0015] Figure 1 An embodiment of the present invention provides a schematic flow chart of a method for preparing a solar cell;

[0016] Figure 2 The embodiment of the present invention provides a schematic diagram of the molecular structure of 4PADCB and 2PACZ;

[0017] Figure 3 An embodiment of the present invention provides a schematic structural diagram of an anode interface modification layer;

[0018] Figure 4 An embodiment of the present invention provides a schematic diagram of the molecular structure of PM6;

[0019] Figure 5 An embodiment of the present invention provides a schematic structural diagram of a donor layer;

[0020] Figure 6 An embodiment of the present invention provides a schematic diagram of the molecular structure of BTP-eC9;

[0021] Figure 7 An embodiment of the present invention provides a schematic structural diagram of a binary active layer;

[0022] Figure 8 An embodiment of the present invention provides a schematic diagram of the molecular structure of PJ1-γ;

[0023] Fig. 9 An embodiment of the present invention provides a schematic structural diagram of a ternary active layer;

[0024] Fig.10 An embodiment of the present invention provides a schematic structural diagram of a cathode interface modification layer;

[0025] Fig.11 An embodiment of the present invention provides a schematic structural diagram of an organic solar cell;

[0026] Fig.12 It is a schematic diagram of the photovoltaic performance effects of solar cells corresponding to the ternary active layers prepared by different methods proposed in the embodiments of the present application. DETAILED DESCRIPTION

[0027] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] It should be understood that when used in this specification and the appended claims, the terms "include" and "comprises" indicate the presence of described features, integers, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or combinations thereof.

[0029] It should also be understood that the terms used in this specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. As used in the specification of the present invention and the appended claims, unless the context clearly indicates otherwise, the singular forms "a", "an" and "the" are intended to include plural forms.

[0030] It should be further understood that the term "and / or" used in the present description and the appended claims refers to and includes any and all possible combinations of one or more of the associated listed items.

[0031] In conjunction with the accompanying drawings, some embodiments of the present application are described in detail below. In the absence of conflict, the following embodiments and features in the embodiments can be combined with each other.

[0032] Solar energy is a non-polluting and renewable energy source. It is inexhaustible and is the first choice for solving the energy crisis. Solution-processable organic solar cells can directly use sunlight to provide electricity for devices. They have the advantages of being semi-transparent, lightweight, and rollable, and have attracted close attention from academia and industry. With the continuous emergence of high-absorption coefficient non-fullerene acceptors, the photoelectric conversion efficiency of single-junction binary organic solar cells has exceeded 19%. However, since the active layer only uses one donor and one acceptor material, the absorption spectrum range is narrow, which limits the improvement of the device's photocurrent.

[0033] In contrast, adding a suitable third component (donor or acceptor) to the binary system can not only expand the capture of the solar spectrum, but also promote interfacial charge transfer, reduce carrier recombination, and further improve the photoelectric conversion efficiency of the device. However, in the related technology, the preparation process of the ternary active layer is to directly add different amounts of the third component (donor or acceptor) to the precursor solution, and determine the optimal doping ratio through a complex screening process, which significantly increases the manufacturing time and processing costs.

[0034] The present application provides a method for preparing an organic solar cell and an organic solar cell, by which the ratio of three components in a ternary active layer can be controlled, and not only the corresponding solvent can be determined according to the material properties of each component, but also the optimization process of the organic solar cell can be simplified, which is suitable for industrial production casting. In industry, low-cost coating technology can be used to prepare the ternary active layer, which is conducive to large-scale preparation and has good application prospects.

[0035] See also Figure 1 , Figure 1 The present invention provides a schematic flow chart of a method for preparing an organic solar cell. The method for preparing an organic solar cell can control the ratio of the three components in the ternary active layer, and can not only determine the corresponding solvent according to the material properties of each component, but also simplify the complex optimization process of the organic solar cell, which is suitable for industrial production casting. In industry, the ternary active layer can be prepared by low-cost coating technology, which is conducive to large-scale preparation and has a good application prospect.

[0036] like Figure 1As shown, the method for preparing the organic solar cell includes: step S101 to step S106.

[0037] S101, providing a conductive substrate, and spin-coating a phosphonic acid-based material solution on the conductive substrate to form an anode interface modification layer on the surface of the conductive substrate.

[0038] The conductive substrate 10 may be any substrate that can be used for support and conduct electricity, such as transparent conductive glass, indium tin oxide, etc. Figure 2 As shown, the phosphonic acid-based material may include a self-assembled monomolecular material 4-(7H-dibenzo[c,g]carbazole-7-yl)butyl)phosphonic acid (4PADCB) or 2-(9H-carbazole-9-acyl)ethyl)phosphonic acid (2PACZ). The phosphonic acid-based material solution is a solution prepared using a phosphonic acid-based material, and is used to prepare the anode interface modification layer 20. The prepared anode interface modification layer 20 is stacked with the conductive substrate 10.

[0039] In some embodiments, after providing the conductive substrate 10, the conductive substrate 10 is ultrasonically cleaned; the conductive substrate 10 after the ultrasonic cleaning is dried at a constant temperature; the conductive substrate 10 after the constant temperature drying is plasma-ozone cleaned to obtain a cleaned conductive substrate 10. In this way, dust and oil attached to the surface of the conductive substrate 10 can be cleaned to avoid affecting the quality of the prepared solar cell.

[0040] Specifically, the dirt on the surface of the conductive substrate 10 can be wiped off with a cotton swab soaked in anhydrous ethanol, and then the conductive substrate 10 is ultrasonically cleaned in cleaning solution, deionized water, acetone, deionized water, and isopropyl alcohol in sequence for 10-30 minutes, and then the cleaned conductive substrate 10 is placed in a constant temperature box at a temperature of 70-90° C. for drying, and finally the dried conductive substrate 10 is subjected to plasma ozone cleaning for about 2-10 minutes.

[0041] For example, since the commercially purchased conductive substrate 10 will inevitably be attached with dust and oil during transportation, the impurities visible to the naked eye on the surface of the conductive substrate 10 can be removed with a cotton swab soaked in ethanol. Subsequently, the pretreated conductive substrate 10 is ultrasonically cleaned in detergent water, deionized water, acetone, deionized water, and isopropanol in sequence, with each step cleaning for 15 minutes. The cleaned conductive substrate 10 is then transferred to a constant temperature drying oven for treatment for 4 hours. Finally, the dried conductive substrate 10 is plasma ozone cleaned for 6 minutes to enhance the hydrophilicity of the surface of the conductive substrate 10, so that the surface of the conductive substrate 10 can be fully cleaned to facilitate the subsequent preparation of the organic solar cell 100.

[0042] In some embodiments, before the phosphonic acid-based material solution is spin-coated on the conductive substrate 10 to form the anode interface modification layer 20 on the surface of the conductive substrate 10, the phosphonic acid-based material is added to the organic solvent to dissolve the phosphonic acid-based material in the organic solvent; the halogen-free solvent is heated and stirred to obtain the phosphonic acid-based material solution, wherein the concentration of the phosphonic acid-based material solution is 0.3-0.5 mg / ml. Thus, a phosphonic acid-based material solution of the corresponding concentration can be prepared.

[0043] Among them, the phosphonic acid-based material may include a self-assembled monomolecular material 4-(7H-dibenzo[c,g]carbazole-7-yl)butyl)phosphonic acid (4PADCB) or 2-(9H-carbazole-9-acyl)ethyl)phosphonic acid (2PACZ), and the organic solvent may include ethanol and other solvents for dissolving the phosphonic acid-based material.

[0044] For example, the phosphonic acid-based material 2PACZ can be heated and stirred to dissolve in the organic solvent ethanol for 8 hours, thereby preparing a phosphonic acid-based material solution with a concentration of 0.3 mg / ml.

[0045] like Figure 3 As shown, in some embodiments, the first rotation speed is determined according to the concentration of the phosphonic acid-based material solution, and the first rotation speed is 3000 rpm; the coating machine is controlled to spin-coat the phosphonic acid-based material solution on the conductive substrate 10 based on the first rotation speed to form an anode interface modification layer 20 on the surface of the conductive substrate 10; the anode interface modification layer 20 is annealed based on annealing parameters, and the annealing parameters include annealing temperature and annealing time, the annealing temperature is 80-120°C, and the annealing time is 3-7 minutes.

[0046] The thickness of the anode interface modification layer 20 may be 10-40 nm, which may be determined according to the concentration of the phosphonic acid-based material solution and the first rotation speed.

[0047] Specifically, the first rotation speed of the coating machine is determined according to the thickness of the anode interface modification layer 20 to be prepared and the concentration of the phosphonic acid-based material solution, and then the coating machine is controlled to spin-coat the phosphonic acid-based material solution on the conductive substrate 10 at the first rotation speed, thereby forming an anode interface modification layer 20 with a target thickness on the surface of the conductive substrate 10.

[0048] Exemplarily, the first rotation speed of the coating machine can be determined to be 3000 rpm according to the thickness of the anode interface modification layer 20 to be prepared and the concentration of the phosphonic acid-based material solution, and then the coating machine is controlled to spin-coat the phosphonic acid-based material solution on the conductive substrate 10 at a rotation speed of 3000 rpm to form a 30 nm anode interface modification layer 20 on the surface of the conductive substrate 10. Finally, the anode interface modification layer 20 is annealed on the heating table, and the annealing temperature is controlled to be 100° C. and the annealing time is 5 minutes.

[0049] S102, preparing a donor solution, and spin-coating the donor solution on the surface of the anode interface modification layer to form a donor layer on the surface of the anode interface modification layer.

[0050] The donor solution may be a solution prepared by using a donor material, and is used to prepare the donor layer 31 . The prepared donor layer 31 is stacked with the anode interface modification layer 20 .

[0051] In some embodiments, a donor material is obtained, and a first solvent is determined based on the donor material; the donor material is added to the first solvent to dissolve the donor material in the first solvent; the first solvent is heated and stirred to obtain a donor solution, and the concentration of the donor solution is 5-10 mg / ml.

[0052] like Figure 4 As shown, the donor material may be a polymer donor material (PBDB-TF, PM6), and the first solvent may include toluene, o-xylene or chloroform, etc., which are solvents that can be used to dissolve the polymer donor material.

[0053] Specifically, the first solvent can be determined according to the donor material, and the donor material can be dissolved in the first solvent to form a donor layer solution, and the concentration of the donor layer solution can be controlled at 5-10 mg / ml.

[0054] For example, the first solvent can be determined to be toluene based on the donor material PM6, and then the polymer donor material PM6 is dissolved in toluene and heated and stirred for 2 hours to dissolve, thereby preparing a donor layer 31PM6 solution with a concentration of 8 mg / ml.

[0055] It should be noted that the first solvent can select the most suitable solvent according to the physical properties of the donor material, so that the donor material can be fully dissolved in the first solvent by utilizing the physical properties, thereby obtaining the optimal donor layer solution. The concentration of the donor layer solution can be determined according to the required thickness of the donor layer 31, and no specific limitation is made here.

[0056] like Figure 5 As shown, in some embodiments, the second rotation speed of the coating machine is determined according to the concentration of the donor solution, and the second rotation speed is 2800 rpm; the coating machine is controlled to spin-coat the donor solution on the anode interface modification layer 20 based on the second rotation speed to form a donor layer 31 on the surface of the anode interface modification layer 20. In this way, a donor layer 31 with a specific thickness can be prepared on the surface of the conductive substrate 10.

[0057] Specifically, the second speed of the coater is determined according to the thickness of the donor layer 31 to be prepared and the concentration of the donor solution, and then the coater is controlled to spin-coat the donor solution on the anode interface modification layer 20 at the second speed, and cooled and dried for 10-30 minutes, thereby forming a donor layer 31 with a target thickness on the surface of the anode interface modification layer 20.

[0058] Exemplarily, the second speed of the coating machine can be determined to be 2800 rpm based on the thickness of the donor layer 31 to be prepared and the concentration of the donor solution, and then the coating machine is controlled to spin-coat the donor solution on the anode interface modification layer 20 at a speed of 2800 rpm, and cooled and dried for 10-30 minutes, thereby forming a PM6 film with a target thickness on the surface of the anode interface modification layer 20.

[0059] S103, preparing a first receptor solution, and spin-coating the first receptor solution on the surface of the donor layer, so that the first receptor solution swells into the donor layer to form a binary active layer.

[0060] The first acceptor solution may be a solution prepared by acceptor materials. The first acceptor solution is used to swell the donor layer 31 to form a binary active layer 32 . The prepared binary active layer 32 is stacked with the anode interface modification layer 20 .

[0061] In some embodiments, a first receptor material is obtained, and a second solvent is determined based on the first receptor material, and the first receptor material is added to the second solvent so that the first receptor material is dissolved in the second solvent; the second solvent is heated and stirred to obtain a first receptor solution, and the concentration of the first receptor solution is 1-4 mg / ml.

[0062] like Figure 6 As shown, the first acceptor material may be an organic photovoltaic OPV material BTP-eC9, and the second solvent may include toluene, o-xylene or chloroform and other solvents that can be used to dissolve the acceptor material.

[0063] Specifically, the second solvent can be determined according to the first receptor material, and the first receptor material can be dissolved in the second solvent to form a first receptor solution, and the concentration of the first receptor solution can be controlled at 1-4 mg / ml.

[0064] For example, the second solvent can be determined to be o-xylene based on the organic photovoltaic OPV material BTP-eC9, and then the organic photovoltaic OPV material BTP-eC9 is dissolved in o-xylene and heated and stirred for 2 hours to prepare a first receptor solution with a concentration of 2 mg / ml.

[0065] It should be noted that the second solvent can select the most suitable solvent according to the physical properties of the first receptor material, so that the first receptor material can be fully dissolved in the second solvent by utilizing the physical properties, thereby obtaining the optimal first receptor solution. The concentration of the first receptor solution can be determined according to the required thickness of the binary active layer 32, and is not specifically limited here.

[0066] like Figure 7 As shown, in some embodiments, the third speed of the coating machine is determined according to the concentration of the first acceptor solution, and the third speed is 3000 rpm; the coating machine is controlled to spin-coat the first acceptor solution on the surface of the donor layer 31 based on the third speed, so that the first acceptor solution swells into the donor layer 31 to form a binary active layer 32. In this way, a binary active layer 32 of a specific thickness can be prepared on the surface of the anode interface modification layer 20.

[0067] Specifically, the third speed of the coating machine is determined according to the thickness of the binary active layer 32 to be prepared and the concentration of the first acceptor solution, and then the coating machine is controlled to spin-coat the first acceptor solution on the donor layer 31 at the third speed, and cooled and dried for 10-30 minutes to allow the first acceptor solution to swell into the donor layer 31 to form a binary active layer 32 with a target thickness on the surface of the anode interface modification layer 20.

[0068] Exemplarily, the third speed of the coating machine can be determined to be 3000 rpm according to the thickness of the binary active layer 32 to be prepared and the concentration of the first acceptor solution, and then the coating machine is controlled to spin-coat the first acceptor solution on the PM6 layer at a speed of 3000 rpm, and cooled and dried for 10-30 minutes to allow the first acceptor solution to swell into the PM6 layer to form a PM6 / BTP-eC9-4F film with a target thickness on the surface of the anode interface modification layer 20.

[0069] S104, preparing a second receptor solution, and spin-coating the second receptor solution on the surface of the binary active layer, so that the second receptor solution swells into the binary active layer to form a ternary active layer.

[0070] The second acceptor solution may be a solution prepared by acceptor materials, and the second acceptor solution is used to swell the ternary active layer 30 to form the ternary active layer 30 . The prepared ternary active layer 30 is stacked with the anode interface modification layer 20 .

[0071] In some embodiments, a second receptor material is obtained, and a third solvent is determined based on the second receptor material, and the second receptor material is added to the third solvent so that the second receptor material is dissolved in the third solvent; the third solvent is heated and stirred to obtain a second receptor solution, and the concentration of the second receptor solution is 6-12 mg / ml.

[0072] like Figure 8As shown, the second receptor material may be a polymer receptor material PJ1-γ, such as poly-NFA, and the third solvent may include toluene, o-xylene or chloroform, etc., which can be used to dissolve the receptor material.

[0073] Specifically, the third solvent can be determined according to the second receptor material, and the second receptor material can be dissolved in the third solvent to form a second receptor solution, and the concentration of the second receptor solution can be controlled at 6-12 mg / ml.

[0074] For example, the third solvent can be determined to be chloroform based on the polymer receptor material PJ1-γ, and then the polymer receptor material PJ1-γ is dissolved in chloroform and heated and stirred for 2 hours to prepare a second receptor solution with a concentration of 10.4 mg / ml.

[0075] It should be noted that the third solvent can select the most suitable solvent according to the physical properties of the second receptor material, so that the second receptor material can be fully dissolved in the third solvent by utilizing the physical properties, thereby obtaining the optimal second receptor solution. The concentration of the second receptor solution can be determined according to the required thickness of the ternary active layer 30, which is not specifically limited here.

[0076] like Fig. 9 As shown, in some embodiments, the fourth speed of the coating machine is determined according to the concentration of the second receptor solution, and the fourth speed is 3200 rpm; the coating machine is controlled to spin-coat the second receptor solution on the surface of the binary active layer 32 based on the tenth speed, so that the second receptor solution swells into the binary active layer 32 to form the ternary active layer 30. In this way, the ternary active layer 30 of a specific thickness can be prepared on the surface of the anode interface modification layer 20.

[0077] The thickness of the ternary active layer 30 may be 50-300 nm, and the specific thickness may be determined according to the thickness of the binary active layer 32 , the concentration of the second receptor solution, and the fourth rotation speed.

[0078] It should be noted that the thickness of the ternary active layer 30 can be comprehensively determined by comprehensively controlling the concentration of the donor layer solution, the concentration of the first acceptor solution and the concentration of the second acceptor solution and controlling the corresponding rotation speed of the coating machine.

[0079] Specifically, the fourth speed of the coating machine is determined according to the thickness of the ternary active layer 30 to be prepared and the concentration of the second acceptor solution, and then the coating machine is controlled to spin-coat the second acceptor solution on the binary active layer 32 at the fourth speed, and cooled and dried for 10-30 minutes to allow the second acceptor solution to swell into the binary active layer 32 to form a ternary active layer 30 with a target thickness on the surface of the anode interface modification layer 20.

[0080] Exemplarily, the fourth speed of the coating machine can be determined to be 3200 rpm according to the thickness of the ternary active layer 30 to be prepared and the concentration of the second acceptor solution, and then the coating machine is controlled to spin-coat the first acceptor solution on the PM6 / BTP-eC9-4F layer at a speed of 3200 rpm, and cooled and dried for 10-30 minutes to allow the first acceptor solution to swell into the PM6 / BTP-eC9-4F layer to form a PM6 / BTP-eC9-4F / PJ1-γ active layer with a target thickness on the surface of the anode interface modification layer 20.

[0081] It can be seen that the ternary active layer 30 prepared by the present application can determine the corresponding solvent according to the material properties of each component, and can adjust the rotation speed of each component by the coating machine, so that the various components of the ternary active layer 30 can reach the optimal ratio. At the same time, it can also simplify the complex optimization process of the organic solar cell 100, which is suitable for industrial production casting. In industry, low-cost coating technology can be used to prepare the ternary active layer 30, which is conducive to large-scale preparation and has a good application prospect.

[0082] S105, preparing a cathode interface modification layer material solution, and spin-coating the cathode interface modification layer material solution on the ternary active layer to form a cathode interface modification layer on the surface of the ternary active layer.

[0083] The cathode interface modification layer 40 is prepared on the surface of the ternary active layer 30 by spin coating a cathode interface modification layer 40 material solution, and is stacked with the ternary active layer 30 .

[0084] In some embodiments, the cathode interface modification layer 40 material is added to an organic solvent to dissolve the cathode interface modification layer 40 material in the organic solvent; the organic solvent is stirred to obtain a cathode interface modification layer 40 material solution, and the concentration of the cathode interface modification layer 40 material solution is 0.5-1 mg / ml. In this way, a cathode interface modification layer 40 material solution with a corresponding concentration can be prepared.

[0085] The material of the cathode interface modification layer 40 may include a material capable of forming the cathode interface modification layer 40 , such as a PNDIT-F3N material.

[0086] Specifically, the PNDIT-F3N material is dissolved in an organic solvent, and then stirred to form a cathode interface modification layer 40 material solution with a concentration of about 0.5-1 mg / ml.

[0087] Exemplarily, a mixed solvent of methanol and acetic acid can be used to dissolve the cathode interface modification layer 40 material PNDIT-F3N, and the ratio of methanol to acetic acid can be 1000:5, so as to stir to form a cathode interface modification layer 40 material solution, and the concentration of the cathode interface modification layer 40 material solution is 0.5 mg / ml.

[0088] like Fig.10 As shown, in some embodiments, the fifth speed of the coating machine is determined according to the concentration of the cathode interface modification layer 40 material solution; the coating machine is controlled to spin-coat the cathode interface modification layer 40 material solution on the ternary active layer 30 based on the fifth speed to form the cathode interface modification layer 40 on the surface of the ternary active layer 30, and the thickness of the cathode interface modification layer 40 is 5-30nm. In this way, a cathode interface modification layer 40 with a specific thickness can be prepared on the ternary active layer 30.

[0089] Specifically, the cathode interface modification layer 40 material solution is spin-coated on the prepared ternary active layer 30 and left to dry for 7-10 minutes, and the thickness of the cathode interface modification layer 40 can be controlled within the range of 5-30 nm.

[0090] Exemplarily, a coating machine is used to spin-coat the cathode interface modification layer 40 material solution onto the prepared photosensitive mixed layer, the rotation speed is controlled at 2000 rpm, and the coating time is 30 s, thereby forming the cathode interface modification layer 40 on the surface of the photosensitive mixed layer, and the thickness of the cathode interface modification layer 40 is controlled at 15 nm.

[0091] S106, forming a metal electrode on the surface of the cathode interface modification layer.

[0092] The metal electrode 50 may include a silver electrode, a gold electrode, an aluminum electrode, or the like.

[0093] like Fig.11 As shown, in some embodiments, a thermal evaporation device is used to dissolve metal; based on a preset vacuum condition, the dissolved metal is evaporated onto the cathode interface modification layer 40 to form a metal electrode 50 on the surface of the cathode interface modification layer 40, and the thickness of the metal electrode 50 is 20-200nm. Thus, a metal electrode 50 with a specific thickness can be prepared on the surface of the cathode interface modification layer 40.

[0094] Specifically, metallic silver can be placed on a tungsten boat and placed under high vacuum conditions, and the metallic silver can be evaporated onto the cathode interface modification layer 40 by thermal evaporation, thereby forming a silver electrode on the surface of the cathode interface modification layer 40, and the thickness of the metal electrode 50 can be controlled within the range of 20-200nm.

[0095] For example, the silver metal is dissolved by thermal evaporation equipment under a vacuum degree of 1×10 -4 Under the condition of Pa, metallic silver will liquefy, and at this time the liquid silver will vaporize onto the cathode interface modification layer 40 to form a silver electrode, and the thickness of the silver electrode is 100 nm, thereby preparing an organic solar cell 100.

[0096] See also Fig.12, Fig.12 Schematic diagram of the photovoltaic performance effect of the organic solar cell 100 corresponding to the ternary active layer 30 obtained by different preparation methods proposed in the embodiments of the present application.

[0097] Fig.12 The photovoltaic performance of the solar cell corresponding to the ternary active layer 30 prepared by the acceptor mixed solution formed by three components (Example 1), the photovoltaic performance of the solar cell corresponding to the ternary active layer 30 prepared by the acceptor mixed solution formed by two components (Example 2), and the photovoltaic performance of the solar cell corresponding to the ternary active layer 30 prepared by the donor layer solution, the first acceptor solution and the second acceptor solution (Example 3) are shown.

[0098] The photovoltaic performance of Example 1, Example 2 and Example 3 is under the AM1.5G standard simulated sunlight source, and the light intensity is controlled at 100mW / cm 2 , and the donor material is PM6, the first acceptor material is BTP-eC9, and the second acceptor material is PJ1-γ. In Example 1, the PM6 / BTP-eC9 / PJ1-γ layer is prepared by preparing a mixed acceptor solution of PM6, BTP-eC9 and PJ1-γ; in Example 2, the PM6 layer is first prepared by a PM6 solution, and then a mixed acceptor solution of BTP-eC9 and PJ1-γ is prepared and spin-coated on the PM6 layer to prepare the PM6 / BTP-eC9 / PJ1-γ layer; in Example 3, the PM6 layer is first prepared by a PM6 solution, and then a PM6 / BTP-eC9 layer is prepared on the PM6 layer by a BTP-eC9 solution, and finally a PM6 / BTP-eC9 / PJ1-γ layer is prepared on the PM6 / BTP-eC9 layer by a PJ1-γ solution.

[0099] It should be noted that the above solutions all use the most suitable solvent to dissolve the materials.

[0100] Depend on Fig.12 The photovoltaic performances of Example 1, Example 2 and Example 3 can be obtained as shown in Table 1.

[0101] Table 1

[0102]

[0103] As can be seen from Table 1, the photovoltaic performance of the solar cell corresponding to the ternary active layer 30 prepared by the donor layer solution, the first acceptor solution and the second acceptor solution has been greatly improved, and the corresponding short-circuit current density J SC , fill factor FF and photoelectric conversion efficiency (PCE) reached 27.352 mA / cm 2, 75.667% and 19.175%, and the photoelectric conversion efficiency PCE is greatly increased to 19.10%. Compared with Example 1 and Example 2, they are significantly increased. It can be seen that the preparation method of the organic solar cell 100 proposed in the embodiment of the present application can significantly improve the photovoltaic performance of the organic solar cell 100, and has good universality, and can greatly simplify the advanced sequential deposition process, has a good application prospect, and is very suitable for industrial-grade preparation and production.

[0104] The present application provides a method for preparing an organic solar cell 100 and an organic solar cell 100, by which the ratio of the three components in the ternary active layer 30 can be controlled, and not only the corresponding solvent can be determined according to the material properties of each component, but also the complex optimization process of the organic solar cell 100 can be simplified, which is suitable for industrial production casting. In industry, low-cost coating technology can be used to prepare the ternary active layer 30, which is conducive to large-scale preparation and has a good application prospect.

[0105] The embodiment of the present application further provides an organic solar cell 100 , which is prepared by using the method for preparing the organic solar cell 100 provided by any of the above embodiments.

[0106] The specific method of preparing the organic solar cell can refer to the corresponding embodiment recorded in the specification of this application, and this embodiment will not be repeated here. The organic solar cell provided by the embodiment of this application has high photovoltaic performance, low manufacturing cost, and can be prepared on a large scale, and has good application prospects.

[0107] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can easily think of various equivalent modifications or replacements within the technical scope disclosed by the present invention, and these modifications or replacements should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be based on the protection scope of the claims.

Claims

1. A method for preparing an organic solar cell, characterized in that: The method comprises: Providing a conductive substrate, and spin coating a phosphonic acid-based material solution on the conductive substrate to form an anode interface modification layer on the surface of the conductive substrate; Preparing a donor solution, and spin-coating the donor solution on the surface of the anode interface modification layer to form a donor layer on the surface of the anode interface modification layer; preparing a first receptor solution, and spin coating the first receptor solution on the surface of the donor layer, so that the first receptor solution swells into the donor layer to form a binary active layer; preparing a second receptor solution, and spin coating the second receptor solution on the surface of the binary active layer, so that the second receptor solution swells into the binary active layer to form a ternary active layer; Preparing a cathode interface modification layer material solution, and spin-coating the cathode interface modification layer material solution on the ternary active layer to form a cathode interface modification layer on the surface of the ternary active layer; forming a metal electrode on the surface of the cathode interface modification layer; The preparation of the donor solution comprises: Obtaining a donor material, and determining a first solvent according to the donor material; adding the donor material to a first solvent so that the donor material is dissolved in the first solvent; Heating and stirring the first solvent to obtain the donor solution, wherein the concentration of the donor solution is 5-10 mg / ml; The step of preparing the first receptor solution comprises: obtaining a first receptor material, and determining a second solvent according to the first receptor material; adding the first receptor material to a second solvent so that the first receptor material is dissolved in the second solvent; heating and stirring the second solvent to obtain the first receptor solution, wherein the concentration of the first receptor solution is 1-4 mg / ml; The step of preparing the second receptor solution comprises: obtaining a second receptor material, and determining a third solvent based on the second receptor material; adding the second receptor material to a third solvent so that the second receptor material is dissolved in the third solvent; The third solvent is heated and stirred to obtain the second receptor solution, wherein the concentration of the second receptor solution is 6-12 mg / ml.

2. The method according to claim 1, characterized in that The step of spin coating the donor solution on the surface of the anode interface modification layer to form a donor layer on the surface of the anode interface modification layer comprises: Determining a second rotation speed of the coating machine according to the concentration of the donor solution, wherein the second rotation speed is 2800 rpm; The coating machine is controlled to spin-coat the donor solution on the anode interface modification layer based on the second rotation speed to form a donor layer on the surface of the anode interface modification layer.

3. The method according to claim 1, characterized in that The method of spin coating the first receptor solution on the surface of the donor layer so that the first receptor solution swells into the donor layer to form a binary active layer comprises: Determining a third rotation speed of the coating machine according to the concentration of the first receptor solution, wherein the third rotation speed is 3000 rpm; The coating machine is controlled to spin-coat the first acceptor solution on the surface of the donor layer based on the third rotation speed, so that the first acceptor solution swells into the donor layer to form a binary active layer.

4. The method according to claim 1, characterized in that The step of spin coating the second receptor solution on the surface of the binary active layer so that the second receptor solution swells into the binary active layer to form a ternary active layer comprises: Determining a fourth rotation speed of the coating machine according to the concentration of the second receptor solution, wherein the fourth rotation speed is 3200 rpm; The coating machine is controlled to spin-coat the second receptor solution on the surface of the binary active layer based on the fourth rotation speed, so that the second receptor solution swells into the binary active layer to form a ternary active layer, and the thickness of the ternary active layer is controlled to be 50-300nm.

5. The method according to claim 1, characterized in that The method of spin coating the phosphonic acid-based material solution on the conductive substrate to form an anode interface modification layer on the surface of the conductive substrate comprises: Determining a first rotation speed of the coating machine according to the concentration of the phosphonic acid-based material solution, wherein the first rotation speed is 3000 rpm; Controlling the coating machine to spin-coat the phosphonic acid-based material solution on the conductive substrate based on the first rotation speed to form an anode interface modification layer on the surface of the conductive substrate, wherein the thickness of the anode interface modification layer is 10-40 nm; The anode interface modification layer is annealed based on annealing parameters, wherein the annealing parameters include annealing temperature and annealing time, wherein the annealing temperature is 80-120° C., and the annealing time is 3-7 minutes.

6. The method according to claim 1, characterized in that The step of forming a metal electrode on the surface of the cathode interface modification layer comprises: Dissolving metals using thermal evaporation equipment; Based on the preset vacuum conditions, the dissolved metal is evaporated onto the cathode interface modification layer to form a metal electrode on the surface of the cathode interface modification layer, and the thickness of the metal electrode is 20-200 nm.