A system and method for producing yellow phosphorus by smelting phosphate ore
By using a combination process of an oxidation smelting furnace and a reduction furnace in phosphate smelting, the problem of high requirements for furnace charge and difficulty in utilization of yellow phosphorus exhaust gas in electric furnace is solved, and efficient, low-carbon and clean yellow phosphorus production is achieved, reducing the number of yellow phosphorus production. Energy consumption and environmental pollution.
Patent Information
- Application Number
- CN202411111872.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-14
AI Technical Summary
The existing electric furnace yellow phosphorus method has high requirements for furnace materials, and yellow phosphorus exhaust gas is difficult to utilize. The reuse of phosphorus sludge affects normal production, resulting in high energy consumption and environmental pollution.
The oxidation and smelting furnace is used to obtain liquid high-phosphorus slag, and a reducing agent is added to the reduction furnace for reduction to generate high-quality phosphorus-containing flue gas. The yellow phosphorus is recovered through condensation, and the moisture content and particle size range of the furnace material are optimized, and the acidity coefficient is controlled. Temperature, reduce the loss of phosphorus and the emission of harmful elements.
It has achieved low-carbon and clean yellow phosphorus production, reduced energy consumption and environmental pollution, improved the utilization rate of phosphate ore and product quality, and reduced equipment investment and labor intensity.
Smart Images

Figure CN118619220B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of phosphate ore smelting, and in particular to a system and method for producing yellow phosphorus by smelting phosphate ore. Background Art
[0002] The main process technology for the current yellow phosphorus production is the electric furnace yellow phosphorus method, which usually involves mixing phosphate ore and silica in proportion and adding them to a reactor for melting. After the melt reaches a certain height, the phosphate ore, silica, and carbon mixture are directly added to the high-temperature melt in the reactor, and the carbon is maintained in excess to cause the melt to undergo a reduction reaction, and then flue gas and phosphorus mud are obtained. The flue gas mainly contains gasified yellow phosphorus and CO. The flue gas is separated and purified to obtain yellow phosphorus products and CO-rich yellow phosphorus tail gas. All the heat required for the production of yellow phosphorus is provided by electricity, and the electricity consumption per ton of yellow phosphorus is about 14,000 to 16,000 kWh, which is a relatively high energy consumption.
[0003] The yellow phosphorus tail gas from traditional electric furnaces contains impurities such as phosphorus, sulfur, arsenic, and fluorine. Practice has shown that burning untreated yellow phosphorus tail gas has strong corrosiveness because it contains many harmful elements and highly corrosive substances. If used as synthesis gas, the various catalysts of synthesis gas have more stringent requirements on impurities and must also be deeply purified; therefore, yellow phosphorus tail gas is difficult to utilize. In addition, during the electric furnace smelting process, a portion of solid dust is always brought out, and the dust content of the furnace gas is 20~50g / Nm 3 If high-carbonate phosphate ore is encountered, the dust will be brought out due to decomposition and crushing at high temperature, which is more serious. The dust content in the furnace gas is as high as 100 g / Nm 3 The above factors greatly affect the quality of yellow phosphorus.
[0004] At the same time, in the traditional electric furnace yellow phosphorus method, excessive moisture content in the charge often worsens the operation, blocks the charge pipe, makes the charge unsmooth, and causes agglomeration and bridging in the electric furnace, causing the charge to collapse, resulting in flames and even explosions; and a large amount of free water enters the furnace, the side reactions increase, the tail gas volume increases, and the content of impurities such as PH3 and H2S in the yellow phosphorus tail gas also increases. Especially in the rainy season, when the moisture content of the raw materials increases, the H2S content in the yellow phosphorus tail gas increases significantly, causing adverse effects on desulfurization. Due to the increase in side reactions, the consumption of raw carbon and electrodes increases, the recovery rate of elemental phosphorus decreases, and the output of product phosphorus decreases.
[0005] Therefore, conventionally, to obtain high-quality yellow phosphorus, the materials entering the furnace need to be dried to a moisture content of less than 2%, and the powder ore needs to be granulated and pelletized before entering the furnace, that is, the phosphate ore needs to be dried, granulated, and other pre-treatments before entering the electric furnace for reduction smelting. For example: Chinese patent application CN107686099A discloses an apparatus and method for producing yellow phosphorus using medium and low-grade phosphate ore, in which the phosphate ore is first processed using a grinding unit and a pelletizing and drying unit to prepare granular materials with low moisture content and a certain particle size, and then the granular materials are put into the furnace for reduction reaction to produce yellow phosphorus. This method can avoid the generation of excessive by-products and dust during the reduction reaction in the furnace, thereby improving the quality of the yellow phosphorus product.
[0006] Phosphorus mud is a byproduct of phosphorus production in electric furnaces and is a hazardous solid waste. Mud phosphorus disposal is an important part of yellow phosphorus production. It not only affects the recovery rate and production cost of yellow phosphorus, but also causes pollution to the surrounding environment. In order to achieve energy conservation and emission reduction, protect the environment, and save resources, it is necessary to effectively recycle and utilize mud phosphorus, as well as reduce the amount of mud phosphorus at the source. At present, the phosphorus evaporation method is used to dispose of rich mud phosphorus, while the lean mud phosphorus is directly returned to the electric furnace for smelting to form high-phosphorus slag for disposal. During the process of returning mud phosphorus to the electric furnace for disposal, elemental phosphorus and water react with each other at high temperature, and the products are hypophosphorous acid (H3PO2) and a small amount of phosphine gas (H3P) and hydrogen (H2), which causes the loss of elemental phosphorus. Hypophosphorous acid reacts with dust, destroying the permeability of raw materials and affecting normal production. Phosphine gas and hydrogen have a low lower explosion limit, which poses certain safety hazards. Summary of the invention
[0007] Therefore, the technical problem to be solved by the present invention is to overcome the defects of the electric furnace yellow phosphorus method in the prior art, such as high requirements on furnace charge, difficulty in utilizing yellow phosphorus tail gas, and impact of phosphorus mud recycling on normal production, thereby providing a system and method for producing yellow phosphorus by smelting phosphate ore to solve the above problems.
[0008] A method for producing yellow phosphorus by smelting phosphate ore comprises: obtaining liquid high-phosphorus slag, adding a reducing agent to the liquid high-phosphorus slag for reduction to obtain phosphorus-containing flue gas, and condensing the phosphorus-containing flue gas to obtain yellow phosphorus;
[0009] The liquid high-phosphorus slag is obtained in an oxidation smelting furnace, and the reducing agent is added and the yellow phosphorus is obtained in a reduction furnace;
[0010] The process of obtaining liquid high-phosphorus slag is as follows: phosphate ore and slag-making flux are mixed to obtain a mixture with an acidity coefficient of 0.65-0.85, and the mixture is oxidatively smelted in an oxidation smelting furnace to obtain molten liquid high-phosphorus slag.
[0011] The acidity coefficient is the mass ratio of SiO2 / CaO. If the acidity is too low or too high, the melting point of the slag will increase and the viscosity will be large, which will affect the fluidity of the metallurgical slag and the reduction behavior of phosphorus in the reduction period; in addition, if the acidity is too high, the phosphorus grade of the mixed phosphate ore will be reduced due to the excessive ratio of the flux, and the unit production cost of phosphorus will be increased; therefore, the acidity coefficient of the mixed material obtained by mixing the phosphate ore and the slag-making flux in the present invention is set to 0.65-0.85.
[0012] In the oxidation smelting and reduction steps of the present invention, if the temperature is too low, the fluidity of the slag is reduced, the subsequent phosphorus reduction is affected, and the discharge of the slag is not conducive, resulting in the difficulty of the process; if the temperature is too high, the unit energy consumption of smelting is increased, the production cost is increased, and the service life of the refractory material of the oxidation furnace is affected. Therefore, the temperature of the oxidation smelting and reduction in the present invention is preferably 1350°C-1500°C.
[0013] The traditional electric furnace process requires that the moisture content of the raw materials entering the furnace must be <2%. For raw materials with a moisture content higher than 2%, it is necessary to carry out the drying and granulation process of the raw materials, which limits the application of the raw materials. After the present invention optimizes the operating process, the moisture content of the raw materials is applicable to a wider range, which can meet the requirements of raw materials with a moisture content of more than 2% directly entering the furnace, shortening the process flow and reducing production costs. However, if the moisture content is too high, a large amount of heat will be taken away in the form of water vapor, resulting in high energy consumption for yellow phosphorus smelting. The moisture content of the mixed material described in the present invention is preferably less than 12%, more preferably 2% to 5%.
[0014] If the particle size is too large, it will take a long time for the material to be completely melted; the particle size of the mixed material in the present invention is preferably ≤50mm.
[0015] In the liquid high-phosphorus slag, the amount of the reducing agent added can be 1 times or more of the theoretical amount, preferably 1 to 2 times, and more preferably 1 to 1.3 times.
[0016] The reducing agent includes at least one of anthracite, blue carbon, graphite powder and coke;
[0017] The slag-making flux is silica, quartz stone, etc.; the fuel is pulverized coal or natural gas, etc.
[0018] If the reducing agent particles are too large, the contact interface between the reaction medium is small and the reaction time is long; if the particles are too small, the dust rate is too high. In the present invention, the reducing agent preferably has a particle size of 15 to 35 mm, which can ensure that the reducing agent participates in the reduction reaction to the greatest extent.
[0019] A system for producing yellow phosphorus by smelting phosphate ore, comprising:
[0020] Oxidation smelting furnace, used for oxidative smelting of phosphate ore and slag-making flux into molten liquid high-phosphorus slag;
[0021] The reduction furnace comprises a liquid high-phosphorus slag input port, a reducing material input port and a phosphorus-containing flue gas outlet, and is used for reducing the liquid high-phosphorus slag to obtain the phosphorus-containing flue gas;
[0022] The water shower tower is connected to the phosphorus-containing flue gas outlet and is used to condense and recover yellow phosphorus products from the phosphorus-containing flue gas.
[0023] The oxidation smelting furnace is a side-blown furnace, a top-blown furnace, a bottom-blown furnace, a top-side combined blowing furnace, and a top-bottom combined blowing furnace; wherein phosphate rock powder, fuel, etc. can be selectively sprayed directly into the molten pool using a loading side-blowing spray gun, which can improve the direct utilization rate of the powdered phosphate rock; when the liquid level of the high-phosphorus slag melt in the side-blown furnace reaches the discharge height, it is discharged periodically and the liquid high-phosphorus slag is transferred into a closed reduction furnace.
[0024] The reduction furnace is an electric furnace, preferably a side-blown electric furnace.
[0025] The technical solution of the present invention has the following advantages:
[0026] 1. The present invention provides a method for producing yellow phosphorus by smelting phosphate ore, which proposes to use an oxidation smelting furnace to quickly oxidize and melt a phosphate ore mixture to prepare molten liquid high-phosphorus slag, which can avoid the need to set requirements on the particle size and water content of the charge, broaden the applicable charge range, and is not affected by the reuse of phosphorus mud; at the same time, by controlling the acidity coefficient of the mixed material composed of phosphate ore and slag-making flux to be 0.65-0.85, the loss of phosphorus element caused by the volatilization of phosphorus element in the process of preparing the molten liquid high-phosphorus slag can be reduced; and in this step, harmful elements and moisture can be effectively removed, avoiding the problem of low quality of phosphorus-containing flue gas when the molten liquid high-phosphorus slag enters the reduction furnace for reduction volatilization and phosphorus refining to volatilize phosphorus into the flue gas to obtain phosphorus-containing flue gas, thereby overcoming the problem of difficult utilization of yellow phosphorus tail gas, and finally obtaining yellow phosphorus product by condensing and recovering high-quality phosphorus-containing flue gas through a multi-stage water shower tower, thereby achieving the purpose of efficient, low-carbon and clean disposal of phosphate ore.
[0027] Among them, the phosphate ore is directly treated by oxidation smelting first. Because the melting process is controlled by oxidation smelting under a specific acidity coefficient, the oxygen potential in the furnace is relatively high, and the phosphorus element in the phosphate ore is not easy to volatilize and enter the slag to form high-phosphorus slag, avoiding the loss of phosphorus element; the oxidation smelting furnace is a molten pool smelting, and there is no raw material layer, so the material state and moisture content of the phosphate ore are not required, and the application range is wider. At the same time, in the process of returning the mud phosphorus to the oxidation smelting furnace for melting, no explosive gases such as phosphine and hydrogen similar to electric furnaces will be generated. Therefore, the oxidation smelting furnace has potential technical advantages for the comprehensive treatment of mud phosphorus. Moreover, during the melting process of the oxidation smelting furnace, oxidation smelting can be used to remove harmful elements such as sulfur, arsenic, fluorine, and chlorine (S, As, F, Cl) in the phosphate ore, and at the same time remove water (H2O) brought by the materials entering the furnace, thereby improving the quality of the volatile phosphorus-containing flue gas of the reduction furnace, reducing the corrosiveness of the furnace gas, and reducing the furnace gas emissions. The furnace gas of the reduction furnace has a high CO content, a high phosphorus concentration, and a low impurity content, which is convenient for reducing the subsequent flue gas purification and disposal load and the corresponding cost, as well as the subsequent acquisition of high-quality yellow phosphorus.
[0028] Specifically, the oxidation smelting furnace mainly completes the melting of the furnace charge, and the phosphorus element is still retained in the slag to form liquid high-phosphorus slag. During the melting process, harmful elements (S, As, F, Cl, I, Na, etc.) and the moisture (H2O) contained in the material entering the reduction furnace can be effectively removed, providing a removal effect for the subsequent reduction furnace to carry out reduction volatilization phosphorus refining, improving the purity of the phosphorus-containing flue gas in the reduction furnace, reducing the smoke rate, reducing the mud phosphorus output in the phosphorus collection process, and improving the phosphorus yield. At the same time, because the oxidation smelting furnace can remove moisture during the melting process, the oxidation smelting furnace has a wide range of applications for the moisture content and particle size (powder ore, lump ore, and pellets) of the furnace charge entering the furnace. The charge with a moisture content of less than 12% can enter the furnace, which can reduce the material drying and powder granulation processes, or the residual heat of the melting furnace flue gas can be used to dry the raw materials, avoiding the investment in a separate drying system. In addition, the bed energy rate of the oxidation smelting furnace used in the present invention is 27~50 t / (d·m 2 ), which is much higher than the bed efficiency of the electric furnace commonly used in yellow phosphorus production, which is 5~12 t / (d·m 2 ), the heat source can be anthracite, natural gas, kerosene, etc., the oxidation smelting furnace adopts oxidation smelting, the tail gas CO content is low, and the combustion heat utilization efficiency is high; at the same time, the reduction furnace only completes the reduction volatilization of liquid high-phosphorus slag and the insulation effect of maintaining the smelting temperature, effectively reducing the influence of the diffusion rate of solute atoms on the phosphorus reduction chemical reaction rate, thereby improving the phosphorus reduction volatilization reaction kinetics, shortening the reaction time, and improving the electric furnace processing capacity and efficiency; compared with the traditional electric furnace refining of yellow phosphorus, the smoke rate is lower, the molten reduction reaction efficiency is high, the reduction reaction time of the reduction furnace is shortened, the reduction furnace volatilization phosphorus refining bed energy rate is improved, the equipment investment is reduced, the power consumption is greatly reduced, and the cost is saved.
[0029] In summary, the present invention improves the tolerance of phosphate rock sources and broadens the utilization boundaries, achieves the purpose of continuous thermal smelting to produce yellow phosphorus, and completely solves the problem of phosphogypsum emissions from the source of phosphorus chemical industry, thereby realizing energy-saving, circular and clean production of phosphorus chemical industry.
[0030] 2. Under the same production capacity conditions, the present invention greatly reduces equipment investment and floor space, improves the on-site operating environment and reduces labor intensity; at the same time, since electrodes are no longer used as heat sources, problems such as difficult electrode operation, easy electrode breakage, and bridging and collapse of electric furnace charges can be effectively avoided. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0032] Figure 1 is a process flow chart of Example 1 of the present invention;
[0033] Figure 2 This is a schematic diagram of the state of the system in the process of smelting and producing yellow phosphorus in Example 1 of the present invention;
[0034] Figure 3 It is a schematic diagram of the state of the system smelting process for producing yellow phosphorus in Example 5 of the present invention. DETAILED DESCRIPTION
[0035] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0036] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0037] Example 1
[0038] A method for producing yellow phosphorus by smelting phosphate ore, such as Figure 1 and Figure 2 As shown, including:
[0039] (1) Obtaining liquid high-phosphorus slag
[0040] The phosphate ore and the slag-forming flux are mixed to obtain a mixed material with an acidity coefficient of 0.8. The phosphate ore used in this embodiment is a medium- and low-grade phosphate ore, wherein the composition of the phosphate ore is shown in Table 1 below;
[0041] Table 1 Phosphate ore composition (wt%)
[0042]
[0043] Specifically, quartz stone, a slag-making flux, is added to the above-mentioned phosphate ore, the mass ratio of the acidity coefficient SiO2 / CaO is controlled to be 0.8, and the mixture is crushed to obtain a particle size of ≤50mm, the moisture content of the mixture is 2.5%, and the mixture is added through the feeding port of the oxygen-enriched side-blowing furnace, the fuel is pulverized coal, and the pulverized coal is sprayed into the melt by blowing, the back pressure of the spray gun is 0.2~0.35 Mpa, the oxygen combustion excess coefficient is 1.2, the melt temperature is 1400℃, and the oxygen enrichment concentration is 75%. Among them, the excess coefficient of oxygen combustion in oxidative smelting refers to the ratio of the actual amount of air supplied during fuel combustion to the theoretical amount of air.
[0044] The smelting products of the oxygen-enriched side-blown furnace include liquid high-phosphorus slag, molten smoke and molten smoke, wherein the molten smoke and molten smoke are obtained by filtering and separating the furnace gas obtained by oxidation melting in the oxygen-enriched side-blown furnace.
[0045] After the pulverized coal is sprayed into the melt, the phosphorus grade P2O5 in the side-blown slag (liquid high-phosphorus slag) is 24.67%. The melting flue gas is mainly CO2 due to complete combustion, with a CO2 volume fraction of 62.79%, which also includes some phosphorus P2O5, and the P2O5 volume fraction is only 0.1%; the side-blowing strengthens the oxidation combustion, and the slag defluorination rate can reach 99%. Specifically, the volume fraction of SiF4 in the melting flue gas reaches 1.52%, and the melting dust contains 7.08% CaF4 by mass, and the liquid high-phosphorus slag contains only 0.06% F substance CaF4. At the same time, the melting flue gas also contains 0.01% H2S by volume and 0.26% SO2 by volume. The melting dust contains 13.50% P2O5, 7.08% CaF2, 0.2% I, and 1.66% Cl.
[0046] The input in the side blowing stage is: 0.21t coal per ton of ore, 279.61Nm oxygen per ton of ore 3 , compressed air consumption per ton of ore is 125.83Nm 3 , quartz consumption per ton of ore is 0.32t; the output is slag rate 80.51%, ton of phosphorus side blowing melting dust 180.46kg, dust rate 1.50%, ton of ore flue gas volume 491.39Nm 3 .
[0047] (2) Restoration
[0048] The high-phosphorus slag from the side-blown furnace is transferred into the electric furnace, and the melt temperature is maintained at 1400°C by electric heat. The reducing agent coke with a particle size of 15-35mm is added, and the amount of coke added is 1.2 times the theoretical amount. The products of the reduction and volatilization phosphorus refining stage in the electric furnace include dephosphorization slag, phosphorus-containing flue gas, ferrophosphorus and volatilized smoke.
[0049] Among them, the P2O5 content in the dephosphorization slag is only 0.46%, and the FeO content is 0.04%; the phosphorus-containing flue gas is mainly CO, with a CO volume fraction of 84.32%, a phosphorus P4 volume fraction of 8.23%, an H2S volume fraction of only 0.16%, a HF volume fraction of only 0.01%, and a SO2 volume fraction of only 0.16%; the iron content in ferrophosphorus is 77.25%, and the P content is 18%; the P2O5 content in the volatile smoke is 24.48%, and the Fe2O3 content is 1.57%.
[0050] In the reduction volatilization phosphorus refining stage of the electric furnace, the electricity consumption per ton of phosphorus is 3958.20kW·h, the coke consumption per ton of phosphorus is 1.17t, and the flue gas volume per ton of phosphorus is 2023.00Nm 3 , 0.14t of ferrophosphorus is produced per ton of phosphorus, and 4.88kg of volatile smoke is emitted per ton of phosphorus.
[0051] (3) Obtaining yellow phosphorus
[0052] The volume fraction of the main components of phosphorus-containing flue gas is P4: 8.23%, CO: 84.32%. After the phosphorus is collected by the water-leaching tower, yellow phosphorus and yellow phosphorus tail gas are obtained. The volume fraction of CO in the yellow phosphorus tail gas reaches 91.86%, HF 0.01%, and P4 0.02%; the calorific value is estimated to be about 12323.50KJ / Nm according to the flue gas composition. 3 After conversion, the yield of yellow phosphorus in this step is 93%.
[0053] Example 2
[0054] A method for producing yellow phosphorus by smelting phosphate ore, comprising:
[0055] (1) Obtaining liquid high-phosphorus slag
[0056] The phosphate rock and silica in Example 1 are mixed to obtain a mixture with a particle size of ≤50 mm and an acidity coefficient SiO2 / CaO of 0.65, and the moisture content of the mixture is 3.0%. The mixture is added through the feeding port of the oxygen-enriched side-blown furnace. Pulverized coal is used as fuel, and the pulverized coal is sprayed into the melt by blowing. The back pressure of the spray gun is 0.2~0.35 Mpa, the oxygen combustion excess coefficient is 1.2, the melt temperature is controlled at 1500°C, and the oxygen enrichment concentration is 75%.
[0057] After adding pulverized coal, the phosphorus grade P2O5 in the side-blown slag (liquid high-phosphorus slag) is 28%. The flue gas is mainly CO2 due to complete combustion, with a CO2 volume fraction of 65%. The side-blowing strengthens the oxidative combustion, and the slag defluorination rate reaches 95%, and the SiF4 volume fraction in the flue gas is 1.4%.
[0058] The input of the side blowing stage is: 0.23t coal consumption per ton of ore, 290 Nm oxygen consumption per ton of ore 3 , compressed air consumption per ton of ore is 140Nm 3 The consumption of quartz stone per ton of ore is 0.28 t; the output is slag rate of 75%, 160 kg of side-blown melting dust per ton of phosphorus, dust rate of 1.45%, and 512 Nm of flue gas per ton of ore. 3 .
[0059] (2) Restoration
[0060] The high phosphorus slag from the side-blowing furnace is transferred into the electric furnace, and the melt temperature is maintained at 1500℃ by electric heat. The reducing agent anthracite is added, and the amount of anthracite added is 1.3 times the theoretical amount, and the particle size of anthracite is 15~35mm. The electric furnace reduction volatilization phosphorus refining stage consumes 4050 kW·h of electricity per ton of phosphorus, 1.20t of anthracite per ton of phosphorus, and the flue gas volume of the electric furnace per ton of phosphorus is 2100Nm 3 , 0.15t of ferrophosphorus is produced per ton of phosphorus, and 4.50kg of volatile smoke is emitted per ton of phosphorus.
[0061] (3) Obtaining yellow phosphorus
[0062] The volume fraction of the main components of phosphorus-containing flue gas is P4: 8.5%, CO: 83%. After the phosphorus is collected by the water-leaching tower, the yellow phosphorus tail gas is obtained. The volume fraction of CO in the yellow phosphorus tail gas reaches 90%, and the volume fraction of HF is 0.015%. According to the flue gas composition, the calorific value is estimated to be about 12200KJ / Nm 3 , the yield of yellow phosphorus is 94%.
[0063] Example 3
[0064] A method for producing yellow phosphorus by smelting phosphate ore, comprising:
[0065] (1) Obtaining liquid high-phosphorus slag
[0066] The phosphate rock and silica in Example 1 are mixed to obtain a mixture with a particle size of ≤50 mm and an acidity coefficient SiO2 / CaO of 0.85. The moisture content of the mixture is 2.8%. The mixture is added through the feeding port of the oxygen-enriched side-blown furnace. Pulverized coal is used as fuel, and the pulverized coal is sprayed into the melt by blowing. The back pressure of the spray gun is 0.2~0.35 Mpa, the oxygen combustion excess coefficient is 1.2, the melt temperature is controlled at 1350°C, and the oxygen enrichment concentration is 75%.
[0067] After adding pulverized coal, the phosphorus grade P2O5 in the side-blown slag (liquid high-phosphorus slag) is 23.80%. The flue gas is mainly CO2 due to complete combustion, with a CO2 volume fraction of 65%. The side-blowing strengthens the oxidative combustion, and the slag defluorination rate reaches 96%, and the SiF4 volume fraction in the flue gas is 1.6%.
[0068] The input in the side blowing stage is: 0.22t coal per ton of ore, 280 Nm oxygen per ton of ore 3 , compressed air consumption per ton of ore is 130Nm 3 The consumption of quartz stone per ton of ore is 0.35 t; the output is slag rate of 82%, 190 kg of side-blown melting dust per ton of phosphorus, dust rate of 1.55%, and 510 Nm of flue gas per ton of ore. 3 .
[0069] (2) Restoration
[0070] The high phosphorus slag from the side-blowing furnace is transferred into the electric furnace, and the melt temperature is maintained at 1350°C by electric heat. The reducing agent anthracite is added, and the amount of anthracite added is 1.25 times the theoretical amount. The particle size of anthracite is 15-35mm. The electric furnace reduction volatilization phosphorus refining stage consumes 3850 kW·h of electricity per ton of phosphorus, consumes 1.15t of anthracite per ton of phosphorus, and the flue gas volume of the electric furnace per ton of phosphorus is 1980Nm 3 , 0.13t of ferrophosphorus is produced per ton of phosphorus, and 4.50kg of volatile smoke is emitted per ton of phosphorus.
[0071] (3) Obtaining yellow phosphorus
[0072] The volume fraction of the main components of phosphorus-containing flue gas is P4: 7.5%, CO: 86%. After the phosphorus is collected by the water-leaching tower, the yellow phosphorus tail gas is obtained. The volume fraction of CO in the yellow phosphorus tail gas reaches 92%, and the volume fraction of HF is 0.01%. According to the flue gas composition, the calorific value is estimated to be about 12500KJ / Nm 3 , the yield of yellow phosphorus is 95%.
[0073] Example 4
[0074] A method for producing yellow phosphorus by smelting phosphate ore, comprising:
[0075] (1) Obtaining liquid high-phosphorus slag
[0076] The phosphate rock and silica in Example 1 are mixed to obtain a mixture with a particle size of ≤50 mm and an acidity coefficient SiO2 / CaO of 0.80, the moisture content of the mixture is adjusted to 10%, and the mixture is added through the feeding port of the oxygen-enriched side-blown furnace. Pulverized coal is used as fuel, and the pulverized coal is sprayed into the melt by blowing. The back pressure of the spray gun is 0.2~0.35 Mpa, the oxygen combustion excess coefficient is 1.2, the melt temperature is controlled to be 1400°C, and the oxygen enrichment concentration is 75%.
[0077] After adding pulverized coal, the phosphorus grade P2O5 in the side-blown slag (liquid high-phosphorus slag) is 25.50%. The flue gas is mainly CO2 due to complete combustion, with a CO2 volume fraction of 68%. The side-blowing strengthens the oxidative combustion, and the slag defluorination rate reaches 96%, and the SiF4 volume fraction in the flue gas is 1.78%.
[0078] The input of the side blowing stage is: 0.20t coal per ton of ore, 270 Nm oxygen per ton of ore 3 , compressed air consumption per ton of ore is 120Nm 3 The consumption of quartz stone per ton of ore is 0.31 t; the output is slag rate of 82%, 176 kg of side-blown melting dust per ton of phosphorus, dust rate of 1.52%, and 485 Nm of flue gas per ton of ore. 3 .
[0079] (2) Restoration
[0080] The high phosphorus slag from the side-blowing furnace is transferred into the electric furnace, and the melt temperature is maintained at 1400°C by electric heat. The reducing agent coke is added, and the amount of coke added is 1.25 times the theoretical amount, and the coke particle size is 15~35mm. The electric furnace reduction volatilization phosphorus refining stage consumes 3875 kW·h of electricity per ton of phosphorus, consumes 1.19t of anthracite per ton of phosphorus, and the flue gas volume of the electric furnace per ton of phosphorus is 2085Nm 3 , 0.138t of ferrophosphorus is produced per ton of phosphorus, and 4.30kg of volatile smoke is emitted per ton of phosphorus.
[0081] (3) Obtaining yellow phosphorus
[0082] The volume fraction of the main components of phosphorus-containing flue gas is P4: 8.6%, CO: 86%. After the phosphorus is collected by the water-leaching tower, the yellow phosphorus tail gas is obtained. The volume fraction of CO in the yellow phosphorus tail gas reaches 93%, and the volume fraction of HF is 0.01%. According to the flue gas composition, the calorific value is estimated to be about 12280KJ / Nm 3 , the yield of yellow phosphorus is 94%.
[0083] Example 5
[0084] A method for producing yellow phosphorus by smelting phosphate ore, comprising:
[0085] (1) Obtaining liquid high-phosphorus slag
[0086] The phosphate rock and silica in Example 1 are mixed to obtain a mixture with a particle size of ≤50 mm and an acidity coefficient SiO2 / CaO of 0.80, the moisture content of the mixture is adjusted to 4.5%, and the mixture is added through the feeding port of the oxygen-enriched side-blown furnace. Pulverized coal is used as fuel, and the pulverized coal is sprayed into the melt by blowing. The back pressure of the spray gun is 0.2~0.35 Mpa, the oxygen combustion excess coefficient is 1.2, the melt temperature is controlled at 1400°C, and the oxygen enrichment concentration is 75%.
[0087] After adding pulverized coal, the phosphorus grade P2O5 in the side-blown slag (liquid high-phosphorus slag) is 25.60%. The flue gas is mainly CO2 due to complete combustion, with a CO2 volume fraction of 67%. The side-blowing strengthens the oxidative combustion, and the slag defluorination rate reaches 94%, and the SiF4 volume fraction in the flue gas is 1.35%.
[0088] The input in the side blowing stage is: 0.20t coal per ton of ore, 272 Nm oxygen per ton of ore 3 , compressed air consumption per ton of ore: 118Nm 3 The consumption of quartz stone per ton of ore is 0.31 t; the output is slag rate of 78%, 172 kg of side-blown melting dust per ton of phosphorus, dust rate of 1.46%, and 487 Nm of flue gas per ton of ore. 3 .
[0089] (2) Restoration
[0090] The high-phosphorus slag from the side-blown furnace is transferred to the side-blown reduction furnace. Figure 3 As shown in the figure, the melt temperature is maintained at 1400℃ by side-blowing lance combustion, and coke is added as a reducing agent. The amount of coke added is 1.6 times the theoretical amount, and the coke particle size is 15-35mm. The side-blowing reduction and volatilization phosphorus refining stage consumes 1.7t of anthracite per ton of phosphorus, and the flue gas volume of the electric furnace per ton of phosphorus is 3500Nm 3 , 0.12t of ferrophosphorus is produced per ton of phosphorus, and 7.6kg of volatile smoke is emitted per ton of phosphorus.
[0091] (3) Obtaining yellow phosphorus
[0092] The volume fraction of the main components of phosphorus-containing flue gas is P4: 6.78%, CO: 72%. After the phosphorus is collected by the water-leaching tower, the yellow phosphorus tail gas is obtained. The volume fraction of CO in the yellow phosphorus tail gas reaches 80%, and the volume fraction of HF is 0.01%. According to the flue gas composition, the calorific value is estimated to be about 10500KJ / Nm 3 , the yield of yellow phosphorus is 92%.
[0093] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A method for producing yellow phosphorus by smelting phosphate ore, comprising: Liquid high-phosphorus slag is obtained, a reducing agent is added to the liquid high-phosphorus slag for reduction to obtain phosphorus-containing flue gas, and the phosphorus-containing flue gas is condensed to obtain yellow phosphorus; the method is characterized in that: The liquid high-phosphorus slag is obtained in an oxidation smelting furnace, and the reducing agent is added and the yellow phosphorus is obtained in a reduction furnace; the reduction furnace is an electric furnace; The process of obtaining liquid high-phosphorus slag is as follows: phosphate ore and slag-making flux are mixed to obtain a mixture with an acidity coefficient of 0.65 to 0.85, and the mixture is oxidized and smelted in an oxidation smelting furnace to obtain molten liquid high-phosphorus slag; The temperature of the oxidation smelting and reduction is 1350°C-1500°C; In the liquid high-phosphorus slag, the amount of reducing agent added is 1 to 2 times the theoretical amount; The reducing agent includes at least one of anthracite, blue carbon, graphite powder and coke.
2. The method according to claim 1, characterized in that The moisture content of the mixed material is below 12%.
3. The method according to claim 2, characterized in that The moisture content of the mixed material is 2% to 5%.
4. The method according to claim 1, characterized in that: The particle size of the mixed material is ≤50mm.
5. The method according to claim 1, characterized in that The particle size of the reducing agent is 15-35 mm.
Citation Information
Cited By
Method and system for recovering phosphorus and iron from ferrophosphorus solid waste
CN122609779A