Semiconductor device and method for manufacturing the same

By utilizing the combined structure of the substrate and the channel layer to form high-concentration two-dimensional hole gas in GaN-based complementary logic circuits, the problem of low concentration of two-dimensional hole gas in the existing technology is solved, and high-performance p channel devices and excellent CMOS device performance.

CN118630013BActive Publication Date: 2024-10-18XIAN JIAOTONG LIVERPOOL UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411095964.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-10-18
Estimated Expiration
2044-08-12

AI Technical Summary

Technical Problem

The concentration of two-dimensional hole gas in existing GaN-based complementary logic circuits is low, making it impossible to realize high-performance p-channel devices.

Method used

By arranging a P-channel metal oxide semiconductor structure and an N-channel metal oxide semiconductor structure on the substrate, the Al element and N element in the substrate are used to form holes with the Ga element and N element in the first channel layer. The heterojunction structure uses a strong polarization effect to increase the concentration of two-dimensional hole gas, and achieves spatial isolation between the two-dimensional electron gas and the two-dimensional hole gas by setting up a stacked structure of a barrier layer and a channel layer.

Benefits of technology

It realizes high-performance p-channel devices and improves the performance, operating frequency and area utilization of CMOS devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118630013B_ABST
    Figure CN118630013B_ABST
Patent Text Reader

Abstract

The present invention discloses a semiconductor device and a preparation method thereof, wherein the semiconductor device comprises a substrate and a P-channel metal oxide semiconductor structure and an N-channel metal oxide semiconductor structure located on the same side of the substrate; the P-channel metal oxide semiconductor structure comprises a first epitaxial structure, and the N-channel metal oxide semiconductor structure comprises a second epitaxial structure; the first epitaxial structure comprises a first channel layer, and the second epitaxial structure comprises a stacked second channel layer and a barrier layer; the first channel layer comprises Ga elements and N elements; the substrate comprises Al elements and N elements; the substrate and the first channel layer form a hole heterojunction structure, and the second channel layer and the barrier layer form an electron heterojunction structure. By adopting the above technical means, the hole heterojunction structure formed by the first channel layer and the substrate has a high concentration, which can realize a high-performance p-channel device and improve the performance of complementary metal oxide semiconductors.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of microelectronic technology, and in particular to a semiconductor device and a preparation method thereof. Background Art

[0002] GaN-based complementary metal oxide semiconductor (CMOS) is the basic building block of current digital circuits due to its outstanding static power consumption advantage.

[0003] The current GaN-based complementary logic circuits are mainly realized through silicon substrates and GaN or AlGaN buffer layers. Two-dimensional hole gas is generated between GaN and AlGaN, but the concentration of the two-dimensional hole gas is low and high-performance p-channel devices cannot be achieved. Summary of the invention

[0004] The present invention provides a semiconductor device and a preparation method thereof, so as to increase the concentration of hole heterojunction structure, realize high-performance p-channel device, and improve the performance of complementary metal oxide semiconductor.

[0005] In a first aspect, an embodiment of the present invention provides a semiconductor device, comprising: a substrate, and a P-channel metal oxide semiconductor structure and an N-channel metal oxide semiconductor structure located on the same side of the substrate;

[0006] The P-channel metal oxide semiconductor structure includes a first epitaxial structure, and the N-channel metal oxide semiconductor structure includes a second epitaxial structure; the first epitaxial structure includes a first channel layer, and the second epitaxial structure includes a stacked second channel layer and a barrier layer; the first channel layer includes Ga elements and N elements;

[0007] The substrate includes Al and N elements; the substrate and the first channel layer form a hole heterojunction structure, and the second channel layer and the barrier layer form an electron heterojunction structure

[0008] Optionally, the first channel layer and the second channel layer are provided in the same layer;

[0009] The hole heterojunction structure is located on a side of the electron heterojunction structure close to the substrate.

[0010] Optionally, the substrate includes an AlN single crystal layer or an AlN template.

[0011] Optionally, the thickness of the first channel layer is less than or equal to the thickness of the second channel layer.

[0012] Optionally, the thickness D1 of the first channel layer satisfies: 10 nm ≤ D1 ≤ 300 nm; the thickness D2 of the second channel layer satisfies: 10 nm ≤ D2 ≤ 300 nm;

[0013] The thickness D3 of the barrier layer satisfies: 2nm≤D3≤50nm.

[0014] Optionally, the first channel layer and the second channel layer both include a GaN layer; or, the first channel layer and the second channel layer both include an AlGaN layer;

[0015] The barrier layer includes an AlGaN layer or an AlN layer.

[0016] Optionally, the semiconductor device further comprises a first electrode structure located on a side of the first epitaxial structure away from the substrate and a second electrode structure located on a side of the second epitaxial structure away from the substrate;

[0017] The first electrode structure includes a first source, a first gate and a first drain; the first source and the first drain form an ohmic contact with the first epitaxial structure respectively; the first gate forms a Schottky contact with the first epitaxial structure;

[0018] The second electrode structure includes a second source, a second gate and a second drain; the second source and the second drain form an ohmic contact with the second epitaxial structure respectively; and the second gate forms a Schottky contact with the second epitaxial structure.

[0019] Optionally, the P-channel metal oxide semiconductor further includes a first gate dielectric layer, and the first gate dielectric layer is located between the first gate and the first channel layer;

[0020] The N-channel metal oxide semiconductor further includes a second gate dielectric layer, and the second gate dielectric layer is located between the second gate and the barrier layer.

[0021] In a second aspect, an embodiment of the present invention further provides a method for preparing a semiconductor device, comprising:

[0022] Providing a substrate, wherein the substrate includes Al element and N element;

[0023] A P-channel metal oxide semiconductor structure and an N-channel metal oxide semiconductor structure are prepared on the same side of the substrate; the P-channel metal oxide semiconductor structure includes a first epitaxial structure, and the N-channel metal oxide semiconductor structure includes a second epitaxial structure; the first epitaxial structure includes a first channel layer, and the second epitaxial structure includes a stacked second channel layer and a barrier layer; the first channel layer includes Ga elements and N elements;

[0024] The substrate and the first channel layer form a hole heterojunction structure, and the second channel layer and the barrier layer form an electron heterojunction structure.

[0025] Optionally, a P-channel metal oxide semiconductor structure and an N-channel metal oxide semiconductor structure are prepared on the same side of the substrate, comprising:

[0026] preparing a channel layer on one side of the substrate;

[0027] Patterning the channel layer to form a first channel layer and a second channel layer; the thickness of the first channel layer is less than or equal to the thickness of the second channel layer;

[0028] A first electrode structure is prepared on a side of the first channel layer away from the substrate; a barrier layer is prepared on a side of the second channel layer away from the substrate, and a second electrode structure is prepared on a side of the barrier layer away from the substrate; the first electrode structure includes a first source, a first gate and a first drain; the first source and the first drain form ohmic contacts with the first channel layer respectively; the first gate forms a Schottky contact with the first channel layer; the second electrode structure includes a second source, a second gate and a second drain; the second source and the second drain form ohmic contacts with the barrier layer respectively; the second gate forms a Schottky contact with the barrier layer.

[0029] The technical solution of the embodiment of the present invention is to set a P-channel metal oxide semiconductor structure and an N-channel metal oxide semiconductor structure on the same substrate, so that a CMOS device can be formed. By setting the substrate to include Al elements and N elements, and the first channel layer to include Ga elements and N elements, a hole heterojunction structure can be formed between the substrate and the first channel layer, and a two-dimensional hole gas is set in the hole heterojunction structure. Further, due to the strong polarization effect between the substrate and the first channel layer, the concentration of the two-dimensional hole gas can be increased, thereby realizing a high-performance p-channel device, thereby obtaining a CMOS device with better performance, higher operating frequency, and higher area utilization. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 A schematic cross-sectional structure diagram of a first semiconductor device provided by an embodiment of the present invention;

[0031] Figure 2 A schematic cross-sectional structure diagram of a second semiconductor device provided by an embodiment of the present invention;

[0032] Figure 3 A schematic cross-sectional structure diagram of a third semiconductor device provided by an embodiment of the present invention;

[0033] Figure 4A schematic diagram of a process flow of a first method for preparing a semiconductor device provided by an embodiment of the present invention;

[0034] Figure 5 A schematic diagram of the process flow of a second method for preparing a semiconductor device provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0035] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0036] Figure 1 A schematic cross-sectional structure diagram of a first semiconductor device provided by an embodiment of the present invention is shown in FIG. Figure 1 As shown, the semiconductor device includes a substrate 10 and a P-channel metal oxide semiconductor structure 20 and an N-channel metal oxide semiconductor structure 30 located on the same side of the substrate 10; the P-channel metal oxide semiconductor structure 20 includes a first epitaxial structure 201, and the N-channel metal oxide semiconductor structure 30 includes a second epitaxial structure 301; the first epitaxial structure 201 includes a first channel layer 2011, and the second epitaxial structure 301 includes a stacked second channel layer 3011 and a barrier layer 3012; the first channel layer 2011 includes Ga elements and N elements; the substrate 10 includes Al elements and N elements; the substrate 10 and the first channel layer 2011 form a hole heterojunction structure, and the second channel layer 3011 and the barrier layer 3012 form an electron heterojunction structure.

[0037] Specifically, a P-channel metal oxide semiconductor structure 20 and an N-channel metal oxide semiconductor structure 30 are arranged on the same substrate 10, so that a CMOS device can be formed. By arranging the substrate 10 to include Al elements and N elements, and the first channel layer 2011 to include Ga elements and N elements, a hole heterojunction structure can be formed between the substrate 10 and the first channel layer 2011, and a two-dimensional hole gas is arranged in the hole heterojunction structure. Further, due to the strong polarization effect between the substrate 10 and the first channel layer 2011, the concentration of the two-dimensional hole gas can be increased, thereby realizing a high-performance p-channel device, thereby obtaining a CMOS device with better performance, higher operating frequency, and higher area utilization.

[0038] Exemplarily, the substrate 10 may be AlN, and the first channel layer 2011 may be GaN, so that the strong polarization effect between AlN and GaN can be understood as the piezoelectric effect caused by the different lattice constants of AlN and GaN on the one hand, and the spontaneous polarization caused by the asymmetry of the positive and negative charge centers of the Al element and the N element on the other hand. As a comparative example, in the prior art, a two-dimensional hole gas is formed between the barrier layer and the channel layer. In the embodiment of the present invention, a high-concentration two-dimensional hole gas is formed by a substrate including Al elements and N elements and a first channel layer including Ga elements and N elements, thereby realizing a high-performance p-channel device.

[0039] Specifically, the second epitaxial structure 301 includes a stacked second channel layer 3011 and a barrier layer 3012, the second channel layer 3011 and the barrier layer 3012 form an electronic heterojunction structure, and a two-dimensional electron gas is arranged in the electronic heterojunction structure. The two-dimensional hole gas and the two-dimensional electron gas can be used as a conductive medium in a semiconductor device to realize the function of a CMOS device.

[0040] The semiconductor device provided by the embodiment of the present invention is provided with a P-channel metal oxide semiconductor structure and an N-channel metal oxide semiconductor structure on the same substrate, so that a CMOS device can be formed. By providing the substrate to include Al elements and N elements, and the first channel layer to include Ga elements and N elements, a hole heterojunction structure can be formed between the substrate and the first channel layer, and a two-dimensional hole gas is provided in the hole heterojunction structure. Furthermore, due to the strong polarization effect between the substrate and the first channel layer, the concentration of the two-dimensional hole gas can be increased, thereby realizing a high-performance p-channel device, thereby obtaining a CMOS device with better performance, higher operating frequency, and higher area utilization.

[0041] Optional, continue to refer to Figure 1 The first channel layer 2011 and the second channel layer 3011 are arranged in the same layer; the hole heterojunction structure is located on the side of the electron heterojunction structure close to the substrate 10.

[0042] Specifically, in the process of preparing the semiconductor device, the first channel layer 2011 and the second channel layer 3011 are formed by patterning the entire channel layer. In the P-channel metal oxide semiconductor structure 20, the first channel layer 2011 and the substrate 10 form a hole heterojunction structure due to the strong polarization effect, and the hole heterojunction structure is located at the interface between the first channel layer 2011 and the substrate 10. In the N-channel metal oxide semiconductor structure 30, an electron heterojunction structure is formed between the second channel layer 3011 and the barrier layer 3012, and the electron heterojunction structure is located at the interface between the second channel layer 3011 and the barrier layer 3012. Therefore, compared with the electron heterojunction structure, the hole heterojunction structure is closer to the substrate 10, so that the hole heterojunction structure can be at the bottom and the electron heterojunction structure can be at the top, and the coupling interference problem between the two-dimensional electron gas and the two-dimensional hole gas can be solved through spatial isolation.

[0043] Optional, continue to refer to Figure 1 The substrate 10 includes an AlN single crystal layer or an AlN template.

[0044] Specifically, as a feasible implementation method, the substrate 10 includes an AlN single crystal layer, that is, the substrate 10 is composed of an AlN single crystal layer and does not contain film layers of other materials. This can ensure a strong polarization effect between AlN and GaN on the one hand, and on the other hand, since AlN is a wide bandgap semiconductor material, it has excellent electrical, thermal and mechanical properties, which is beneficial to improving the performance of semiconductor devices.

[0045] As another feasible implementation, the substrate 10 includes an AlN template, that is, the substrate 10 is composed of an AlN layer arranged on a sapphire substrate. This can ensure a strong polarization effect between AlN and GaN, thereby increasing the two-dimensional hole gas concentration, and can achieve diversified settings for the substrate 10 on the other hand.

[0046] Optional, continue to refer to Figure 1 , the thickness of the first channel layer 2011 is less than or equal to the thickness of the second channel layer 3011 .

[0047] Specifically, in the preparation process of the semiconductor device, the first channel layer 2011 and the second channel layer 3011 can be formed by patterning the entire channel layer, and only the channel layer corresponding to the P-channel metal oxide semiconductor structure region can be etched, and there is no need to etch the channel layer corresponding to the N-channel metal oxide semiconductor structure region. In this way, the thickness of the first channel layer 2011 is less than the thickness of the second channel layer 3011, which is beneficial to ensure that the hole heterojunction structure is located on the side of the electron heterojunction structure close to the substrate 10, and then the two-dimensional electron gas and the two-dimensional hole gas can be spatially isolated to prevent coupling interference between the two.

[0048] Exemplarily, the channel layer region corresponding to the P-channel metal oxide semiconductor structure and the channel layer region corresponding to the N-channel metal oxide semiconductor structure can be isolated only by the isolation structure 40 to form the first channel layer 2011 and the second channel layer 3011, that is, the thickness of the first channel layer 3011 is not changed, so that the thickness of the first channel layer 2011 is equal to the thickness of the second channel layer 3011, which is beneficial to ensure that the hole heterojunction structure is located on the side of the electron heterojunction structure close to the substrate 10, and then the two-dimensional electron gas and the two-dimensional hole gas can be isolated by space to prevent coupling interference between the two.

[0049] Optional, continue to refer to Figure 1 The thickness D1 of the first channel layer 2011 satisfies: 10 nm ≤ D1 ≤ 300 nm; the thickness D2 of the second channel layer 3011 satisfies: 10 nm ≤ D2 ≤ 300 nm; and the thickness D3 of the barrier layer 3012 satisfies: 2 nm ≤ D3 ≤ 50 nm.

[0050] Specifically, in the prior art, the thickness of the barrier layer in the P-channel metal oxide semiconductor structure and the N-channel metal oxide semiconductor structure is adjusted respectively to spatially isolate the two-dimensional electron gas and the two-dimensional hole gas. However, the thickness of the barrier layer is generally between 15nm and 20nm. If it exceeds this range, it will affect the heterojunction structure. Therefore, the degree of freedom of adjusting the thickness of the barrier layer in the prior art is small, and the isolation effect of the two-dimensional electron gas and the two-dimensional hole gas is poor. However, in the embodiment of the present invention, the hole heterojunction structure is located on the side of the electronic heterojunction structure close to the substrate 10, that is, the two-dimensional hole gas is at the bottom, the two-dimensional electron gas is at the top, the two-dimensional hole gas is located between the substrate 10 and the first channel layer 2011, and the two-dimensional electron gas is located between the second channel layer 3011 and the barrier layer 3012. In this way, there is no need to adjust the thickness of the barrier layer 3012. For example, only by adjusting the thickness of the second channel layer 3011, the spatial isolation of the two-dimensional electron gas and the two-dimensional hole gas can be achieved to prevent coupling interference between the two. In addition, the thickness D1 of the first channel layer 2011 satisfies: 10nm≤D1≤300nm; the thickness D2 of the second channel layer 3011 satisfies: 10nm≤D2≤300nm, which means that the thickness of the channel layer can be adjusted with greater freedom, further ensuring better spatial isolation between the two-dimensional electron gas and the two-dimensional hole gas.

[0051] Optional, continue to refer to Figure 1 , the first channel layer 2011 and the second channel layer 3011 both include GaN layers; or, the first channel layer 2011 and the second channel layer 3011 both include AlGaN layers; and the barrier layer 3012 includes an AlGaN layer or an AlN layer.

[0052] Specifically, the first channel layer 2011 and the second channel layer 3011 both include GaN layers or the first channel layer 2011 and the second channel layer 3011 both include AlGaN layers, so that a diversified design of the channel layer can be achieved. When the first channel layer 2011 and the second channel layer 3011 are both AlGaN layers, the Al component can be 10%-30%, which is conducive to ensuring the generation of a heterojunction structure.

[0053] Specifically, the barrier layer 3012 includes an AlGaN layer or an AlN layer, so that a variety of designs can be realized for the barrier layer 3012. When the barrier layer 3012 is an AlGaN layer, the Al component can be 25%-60%, which is conducive to ensuring that an electronic heterojunction structure is formed between the barrier layer 3012 and the second channel layer 3011.

[0054] Optional, continue to refer to Figure 1 The semiconductor device also includes a first electrode structure 50 located on the side of the first epitaxial structure 201 away from the substrate 10 and a second electrode structure 60 located on the side of the second epitaxial structure 301 away from the substrate 10; the first electrode structure 50 includes a first source 501, a first gate 502 and a first drain 503; the first source 501 and the first drain 503 respectively form ohmic contacts with the first epitaxial structure 201; the first gate 502 forms a Schottky contact with the first epitaxial structure 201; the second electrode structure 60 includes a second source 601, a second gate 602 and a second drain 603; the second source 601 and the second drain 603 respectively form ohmic contacts with the second epitaxial structure 301; the second gate 602 forms a Schottky contact with the second epitaxial structure 301.

[0055] Specifically, the first electrode structure 50 includes a first source 501, a first gate 502 and a first drain 503. The second electrode structure 60 includes a second source 601, a second gate 602 and a second drain 603. Specifically, the source can be used as an input terminal of the semiconductor device, and the drain can be used as an output terminal of the semiconductor device.

[0056] For example, a heavily doped p-type GaN layer may be provided between the first source 501 and the first channel layer 2011, and a heavily doped p-type GaN layer may be provided between the first drain 503 and the first channel layer 2011. A heavily doped n-type GaN layer may be provided between the second source 601 and the second channel layer 3011, and a heavily doped n-type GaN layer may be provided between the second drain 603 and the second channel layer 3011, thereby reducing the ohmic contact resistance.

[0057] Figure 2 A schematic cross-sectional structure diagram of a second semiconductor device provided by an embodiment of the present invention is shown in FIG. Figure 2As shown, it should be noted that the N-channel metal oxide semiconductor structure 30 may also include a cap layer 3013, which is located on the side of the barrier layer 3012 away from the substrate 10. By setting the cap layer 3013, the surface state of the semiconductor device can be reduced, the surface leakage of the subsequent semiconductor device can be reduced, and the current collapse can be suppressed, thereby improving the performance and reliability of the epitaxial structure and the semiconductor device. Further, the cap layer 3013 can be a heavily doped GaN layer. Exemplarily, the cap layer 3013 can be doped with magnesium ions, and the doping concentration of the magnesium ions can be 1×10 20 cm -3 , to achieve heavy doping of the doping medium.

[0058] Optional, Figure 3 A schematic cross-sectional structure diagram of a third semiconductor device provided by an embodiment of the present invention is shown in FIG. Figure 3 As shown, the P-channel metal oxide semiconductor 20 further includes a first gate dielectric layer 70 located between the first gate 502 and the first channel layer 2011 ; the N-channel metal oxide semiconductor 30 further includes a second gate dielectric layer 80 located between the second gate 602 and the barrier layer 3012 .

[0059] Specifically, an atomic layer deposition process or a plasma enhanced atomic layer deposition process is used to prepare a gate dielectric layer between the gate and the epitaxial structure, and the first gate dielectric layer 70 is located between the first gate 502 and the first channel layer 2011. The second gate dielectric layer 80 can be located between the second gate 602 and the barrier layer 3012, or when the second epitaxial structure 301 includes a cap layer 3013, the second gate dielectric layer 80 is located between the second gate 602 and the cap layer 3013, so that a "metal-insulator-semiconductor" structure can be formed, and a better leakage suppression effect of the semiconductor device can be obtained.

[0060] For example, the gate dielectric layer may be made of Al 2 O 3 wait.

[0061] In summary, the semiconductor device provided by the embodiment of the present invention, by setting the substrate to include Al elements and N elements, and the first channel layer to include Ga elements and N elements, a hole heterojunction structure can be formed between the substrate and the first channel layer, and a two-dimensional hole gas is provided in the hole heterojunction structure. Further, due to the strong polarization effect between the substrate and the first channel layer, the concentration of the two-dimensional hole gas can be increased, thereby realizing a high-performance p-channel device, thereby obtaining a CMOS device with better performance, higher operating frequency, and higher area utilization. In addition, by setting the hole heterojunction structure to be located on the side of the electron heterojunction structure close to the substrate, that is, the two-dimensional hole gas is at the bottom and the two-dimensional electron gas is at the top, the spatial isolation between the two-dimensional electron gas and the two-dimensional hole gas can be ensured by adjusting the thickness of the channel layer, thereby preventing coupling interference between the two. Since the thickness of the channel layer can be 10nm-300nm, that is, the channel layer thickness can be adjusted with a large degree of freedom, so the spatial isolation effect between the two-dimensional electron gas and the two-dimensional hole gas is good.

[0062] Based on the same inventive concept, an embodiment of the present invention further provides a method for preparing a semiconductor device. Figure 4 A process flow diagram of a method for preparing a semiconductor device provided by an embodiment of the present invention is shown in FIG. Figure 4 As shown, the method for preparing the semiconductor device includes:

[0063] S101. Provide a substrate, wherein the substrate includes Al elements and N elements.

[0064] For example, the substrate 10 may be AlN.

[0065] S102. Prepare a P-channel metal oxide semiconductor structure and an N-channel metal oxide semiconductor structure on the same side of the substrate; the P-channel metal oxide semiconductor structure includes a first epitaxial structure, and the N-channel metal oxide semiconductor structure includes a second epitaxial structure; the first epitaxial structure includes a first channel layer, and the second epitaxial structure includes a stacked second channel layer and a barrier layer; the first channel layer includes Ga elements and N elements; the substrate and the first channel layer form a hole heterojunction structure, and the second channel layer and the barrier layer form an electron heterojunction structure.

[0066] Specifically, a P-channel metal oxide semiconductor structure 20 and an N-channel metal oxide semiconductor structure 30 are arranged on the same substrate 10, so that a CMOS device can be formed. By arranging the substrate 10 to include Al elements and N elements, and the first channel layer 2011 to include Ga elements and N elements, a hole heterojunction structure can be formed between the substrate 10 and the first channel layer 2011, and a two-dimensional hole gas is arranged in the hole heterojunction structure. Further, due to the strong polarization effect between the substrate 10 and the first channel layer 2011, the concentration of the two-dimensional hole gas can be increased, thereby realizing a high-performance p-channel device, thereby obtaining a CMOS device with better performance, higher operating frequency, and higher area utilization.

[0067] Specifically, a hole heterojunction structure may be formed between the substrate 10 and the first channel layer 2011, and a two-dimensional hole gas is provided in the hole heterojunction structure. The second channel layer 3011 and the barrier layer 3012 form an electron heterojunction structure, and a two-dimensional electron gas is provided in the electron heterojunction structure. The two-dimensional hole gas and the two-dimensional electron gas can be used as conductive media in semiconductor devices to realize CMOS device functions.

[0068] It is understandable that after preparing the first epitaxial structure 201 , the first electrode structure 50 and the second electrode structure 60 may also be prepared. The P-channel metal oxide semiconductor structure 20 and the N-channel metal oxide semiconductor structure 30 are isolated from each other by an isolation structure 40 .

[0069] The method for preparing a semiconductor device provided by an embodiment of the present invention comprises a substrate including Al elements and N elements, and a first channel layer including Ga elements and N elements, so that a hole heterojunction structure can be formed between the substrate and the first channel layer, and a two-dimensional hole gas is provided in the hole heterojunction structure. Furthermore, due to the strong polarization effect between the substrate and the first channel layer, the concentration of the two-dimensional hole gas can be increased, thereby realizing a high-performance p-channel device, thereby obtaining a CMOS device with better performance, higher operating frequency, and higher area utilization.

[0070] Optional, Figure 5 A schematic diagram of a process flow of a second method for preparing a semiconductor device provided by an embodiment of the present invention, Figure 5 Based on the above embodiments, the operations of preparing a P-channel metal oxide semiconductor structure and an N-channel metal oxide semiconductor structure on the same side of a substrate are described in detail. Figure 5 As shown, the method for preparing the semiconductor device includes:

[0071] S201. Provide a substrate, wherein the substrate includes Al elements and N elements.

[0072] S202, preparing a channel layer on one side of the substrate.

[0073] Specifically, a whole channel layer 100 is prepared on one side of the substrate 10 .

[0074] S203 , patterning the channel layer to form a first channel layer and a second channel layer; the thickness of the first channel layer is less than or equal to the thickness of the second channel layer.

[0075] Specifically, the patterned channel layer 100 forms a first channel layer 2011 and a second channel layer 3011 , and the P-channel metal oxide semiconductor structure 20 and the N-channel metal oxide semiconductor structure 30 are isolated from each other by an isolation structure 40 .

[0076] Furthermore, the thickness of the first channel layer 2011 is less than or equal to the thickness of the second channel layer 3011, which is conducive to ensuring that the hole heterojunction structure is located on the side of the electron heterojunction structure close to the substrate 10, thereby isolating the two-dimensional electron gas and the two-dimensional hole gas by space to prevent coupling interference between the two.

[0077] Specifically, the thickness of the first channel layer 2011 can be 10nm-300nm; the thickness of the second channel layer 3011 can be 10nm-300nm, which means that the thickness of the channel layer can be adjusted with greater freedom, which can further ensure better spatial isolation between the two-dimensional electron gas and the two-dimensional hole gas.

[0078] S204, preparing a first electrode structure on a side of the first channel layer away from the substrate; preparing a barrier layer on a side of the second channel layer away from the substrate, and preparing a second electrode structure on a side of the barrier layer away from the substrate; the first electrode structure includes a first source, a first gate and a first drain; the first source and the first drain form ohmic contacts with the first channel layer respectively; the first gate forms a Schottky contact with the first channel layer; the second electrode structure includes a second source, a second gate and a second drain; the second source and the second drain form ohmic contacts with the barrier layer respectively; the second gate forms a Schottky contact with the barrier layer; the substrate and the first channel layer form a hole heterojunction structure, and the second channel layer and the barrier layer form an electron heterojunction structure.

[0079] Specifically, the first electrode structure 50 includes a first source 501, a first gate 502 and a first drain 503. The second electrode structure 60 includes a second source 601, a second gate 602 and a second drain 603. Specifically, the source can be used as an input terminal of the semiconductor device, and the drain can be used as an output terminal of the semiconductor device.

[0080] It should be noted that the N-channel metal oxide semiconductor structure may also include a cap layer, which is located on the side of the barrier layer 3012 away from the substrate 10. By setting the cap layer, the surface state of the semiconductor device can be reduced, the surface leakage of the subsequent semiconductor device can be reduced, and the current collapse can be suppressed, thereby improving the performance and reliability of the epitaxial structure and the semiconductor device.

[0081] The method for preparing a semiconductor device provided by an embodiment of the present invention can form a first channel layer and a second channel layer by patterning the entire channel layer, and the thickness of the first channel layer is less than or equal to the thickness of the second channel layer. In this way, there is no need to adjust the thickness of the barrier layer. For example, only by adjusting the thickness of the second channel layer, spatial isolation of the two-dimensional electron gas and the two-dimensional hole gas can be achieved to prevent coupling interference between the two.

[0082] Note that the above are only preferred embodiments of the present invention and the technical principles used. Those skilled in the art will understand that the present invention is not limited to the specific embodiments described herein, and that various obvious changes, readjustments and substitutions can be made by those skilled in the art without departing from the scope of protection of the present invention. Therefore, although the present invention has been described in more detail through the above embodiments, the present invention is not limited to the above embodiments, and may include more other equivalent embodiments without departing from the concept of the present invention, and the scope of the present invention is determined by the scope of the appended claims.

Claims

1. A semiconductor device, It is characterized in that include: A substrate and a P-channel metal oxide semiconductor structure and an N-channel metal oxide semiconductor structure located on the same side of the substrate; The P-channel metal oxide semiconductor structure includes a first epitaxial structure, and the N-channel metal oxide semiconductor structure includes a second epitaxial structure; the first epitaxial structure includes a first channel layer, and the second epitaxial structure includes a stacked second channel layer and a barrier layer; the first channel layer includes Ga elements and N elements; The substrate includes Al elements and N elements; the substrate and the first channel layer form a hole heterojunction structure, and the second channel layer and the barrier layer form an electron heterojunction structure.

2. The semiconductor device according to claim 1, It is characterized in that The first channel layer and the second channel layer are arranged in the same layer; The hole heterojunction structure is located on a side of the electron heterojunction structure close to the substrate.

3. The semiconductor device according to claim 1, It is characterized in that The substrate includes an AlN single crystal layer or an AlN template.

4. The semiconductor device according to claim 1, It is characterized in that The thickness of the first channel layer is less than or equal to the thickness of the second channel layer.

5. The semiconductor device according to claim 4, It is characterized in that The thickness D1 of the first channel layer satisfies: 10 nm ≤ D1 ≤ 300 nm; the thickness D2 of the second channel layer satisfies: 10 nm ≤ D2 ≤ 300 nm; The thickness D3 of the barrier layer satisfies: 2nm≤D3≤50nm.

6. The semiconductor device according to claim 1, It is characterized in that The first channel layer and the second channel layer both include GaN layers; or the first channel layer and the second channel layer both include AlGaN layers; The barrier layer includes an AlGaN layer or an AlN layer.

7. The semiconductor device according to claim 1, It is characterized in that The semiconductor device further comprises a first electrode structure located on a side of the first epitaxial structure away from the substrate and a second electrode structure located on a side of the second epitaxial structure away from the substrate; The first electrode structure includes a first source, a first gate and a first drain; the first source and the first drain form ohmic contacts with the first epitaxial structure respectively; The first gate forms a Schottky contact with the first epitaxial structure; The second electrode structure includes a second source, a second gate and a second drain; the second source and the second drain form an ohmic contact with the second epitaxial structure respectively; and the second gate forms a Schottky contact with the second epitaxial structure.

8. The semiconductor device according to claim 7, It is characterized in that The P-channel metal oxide semiconductor further includes a first gate dielectric layer, and the first gate dielectric layer is located between the first gate and the first channel layer; The N-channel metal oxide semiconductor further includes a second gate dielectric layer, and the second gate dielectric layer is located between the second gate and the barrier layer.

9. A method for preparing a semiconductor device, It is characterized in that include: Providing a substrate, wherein the substrate includes Al element and N element; A P-channel metal oxide semiconductor structure and an N-channel metal oxide semiconductor structure are prepared on the same side of the substrate; the P-channel metal oxide semiconductor structure includes a first epitaxial structure, and the N-channel metal oxide semiconductor structure includes a second epitaxial structure; the first epitaxial structure includes a first channel layer, and the second epitaxial structure includes a stacked second channel layer and a barrier layer; the first channel layer includes Ga elements and N elements; The substrate and the first channel layer form a hole heterojunction structure, and the second channel layer and the barrier layer form an electron heterojunction structure.

10. The preparation method according to claim 9, It is characterized in that A P-channel metal oxide semiconductor structure and an N-channel metal oxide semiconductor structure are prepared on the same side of the substrate, comprising: preparing a channel layer on one side of the substrate; Patterning the channel layer to form a first channel layer and a second channel layer; the thickness of the first channel layer is less than or equal to the thickness of the second channel layer; A first electrode structure is prepared on a side of the first channel layer away from the substrate; a barrier layer is prepared on a side of the second channel layer away from the substrate, and a second electrode structure is prepared on a side of the barrier layer away from the substrate; the first electrode structure includes a first source, a first gate and a first drain; the first source and the first drain form ohmic contacts with the first channel layer respectively; the first gate forms a Schottky contact with the first channel layer; the second electrode structure includes a second source, a second gate and a second drain; the second source and the second drain form ohmic contacts with the barrier layer respectively; the second gate forms a Schottky contact with the barrier layer.

Citation Information

Patent Citations

  • III nitride complementary transistors

    CN107851612A

  • Structure for realizing gallium nitride CMOS (Complementary Metal Oxide Semiconductor Transistor) logic circuit