Electrolyte and secondary battery
By adding specific compounds to the electrolyte to fix transition metal ions, the problem of LNMO positive electrode material's capacity attenuation and poor high-temperature storage performance during the cycle process is solved, and the good cycle performance and high-temperature storage performance of the secondary battery are achieved, reducing the material cost.
Patent Information
- Application Number
- CN202411104240.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-13
AI Technical Summary
The capacity of lithium nickel manganese oxide (LNMO) cathode material rapidly decays during circulation and has poor storage performance under high temperature conditions. The existing doping method increases the cost of materials and is difficult to effectively solve these problems.
An electrolyte solution containing a specific compound is provided. By adding the compound, the transition metal ions are fixed on the positive electrode side to avoid the destruction of the positive electrode interface layer protective film, thereby achieving good cycling performance and high-temperature storage performance.
The good cycle performance of the secondary battery and good storage performance under high temperature conditions are achieved, gas production is suppressed, storage capacity is restored, and material costs are reduced.
Smart Images

Figure SMS_11 
Figure SMS_16 
Figure SMS_17
Abstract
Description
Technical Field
[0001] The present application relates to the field of power storage, and in particular to electrolytes and secondary batteries. Background Art
[0002] Lithium-ion batteries are the hottest power source in the field of portable electronic devices, and have recently shown great potential in electric and hybrid vehicle applications. However, the energy density of commercial lithium-ion batteries is limited, resulting in certain resistance to their promotion in the market. The energy density of lithium-ion batteries is determined by capacity and platform voltage, but high capacity and high platform voltage can lead to chemical, structural and thermodynamic instability of active materials, posing a great challenge to safety.
[0003] As the next generation of high energy density lithium-ion battery cathode material, lithium nickel manganese oxide (LNMO) has attracted widespread attention from the public. It has low processing cost, high energy density, high platform voltage, and can meet the needs of high energy density and long battery life. However, LNMO still faces the problem of rapid capacity decay during the cycle and poor storage performance at high temperatures. The current solution is to introduce dopants into the active material, such as Fe 3+ Cr 3+ 、Al 3+ 、Zr 4+ However, these doping methods pose a great challenge to material costs. Therefore, it is necessary to develop electrolyte additives that can trap metal ions when transition metal ions escape from LNMO cathode materials to overcome the above-mentioned capacity decay and poor storage performance problems. Summary of the invention
[0004] The present application mainly provides an electrolyte and a secondary battery to solve the problem of rapid capacity decay of LNMO positive electrode materials during the cycle and poor storage of new energy under high temperature conditions in the prior art. When the electrolyte containing the compound shown in Formula I provided by the present application is applied to the secondary battery, the secondary battery has good cycle performance and good storage performance under high temperature conditions.
[0005] To solve the above technical problems, this application provides the following solutions:
[0006] In a first aspect, the present application provides an electrolyte comprising a compound represented by the following formula I:
[0007] Formula I;
[0008] Among them, A is selected from an alkyl group having 1-3 carbon atoms or an alkenyl group having 2-3 carbon atoms; R1 is any one selected from an alkyl group having 1-3 carbon atoms, an alkenyl group having 2-5 carbon atoms, an ester group having 1-3 carbon atoms, a carbonyl-containing substituent having 1-3 carbon atoms and a hydrogen atom.
[0009] In a second aspect, the present application provides a secondary battery comprising the electrolyte as described above.
[0010] On the basis of conforming to the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present application.
[0011] The reagents and raw materials used in this application are commercially available.
[0012] The positive effects of this application are:
[0013] The present application provides an electrolyte, which includes a compound shown in Formula I. By adding the compound, transition metal ions can be fixed on the positive electrode side to avoid damage to the positive electrode interface layer protective film, thereby achieving good cycle performance and good storage performance under high temperature conditions. DETAILED DESCRIPTION
[0014] Electrolyte
[0015] The first aspect of the present application provides an electrolyte solution, which includes a compound represented by the following formula I:
[0016] Formula I;
[0017] Among them, A is selected from an alkyl group having 1-3 carbon atoms or an alkenyl group having 2-3 carbon atoms; R1 is any one selected from an alkyl group having 1-3 carbon atoms, an alkenyl group having 2-5 carbon atoms, an ester group having 1-3 carbon atoms, a carbonyl-containing substituent having 1-3 carbon atoms and a hydrogen atom.
[0018] The electrolyte of the present invention is suitable for secondary batteries, and generally comprises an electrolyte, a solvent and an additive. When the secondary battery is a lithium ion battery, the electrolyte is a lithium salt; when the secondary battery is a sodium ion battery, the electrolyte is a sodium salt.
[0019] In the present application, the compound represented by formula I may be:
[0020] Formula I-1;
[0021] Here, R1 is any one selected from an alkyl group having 1 to 3 carbon atoms, an alkenyl group having 2 to 5 carbon atoms, an ester group having 1 to 3 carbon atoms, a carbonyl-containing substituent having 1 to 3 carbon atoms, and a hydrogen atom.
[0022] In the present application, the compound represented by formula I is selected from at least one of the following compounds:
[0023] , , ,
[0024] , , and .
[0025] In the present application, the content of the compound represented by formula I may be 0.1 wt%-5 wt%, preferably 0.1wt%-3wt%, and more preferably 0.2 wt%-1wt%, and the percentage is the mass of the compound represented by formula I to the mass of the electrolyte. As the content of the compound represented by formula I increases, the storage capacity recovery rate and gas production performance will be better, but when its content is too much, its internal dipole interaction will make it difficult to be adsorbed at the interface, and it cannot play the role of trapping transition metal ions.
[0026] In some specific embodiments, the content of the compound represented by Formula I may be 0.1 wt%, 0.2 wt%, 0.5 wt%, 3 wt% or 5 wt%, where the percentage is the mass of the compound represented by Formula I to the mass of the electrolyte.
[0027] In the present application, the electrolyte includes an organic solvent conventionally used in the art, and the organic solvent can be any non-aqueous solvent used for non-aqueous electrolytes to date. Examples include, but are not limited to, linear or cyclic carbonates, such as ethylene carbonate, propylene carbonate, diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, dipropyl carbonate, fluoroethylene carbonate; ethers, such as 1,2-dimethoxyethane, 1,2-diethoxyethane, γ-butyrolactone, tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxolane, 4-methyl-1,3-dioxolane, diethyl ether; sulfones, such as cyclopentane sulfone, methylcyclopentane sulfone; nitriles, such as acetonitrile, propionitrile; esters, such as acetate, propionate, butyrate, etc. These non-aqueous solvents can be used alone or in combination.
[0028] In some embodiments of the present application, the organic solvent preferably includes cyclic esters and chain esters; the cyclic esters include ethylene carbonate and / or fluoroethylene carbonate; the chain esters include one or more of dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, ethyl acetate, methyl acetate, propyl acetate, ethyl propionate, trifluoroethyl methyl carbonate and bistrifluoroethyl carbonate.
[0029] Among them, the content of the cyclic ester is preferably 10wt%-30wt%, more preferably 20wt%-30wt%, for example 26.1wt%, 26.19wt%, 26.22wt%, 25.95wt%, 25.35wt% or 24.75wt%, where the percentage is the mass of the cyclic ester to the mass of the electrolyte.
[0030] Wherein, the content of the chain ester is preferably 20wt%-75wt%, for example 60.9 wt%, 61.18 wt%, 61.11wt%, 60.55 wt%, 59.15 wt% or 57.75 wt%, where the percentage is the mass of the chain ester to the mass of the electrolyte.
[0031] In some specific embodiments, the cyclic ester is fluoroethylene carbonate.
[0032] In some specific embodiments, the linear ester is trifluoroethyl methyl carbonate and / or bistrifluoroethyl carbonate.
[0033] In some specific embodiments, the organic solvent includes fluoroethylene carbonate and trifluoroethyl methyl carbonate, wherein the mass ratio of fluoroethylene carbonate to trifluoroethyl methyl carbonate is 3:7.
[0034] In the present application, the electrolyte includes a lithium salt, which may be a lithium salt conventionally used in the art, preferably one or more selected from lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethylsulfonyl)imide, lithium difluorooxalatoborate and lithium difluorooxalatophosphate.
[0035] The amount of the lithium salt is preferably 10.5 wt %-14 wt %, for example 12.5 wt %, where the percentage is the mass of the lithium salt relative to the mass of the electrolyte.
[0036] In some specific embodiments, the lithium salt includes lithium hexafluorophosphate and lithium bisfluorosulfonyl imide, and the mass ratio of lithium hexafluorophosphate to lithium bisfluorosulfonyl imide is (3.33-12):1, such as 12:1, 11:1, 5.5:1, 3.5:1 or 3.33:1.
[0037] In the present application, the electrolyte may also include 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, and the content of the 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether is preferably 25wt%-35wt%, and the percentage is the percentage of the mass of the 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether to the mass of the electrolyte.
[0038] In some specific embodiments, the content of 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether is 20 wt%, 25 wt%, 30 wt%, 35 wt% or 40 wt%.
[0039] In some specific embodiments, the electrolyte is prepared by mixing an organic solvent, a lithium salt and a compound. Preferably, the lithium salt is first mixed with the organic solvent and then the compound is added.
[0040] Secondary battery
[0041] The secondary battery provided in the second aspect of the present application includes the electrolyte as described above.
[0042] In the present application, the secondary battery may be a secondary battery known in the art, such as a lithium ion battery or a sodium ion battery, preferably a lithium ion battery, and the lithium ion battery comprises a positive electrode sheet, a negative electrode sheet, a separator and the electrolyte as described above.
[0043] Wherein, the positive electrode sheet comprises a positive electrode material layer and a composite current collector.
[0044] The positive electrode material layer may include a positive electrode active material, and a binder and a conductive agent may be further added as needed.
[0045] The positive electrode active material may be a positive electrode active material conventionally used for positive electrodes of lithium ion batteries in the art, and the positive electrode active material may include one or more of lithium cobalt oxide (LCO), lithium nickel oxide (LNO), lithium manganese oxide (LMO), lithium nickel manganese oxide (LNMO), lithium nickel cobalt manganese oxide (NCM), lithium nickel cobalt aluminum oxide (NCA) and lithium rich manganese-based oxide (LRMO).
[0046] The binder may be a component that helps the active material to bind to the conductive agent and helps the active material to bind to the current collector, and may be generally selected from polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, fluororubber, and various copolymers.
[0047] The conductive agent can be a reagent for ensuring that the electrode has good charge and discharge performance. It can be selected from graphite materials such as natural graphite and artificial graphite, carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black and other carbon black materials, carbon fibers, metal fibers and other conductive fibers, metal powders such as carbon fluoride powder, aluminum powder, nickel powder and other metal powders, zinc oxide, potassium titanate and other conductive whiskers, and titanium dioxide and other conductive metal oxides or polyphenylene derivatives.
[0048] Wherein, the negative electrode sheet comprises a negative electrode material layer and a composite current collector.
[0049] The negative electrode material layer may include a negative electrode active material, and a binder, a conductive agent, and a thickener may be further added as needed.
[0050] The negative electrode active material may be a conventional negative electrode active material in the art, and may include but is not limited to graphite.
[0051] The conductive agent may be a conventional conductive agent for negative electrode sheets in the art, and may include but is not limited to conductive carbon black.
[0052] The thickener may be a conventional thickener used for negative electrode sheets in the art, and may include but is not limited to sodium carboxymethyl cellulose.
[0053] The binder may be a conventional binder for negative electrode plates in the art, and may include but is not limited to styrene-butadiene rubber.
[0054] In some specific embodiments, the mass ratio of the negative electrode active material, the conductive agent, the binder, and the thickener is 96:2:1:1.
[0055] The separator may be a conventional separator for lithium-ion batteries in the art, for example, including but not limited to polyethylene (PE) with coating.
[0056] In some specific embodiments, the separator is a polyethylene film with a nano-aluminum oxide coating, wherein the thickness of the polyethylene-based film is 9 μm, and the thickness of the nano-aluminum oxide coating is 3 μm.
[0057] In the present application, the preparation method of the secondary battery can be a conventional preparation method in the field, which can be a battery cell obtained by winding the positive electrode sheet, the negative electrode sheet and the separator, and then packaging them in a packaging shell and injecting the electrolyte; or it can be a battery cell obtained by stacking the negative electrode sheet, the separator, the positive electrode sheet and the separator in this order, and then packaging them in a packaging shell and injecting the electrolyte.
[0058] The present application is further described below by way of examples, but the present application is not limited to the scope of the examples. The experimental methods without specific conditions in the following examples are selected according to conventional methods and conditions, or according to the product instructions.
[0059] Preparation Examples 1-7
[0060] Pyrazine and cyclic phosphate are used as reaction raw materials and dissolved in dimethyl carbonate. oC, add sodium methoxide to the mixed solution, react for 4-6 hours, remove the inorganic sodium methoxide by extraction, and obtain compound 1-7 by recrystallization.
[0061] Table 1
[0062]
[0063] Example 1
[0064] (1) Preparation of electrolyte
[0065] In a glove box with a nitrogen content of 99.999%, an actual oxygen content of 0.1 ppm and a moisture content of 0.1 ppm, fluoroethylene carbonate and trifluoroethyl methyl carbonate battery-grade organic solvents in a mass ratio of 3:7 were evenly mixed, and then fully dried lithium hexafluorophosphate was added, and then 0.5wt% of compound 1 was added to prepare an electrolyte; wherein, based on the total mass of the electrolyte being 100%, the mass percentage of lithium hexafluorophosphate was 12.5wt%.
[0066] (2) Preparation of positive electrode
[0067] The positive electrode active material LiNi 0.5 Mn 1.5 O4, conductive agent acetylene black, and binder polyvinylidene fluoride are fully stirred and mixed in an N-methylpyrrolidone solvent system in a mass ratio of 95:3:2, and then coated on aluminum foil, dried, and cold pressed to obtain a positive electrode sheet.
[0068] (3) Preparation of negative electrode sheet
[0069] The negative electrode active material graphite, the conductive agent acetylene black, the binder styrene butadiene rubber, and the thickener sodium carboxymethyl cellulose were fully stirred and mixed in a deionized water solvent system in a mass ratio of 96:2:1:1, and then coated on a copper foil, dried, and cold pressed to obtain a negative electrode sheet.
[0070] (4) Preparation of diaphragm
[0071] A polyethylene with a thickness of 9 μm is used as a base film, and a nano-aluminum oxide coating with a thickness of 3 μm is coated on the base film to obtain a separator.
[0072] (5) Assembly of secondary batteries
[0073] The positive electrode sheet, separator and negative electrode sheet prepared in the above steps are stacked in order, so that the separator is placed between the positive electrode sheet and the negative electrode sheet to play an isolating role, and the sheets are stacked to obtain a bare cell. Then the bare cell is placed in an aluminum-plastic film and then heated to 80 °C. oAfter baking at 400 °C to remove water, the electrolyte prepared in step (1) is injected and sealed. After that, the finished secondary battery is obtained through processes such as standing, hot and cold pressing, formation, clamping, and capacity division.
[0074] Example 2
[0075] The only difference from Example 1 is that Compound 2 is used instead of Compound 1.
[0076] Example 3
[0077] The only difference from Example 1 is that Compound 6 is used instead of Compound 1.
[0078] Example 4
[0079] The only difference from Example 1 is that Compound 7 is used instead of Compound 1.
[0080] Example 5
[0081] The only difference from Example 4 is that 0.1 wt % of Compound 7 is used instead of 0.5 wt % of Compound 7.
[0082] Example 6
[0083] The only difference from Example 4 is that 0.2 wt % of Compound 7 is used instead of 0.5 wt % of Compound 7.
[0084] Example 7
[0085] The only difference from Example 4 is that 1 wt % of Compound 7 is used instead of 0.5 wt % of Compound 7.
[0086] Example 8
[0087] The only difference from Example 4 is that 3 wt % of Compound 7 is used instead of 0.5 wt % of Compound 7.
[0088] Example 9
[0089] The only difference from Example 4 is that 5 wt % of Compound 7 is used instead of 0.5 wt % of Compound 7.
[0090] Example 10
[0091] The difference from Example 4 is that ethylene carbonate is used instead of fluoroethylene carbonate.
[0092] Embodiment 11
[0093] The difference from Example 4 is that bistrifluoroethyl carbonate is used instead of trifluoroethyl methyl carbonate.
[0094] Example 12
[0095] The difference from Example 4 is that dimethyl carbonate is used instead of trifluoroethyl methyl carbonate.
[0096] Example 13
[0097] The difference from Example 4 is that lithium hexafluorophosphate and lithium bisfluorosulfonyl imide are used to replace lithium hexafluorophosphate, wherein the mass ratio of lithium hexafluorophosphate to lithium bisfluorosulfonyl imide is 3.5:1.
[0098] Embodiment 14
[0099] The difference from Example 4 is that lithium hexafluorophosphate and lithium bisfluorosulfonyl imide are used to replace lithium hexafluorophosphate, wherein the mass ratio of lithium hexafluorophosphate to lithium bisfluorosulfonyl imide is 11:1.
[0100] Embodiment 15
[0101] The difference from Example 4 is that lithium hexafluorophosphate and lithium bisfluorosulfonyl imide are used to replace lithium hexafluorophosphate, wherein the mass ratio of lithium hexafluorophosphate to lithium bisfluorosulfonyl imide is 5.5:1.
[0102] Example 16
[0103] The difference from Example 4 is that 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether is used to partially replace trifluoroethyl methyl carbonate, wherein, based on the total mass of the electrolyte as 100%, the mass proportion of 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether is 20wt%.
[0104] Embodiment 17
[0105] The difference from Example 4 is that 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether is used to partially replace trifluoroethyl methyl carbonate, wherein, based on the total mass of the electrolyte as 100%, the mass proportion of 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether is 25wt%.
[0106] Embodiment 18
[0107] The difference from Example 4 is that trifluoroethyl methyl carbonate is partially replaced by 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, wherein the mass proportion of 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether is 30wt% based on the total mass of the electrolyte as 100%.
[0108] Embodiment 19
[0109] The difference from Example 4 is that 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether is used to partially replace trifluoroethyl methyl carbonate, wherein, based on the total mass of the electrolyte as 100%, the mass proportion of 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether is 35wt%.
[0110] Embodiment 20
[0111] The difference from Example 4 is that 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether is used to partially replace trifluoroethyl methyl carbonate, wherein, based on the total mass of the electrolyte as 100%, the mass proportion of 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether is 40wt%.
[0112] Comparative Example 1
[0113] The only difference from Example 4 is that Compound 7 is not added, wherein, based on the total mass of the electrolyte being 100%, the mass percentage of lithium hexafluorophosphate is 12.5 wt %, and the remainder is the organic solvent.
[0114] Comparative Example 2
[0115] The only difference from Example 4 is that Compound 8 is used instead of Compound 7. Compound 8 is pyrazine purchased from Maclean with a purity of 99%.
[0116] Comparative Example 3
[0117] The only difference from Example 4 is that Compound 9 is used to replace Compound 7. Compound 9 is composed of and The formed ionic liquid.
[0118] Comparative Example 4
[0119] The only difference from Example 4 is that Compound 10 is used to replace Compound 7. The structure of Compound 10 is , the synthetic route of compound 10 is:
[0120] .
[0121] Effect Example
[0122] 1. 60℃ storage capacity recovery rate:
[0123] At 25°C, the secondary batteries prepared in the examples and comparative examples were charged to 4.85V at 0.33C constant current, and then charged to 0.05C at constant voltage, and left to stand for 30 minutes. After repeating 2-3 times, the last 0.33C discharge capacity C1 was recorded. The fully charged batteries were then placed in a 60°C oven for 30 days (1M), the cells were cooled, and the oven temperature was adjusted to 25 oC, let stand for 10 minutes, discharge at 0.33C constant current to 2.5V, then charge and discharge at 0.33C rate, 2.5V-4.85V voltage range, after 2 cycles, record the last discharge capacity C2. Calculate the capacity recovery rate of the lithium-ion battery relative to that before storage according to the following formula, and the results are recorded in Table 2.
[0124] Capacity recovery rate (%) = (C2 / C1) × 100%
[0125] 2. Gas production growth rate:
[0126] The secondary batteries prepared in the embodiments and comparative examples were fully charged and stored in a 60°C incubator. Their volumes were tested every 7 days. The volume growth rate after 30 days of storage (1M) was recorded and calculated as the gas production growth rate. The results are recorded in Table 2.
[0127] 3.25 o C Cycle Performance
[0128] Adjust the incubator temperature to 25 o C, the secondary batteries prepared in the embodiments and comparative examples were allowed to stand for 10 min, first discharged at 1C to 3.4V, allowed to stand for 10 min, then charged at 0.5C constant current to 4.85V, and then charged at constant voltage until the current stabilized to 0.05C. After standing for half an hour, they were discharged at 1C constant current to 3.4V, which was recorded as the first discharge capacity C3. This charge and discharge process was cycled for 500cls, and the discharge capacity C4 of the 500th cycle was recorded. The capacity retention rate of the 500th cycle = (C4 / C3) × 100%. The results are recorded in Table 2.
[0129] Table 2
[0130]
[0131]
[0132] When the electrolyte provided in the present application is used in a secondary battery, the secondary battery has good cycle performance, good storage performance under high temperature conditions and inhibits gas production. In some specific embodiments, 60 o C storage capacity recovery rate @1M is more than 82.4%, 60 o C gas production growth rate @1M is less than 16.4%, 25 o The capacity retention rate of the C cycle performance for 500 cycles is above 78.3%. In a preferred embodiment, 60 o C storage capacity recovery rate @1M is more than 89.2%, 60 o C gas production growth rate @1M is less than 8.1%, 25 o The capacity retention rate of C cycle performance after 500 cycles is over 89.1%.
[0133] Examples 1-4 verify the effect data of different compounds added to the electrolyte in the present application and applied to secondary batteries. It can be seen that the secondary batteries containing different compounds all show good cycle performance, high temperature storage performance and the ability to inhibit gas production, among which compound 2 shows better effect.
[0134] Examples 4-9 verify the effect data when the same type of compound but different dosage is applied to secondary batteries. It can be seen that the dosage of conventional additives can achieve good performance, and the effect is better when the dosage is 0.1 wt%-3wt%, and the effect is even better when the dosage is 0.2 wt%-1wt%.
[0135] Examples 4 and 10-12 verify that the amount of organic solvent is the same, but the type is different; Examples 4 and 13-15 verify that the type and amount of lithium salt are different; Examples 4 and Examples 16-20 verify different amounts of 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether; It can be seen that only changing the type of organic solvent, the type of lithium salt or other additives, combined with other features, will have a certain impact on the technical effect, but can solve the technical problems of this application. The pyrazine group of the compound of the present application contains a lone pair of electrons on the p orbital of the nitrogen atom exposed on the outside, which will interact with the empty d orbital of the transition metal ion to complex the transition metal ion; and the phosphate group will be adsorbed on the positive electrode side due to electrostatic interaction, ensuring the pyrazine group's complexing ability; through the coordination of the pyrazine group and the phosphate, the transition metal ion is fixed on the positive electrode side to avoid the destruction of the positive electrode interface layer protective film, thereby achieving good cycle performance and good storage performance under high temperature conditions.
[0136] Compared with the examples, Comparative Example 1 does not contain the compound of the present application. It can be seen that 60 o C Storage capacity recovery rate @1M, 60 o C gas production growth rate @1M, and 25 o The capacity retention rate of C cycle performance after 500 cycles is very poor.
[0137] Comparative Examples 2-4 are compared with Example 4, and the difference is that the compounds are different, and the effects of various aspects are also reduced to varying degrees. It can be seen from the comparison of Comparative Examples 2 and 3 that the zwitterionic structure of the compound is the key to improving performance, and the lack of a part of it or not connected in a covalent bond manner cannot achieve the effect of the present application. It can also be seen from the comparison with Comparative Example 4 that even if the zwitterions are connected in a covalent bond manner, their structure is not within the scope of the present application, and the effect of the present application cannot be achieved.
[0138] The embodiments described above are only some embodiments of the present application, which are convenient for those skilled in the art to understand and use the present application. Obviously, any person skilled in the art can slightly modify or change the present embodiment and apply it to other embodiments without creative work. Therefore, the present application is not limited to the above embodiments, and any equal changes, simple modifications and modifications made within the scope of the present application still belong to the scope of the present application.
Claims
1. An electrolyte, characterized in that: It includes the compound shown in the following formula I: Formula I; Among them, A is selected from an alkyl group having 1-3 carbon atoms or an alkenyl group having 2-3 carbon atoms; R1 is any one selected from an alkyl group having 1-3 carbon atoms, an alkenyl group having 2-5 carbon atoms, an ester group having 1-3 carbon atoms, a carbonyl-containing substituent having 1-3 carbon atoms and a hydrogen atom.
2. The electrolyte according to claim 1, characterized in that The compound represented by formula I is: Formula I-1; Here, R1 is any one selected from an alkyl group having 1 to 3 carbon atoms, an alkenyl group having 2 to 5 carbon atoms, an ester group having 1 to 3 carbon atoms, a carbonyl-containing substituent having 1 to 3 carbon atoms, and a hydrogen atom.
3. The electrolyte according to claim 1, characterized in that The compound represented by formula I is selected from at least one of the following compounds: , , , , , and .
4. The electrolyte according to claim 1, characterized in that The content of the compound represented by formula I is 0.1wt%-3wt%, and the percentage is the percentage of the mass of the compound to the mass of the electrolyte.
5. The electrolyte according to claim 1, characterized in that The electrolyte satisfies one or two of the following conditions (1)-(2): (1) The electrolyte includes an organic solvent, and the organic solvent includes a cyclic ester and a chain ester; the cyclic ester includes ethylene carbonate and / or fluoroethylene carbonate; the chain ester includes one or more of dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, ethyl acetate, methyl acetate, propyl acetate, ethyl propionate, trifluoroethyl methyl carbonate and bistrifluoroethyl carbonate; (2) The electrolyte includes a lithium salt, and the lithium salt is selected from one or more of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethylsulfonyl)imide and lithium difluorooxalatoborate.
6. The electrolyte according to claim 5, characterized in that The electrolyte satisfies one or more of the following conditions (1)-(3): (1) The content of the cyclic ester is 10wt%-30wt%, where the percentage is the mass of the cyclic ester relative to the mass of the electrolyte; (2) The content of the chain ester is 20wt%-75wt%, where the percentage is the percentage of the mass of the chain ester to the mass of the electrolyte; (3) The content of the lithium salt is 10.5 wt %-14 wt %, where the percentage is the mass of the lithium salt relative to the mass of the electrolyte.
7. The electrolyte according to claim 5, characterized in that The lithium salt includes lithium hexafluorophosphate and lithium bis(fluorosulfonyl)imide, and the mass ratio of the lithium hexafluorophosphate to the lithium bis(fluorosulfonyl)imide is (3.33-12):
1.
8. The electrolyte according to claim 1, characterized in that The electrolyte includes 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether.
9. The electrolyte according to claim 8, characterized in that The content of the 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether is 25wt%-35wt%, and the percentage is the percentage of the mass of the 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether to the mass of the electrolyte.
10. A secondary battery, characterized in that: It comprises the electrolyte according to any one of claims 1 to 9.