A battery nanofiber barrier film and preparation method thereof

The preparation of nanofiber barrier membranes through electrospinning technology solves the problems of low porosity and poor thermal stability of lithium-ion battery separators, achieves higher electrolyte absorption and mechanical properties, and extends the service life of the battery.

CN118630422BActive Publication Date: 2024-11-22QINGDAO UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410875014.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-11-22
Estimated Expiration
2044-07-02

AI Technical Summary

Technical Problem

At this stage, the porosity and poor thermal stability of lithium-ion battery separators have low porosity and poor thermal stability, resulting in low liquid absorption of the battery and shrinking the size of the membrane at high temperatures, affecting the normal use of the battery.

Method used

The nanofiber barrier membrane of battery is prepared by electrospinning technology. By mixing functional filler and polyamic acid solution, a porous structure and core-shell structure are formed, which enhances mechanical properties and conductivity, prevents the membrane from shrinking, and remains stable under high temperature conditions. .

Benefits of technology

It improves the battery's absorption capacity and ion conductivity to the electrolyte, extends the battery's cycle life, and ensures the battery's safety and normal use at high temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004922745160000111
    Figure BDA0004922745160000111
  • Figure BDA0004922745160000121
    Figure BDA0004922745160000121
Patent Text Reader

Abstract

The invention discloses a battery nanofiber barrier membrane and a preparation method thereof. The membrane is prepared by mixing a functionalized filler and a polyamic acid solution and performing electrostatic spinning. The functionalized filler has a porous structure inside and a porous cellulose structure on the surface, which can enhance the absorption of electrolyte by the barrier membrane, and forms a multi-layer coated core-shell structure to enhance the mechanical properties of the barrier membrane. The imide segment contains an organosilicon segment and a benzene ring structure, and the membrane is cross-linked by the functionalized filler so that when the battery temperature rises, the membrane will not soften and shrink, thereby ensuring the safety of the battery membrane. The functionalized filler can support the barrier membrane and effectively prevent the shrinkage of the barrier membrane. Meanwhile, the porous cavity structure and its own conductivity can accelerate the transfer of lithium ions between electrodes, effectively improving the ion conductivity, thereby enhancing the battery cycle life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery barrier film preparation, and in particular to a battery nanofiber barrier film and a preparation method thereof. Background Art

[0002] Lithium batteries are successfully used in portable devices such as mobile phones, computers and cameras because of their high energy density, stable cycle characteristics, low discharge rate and high operating voltage. Lithium-ion batteries are mainly composed of four major components: positive electrode, negative electrode, electrolyte and separator. The separator isolates the positive and negative electrodes to prevent the internal short circuit of the battery caused by the physical contact between the two electrodes, and at the same time realizes the free transfer of lithium ions during battery charging and discharging. The commercial separators currently used in lithium-ion batteries are polyethylene separators, polypropylene separators and their composite separators. These separators have good chemical stability and mechanical strength and are used in portable electronic devices. However, these separators have two inherent limitations: one is low porosity. The low porosity caused by its semi-crystalline structure and melt-blown technology hinders the absorption of liquid electrolyte by the separator, making the separator have poor electrolyte wettability, resulting in low rate capability of the battery; the other is poor thermal stability, which causes this type of separator to show severe dimensional shrinkage at high temperatures, affecting the normal use of the battery. Summary of the invention

[0003] The purpose of the present invention is to provide a battery nanofiber barrier membrane and a preparation method thereof, which solves the problems of low liquid absorption rate of battery barrier membranes at the current stage and shrinkage of battery membranes after long-term use.

[0004] The technical problems to be solved by the present invention are:

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A method for preparing a battery nanofiber barrier film specifically comprises the following steps:

[0007] Step A1: Tetramethyltetraphenylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, tetramethylammonium hydroxide and dimethyl sulfoxide are uniformly mixed, nitrogen is introduced for protection, and the reaction is carried out for 3-5 hours at a speed of 120-150 r / min and a temperature of 90-95° C. to obtain a modified monomer;

[0008] Step A2: The modified filler, thionyl chloride and tetrahydrofuran are mixed, and the reaction is carried out for 1-1.5 hours at a speed of 120-150 r / min and a temperature of 40-50° C. to obtain a functionalized filler; the modified monomer, 4,4'-diaminodiphenyl ether, 3,3'-dihydroxybenzidine, pyromellitic acid dianhydride and N,N-dimethylformamide are mixed, nitrogen is introduced for protection, and the reaction is stirred for 20-25 hours at a speed of 200-300 r / min and a temperature of 25-30° C. to obtain a polyamic acid solution;

[0009] Step A3: Evenly mix the functional filler, nanocellulose and polyamic acid solution, stir and add potassium carbonate to a pH value of 8.5-9 at a rotation speed of 120-150r / min, stir for 4-6h, adjust the pH value to 5-6, and electrospin into a film and dry it at a voltage of 20-25kv, a liquid feed volume of 1.2-1.5mL / h, and a receiving distance of 18-20cm. Then, keep warm for 40-50min at 100°C, 200°C and 250°C, respectively, to obtain a battery nanofiber barrier membrane.

[0010] Furthermore, the usage ratio of tetramethyltetraphenylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane and tetramethylammonium hydroxide described in step A1 is 2:1:1.2.

[0011] Furthermore, the modified filler and thionyl chloride described in step A2 are used in a ratio of 1 g:3 mL, and the modified monomer, 4,4'-diaminodiphenyl ether, 3,3'-dihydroxybenzidine, pyromellitic acid dianhydride and N,N-dimethylformamide are used in a ratio of 1 mmol:5 mmol:1 mmol:7 mmol:10 mL.

[0012] Furthermore, the dosage ratio of the functional filler, nanocellulose and polyamic acid solution described in step A3 is 80 mg:5 mg:3 mL.

[0013] Further, the modified filler is prepared by the following steps:

[0014] Step B1: dissolving zirconium tetrachloride in N,N-dimethylformamide, stirring and adding 2,5-dimercaptoterephthalic acid at a speed of 120-150 r / min and a temperature of 25-30° C., raising the temperature to 85-90° C., reacting for 20-25 hours, filtering to remove the filtrate, dispersing the filter cake in toluene, adding γ-methacryloxypropyltrimethoxysilane and benzophenone, reacting for 2-3 hours at a speed of 60-80 r / min and irradiating with 365 nm ultraviolet light, to obtain a zirconium organic framework;

[0015] Step B2: Mix the zirconium organic framework, methyltriethoxysilane, dimethyldimethoxysilane and ethanol uniformly, stir and add deionized water and hydrochloric acid at a speed of 120-150r / min and a temperature of 70-75°C, react for 2-3h, add tetrabutyl titanate, react for 3-5h, distill off the ethanol, heat to 120-130°C, react for 4-6h, centrifuge to remove the supernatant, place the substrate in a tube furnace, keep warm for 3-4h at a temperature of 500-550°C under argon protection, and obtain a precursor;

[0016] Step B3: Disperse the precursor in ethanol, stir and add γ-aminopropyltriethoxysilane and deionized water at a speed of 120-150r / min and a temperature of 60-65°C, and react for 2-3h to obtain a modified precursor, mix the modified precursor, carboxymethyl cellulose, dicyclohexylcarbodiimide and acetone, and react for 3-5h at a speed of 200-300r / min and a temperature of 50-60°C to obtain a modified filler.

[0017] Furthermore, the molar ratio of zirconium tetrachloride, 2,5-dimercaptoterephthalic acid and γ-methacryloxypropyltrimethoxysilane in step B1 is 1:1:2.2, and the amount of benzophenone is 2% of the mass of γ-methacryloxypropyltrimethoxysilane.

[0018] Furthermore, the amount ratio of the zirconium organic framework, methyltriethoxysilane, dimethyldimethoxysilane, ethanol, deionized water, hydrochloric acid and tetrabutyl titanate described in step B2 is 1g:5mL:8mL:30mL:10mL:1mL:3mL, and the mass fraction of hydrochloric acid is 5%.

[0019] Furthermore, the amount of γ-aminopropyltriethoxysilane used in step B3 is 3% of the mass of the precursor, and the mass ratio of the modified precursor, carboxymethyl cellulose, and dicyclohexylcarbodiimide is 1:5:0.5.

[0020] Beneficial effects of the present invention: A battery nanofiber barrier membrane prepared by the present invention is prepared by mixing a functionalized filler and a polyamic acid solution and electrospinning, wherein the functionalized filler is prepared by using a modified filler and thionyl chloride as raw materials, so that the carboxyl group on the surface of the modified filler reacts with the thionyl chloride to form an acyl chloride, and the modified filler is complexed with zirconium tetrachloride and 2,5-dimercaptoterephthalic acid to form a metal organic framework, and then under the condition of ultraviolet light irradiation, the double bond on the γ-methacryloxypropyltrimethoxysilane is grafted with the thiol group on the metal organic framework to prepare a zirconium organic film. The invention discloses a novel nanostructured carbon nanotube composite material, wherein the nanostructured carbon nanotube is prepared by hydrolyzing and condensing a zirconium organic framework, methyltriethoxysilane, dimethyldimethoxysilane and tetrabutyl titanate to form titanium-containing organic silicon on the surface of the zirconium organic framework, and then calcining the nanostructured carbon nanotube at high temperature in an argon atmosphere to form a composite precursor of carbon tubes, silicon dioxide and titanium dioxide, treating the precursor with γ-aminopropyltriethoxysilane to cut off active amino groups on the surface of the precursor to obtain a modified precursor, and reacting the modified precursor with carboxymethyl cellulose to dehydrate the amino groups on the modified precursor and the carboxyl groups on the carboxymethyl cellulose to obtain a modified filler.

[0021] The polyamic acid solution is subjected to ring-opening polymerization with tetramethyltetraphenylcyclotetrasiloxane and 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane as raw materials to form a polysiloxane containing amino groups at both ends to obtain a modified monomer, and the modified monomer, 4,4'-diaminodiphenyl ether, 3,3'-dihydroxybenzidine and pyromellitic acid dianhydride are subjected to condensation reaction to obtain a polyamic acid solution, and the polyamic acid solution and a functional filler are blended under alkaline conditions to react the acyl chloride on the functional filler with the phenolic hydroxyl group of the side chain of the polyamic acid molecular chain to crosslink the linear polyamic acid molecular chain, and then thermal imidization is carried out under high temperature conditions to obtain a barrier film.

[0022] The functional filler has a porous structure inside and a porous cellulose structure on the surface, which can enhance the absorption of electrolyte by the barrier membrane, and form a multi-layer coated core-shell structure to increase the mechanical properties of the barrier membrane. The imide segment contains silicone segments and benzene ring structures, and is cross-linked by the functional filler, so that the membrane is not prone to softening and shrinking when the battery temperature rises, thereby ensuring the safety of the battery membrane. The functional filler can support the barrier membrane and effectively prevent the shrinkage of the barrier membrane. At the same time, the porous cavity structure and its own conductivity can accelerate the transfer of lithium ions between electrodes, effectively improving the ion conductivity, thereby increasing the battery cycle life. DETAILED DESCRIPTION

[0023] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] Example 1

[0025] A method for preparing a battery nanofiber barrier film specifically comprises the following steps:

[0026] Step A1: Tetramethyltetraphenylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, tetramethylammonium hydroxide and dimethyl sulfoxide are uniformly mixed, nitrogen is introduced for protection, and the mixture is reacted for 3 hours at a speed of 120 r / min and a temperature of 90° C. to obtain a modified monomer;

[0027] Step A2: The modified filler, thionyl chloride and tetrahydrofuran are mixed, and the reaction is carried out at a speed of 120 r / min and a temperature of 40° C. for 1 hour to obtain a functional filler; the modified monomer, 4,4'-diaminodiphenyl ether, 3,3'-dihydroxybenzidine, pyromellitic dianhydride and N,N-dimethylformamide are mixed, nitrogen is introduced for protection, and the mixture is stirred at a speed of 200 r / min and a temperature of 25° C. for 20 hours to obtain a polyamic acid solution;

[0028] Step A3: Mix the functional filler, nanocellulose and polyamic acid solution evenly, stir and add potassium carbonate to the pH value of 8.5 at a rotation speed of 120r / min, stir for 4h, adjust the pH value to 5, and electrospin into a film and dry it at a voltage of 20kv, a liquid feed volume of 1.2mL / h, and a receiving distance of 18cm. Then, keep the temperature at 100℃, 200℃ and 250℃ for 40min to obtain a battery nanofiber barrier membrane.

[0029] The usage ratio of tetramethyltetraphenylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane and tetramethylammonium hydroxide described in step A1 is 2:1:1.2.

[0030] The modified filler and thionyl chloride described in step A2 are used in a ratio of 1 g:3 mL, and the modified monomer, 4,4'-diaminodiphenyl ether, 3,3'-dihydroxybenzidine, pyromellitic acid dianhydride and N,N-dimethylformamide are used in a ratio of 1 mmol:5 mmol:1 mmol:7 mmol:10 mL.

[0031] The dosage ratio of the functional filler, nanocellulose and polyamic acid solution described in step A3 is 80 mg:5 mg:3 mL.

[0032] The modified filler is prepared by the following steps:

[0033] Step B1: dissolving zirconium tetrachloride in N,N-dimethylformamide, stirring and adding 2,5-dimercaptoterephthalic acid at a speed of 120 r / min and a temperature of 25°C, heating to 85°C, reacting for 20 hours, filtering to remove the filtrate, dispersing the filter cake in toluene, adding γ-methacryloxypropyltrimethoxysilane and benzophenone, reacting for 2 hours at a speed of 60 r / min and irradiating with 365 nm ultraviolet light, to obtain a zirconium organic framework;

[0034] Step B2: Mix the zirconium organic framework, methyltriethoxysilane, dimethyldimethoxysilane and ethanol uniformly, stir and add deionized water and hydrochloric acid at a speed of 120 r / min and a temperature of 70°C, react for 2 hours, add tetrabutyl titanate, react for 3 hours, distill off the ethanol, heat to 120°C, react for 4 hours, centrifuge to remove the supernatant, place the substrate in a tube furnace, keep warm for 3 hours at a temperature of 500°C under argon protection, and obtain a precursor;

[0035] Step B3: Disperse the precursor in ethanol, stir and add γ-aminopropyltriethoxysilane and deionized water at a speed of 120 r / min and a temperature of 60°C, and react for 2 hours to obtain a modified precursor. Mix the modified precursor, carboxymethyl cellulose, dicyclohexylcarbodiimide and acetone, and react for 3 hours at a speed of 200 r / min and a temperature of 50°C to obtain a modified filler.

[0036] The molar ratio of zirconium tetrachloride, 2,5-dimercaptoterephthalic acid and γ-methacryloxypropyltrimethoxysilane in step B1 is 1:1:2.2, and the amount of benzophenone is 2% of the mass of γ-methacryloxypropyltrimethoxysilane.

[0037] The amount ratio of the zirconium organic framework, methyltriethoxysilane, dimethyldimethoxysilane, ethanol, deionized water, hydrochloric acid and tetrabutyl titanate described in step B2 is 1g:5mL:8mL:30mL:10mL:1mL:3mL, and the mass fraction of hydrochloric acid is 5%.

[0038] The amount of γ-aminopropyltriethoxysilane used in step B3 is 3% of the mass of the precursor, and the mass ratio of the modified precursor, carboxymethyl cellulose, and dicyclohexylcarbodiimide is 1:5:0.5.

[0039] Example 2

[0040] A method for preparing a battery nanofiber barrier film specifically comprises the following steps:

[0041] Step A1: Tetramethyltetraphenylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, tetramethylammonium hydroxide and dimethyl sulfoxide are uniformly mixed, nitrogen is introduced for protection, and the mixture is reacted for 4 hours at a speed of 120 r / min and a temperature of 95° C. to obtain a modified monomer;

[0042] Step A2: The modified filler, thionyl chloride and tetrahydrofuran are mixed, and the reaction is carried out at a speed of 120 r / min and a temperature of 45° C. for 1.3 hours to obtain a functional filler; the modified monomer, 4,4'-diaminodiphenyl ether, 3,3'-dihydroxybenzidine, pyromellitic acid dianhydride and N,N-dimethylformamide are mixed, nitrogen is introduced for protection, and the mixture is stirred at a speed of 200 r / min and a temperature of 28° C. for 23 hours to obtain a polyamic acid solution;

[0043] Step A3: Mix the functional filler, nanocellulose and polyamic acid solution evenly, stir and add potassium carbonate to a pH value of 9 at a rotation speed of 120 r / min, stir for 5 hours, adjust the pH value to 6, and electrospin into a film and dry it at a voltage of 20 kv, a liquid feed volume of 1.5 mL / h, and a receiving distance of 18 cm. Then, keep the temperature at 100°C, 200°C and 250°C for 45 minutes to obtain a battery nanofiber barrier membrane.

[0044] The usage ratio of tetramethyltetraphenylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane and tetramethylammonium hydroxide described in step A1 is 2:1:1.2.

[0045] The modified filler and thionyl chloride described in step A2 are used in a ratio of 1 g:3 mL, and the modified monomer, 4,4'-diaminodiphenyl ether, 3,3'-dihydroxybenzidine, pyromellitic acid dianhydride and N,N-dimethylformamide are used in a ratio of 1 mmol:5 mmol:1 mmol:7 mmol:10 mL.

[0046] The dosage ratio of the functional filler, nanocellulose and polyamic acid solution described in step A3 is 80 mg:5 mg:3 mL.

[0047] The modified filler is prepared by the following steps:

[0048] Step B1: dissolving zirconium tetrachloride in N,N-dimethylformamide, stirring and adding 2,5-dimercaptoterephthalic acid at a speed of 120 r / min and a temperature of 28°C, heating to 90°C, reacting for 25 hours, filtering to remove the filtrate, dispersing the filter cake in toluene, adding γ-methacryloxypropyltrimethoxysilane and benzophenone, reacting for 3 hours at a speed of 60 r / min and irradiating with 365 nm ultraviolet light, to obtain a zirconium organic framework;

[0049] Step B2: Mix the zirconium organic framework, methyltriethoxysilane, dimethyldimethoxysilane and ethanol uniformly, stir and add deionized water and hydrochloric acid at a speed of 120 r / min and a temperature of 75°C, react for 2 hours, add tetrabutyl titanate, react for 4 hours, distill off the ethanol, heat to 125°C, react for 5 hours, centrifuge to remove the supernatant, place the substrate in a tube furnace, keep warm for 4 hours at a temperature of 530°C under argon protection, and obtain a precursor;

[0050] Step B3: Disperse the precursor in ethanol, stir and add γ-aminopropyltriethoxysilane and deionized water at a speed of 120 r / min and a temperature of 65°C, and react for 2 hours to obtain a modified precursor. Mix the modified precursor, carboxymethyl cellulose, dicyclohexylcarbodiimide and acetone, and react for 4 hours at a speed of 300 r / min and a temperature of 55°C to obtain a modified filler.

[0051] The molar ratio of zirconium tetrachloride, 2,5-dimercaptoterephthalic acid and γ-methacryloxypropyltrimethoxysilane in step B1 is 1:1:2.2, and the amount of benzophenone is 2% of the mass of γ-methacryloxypropyltrimethoxysilane.

[0052] The amount ratio of the zirconium organic framework, methyltriethoxysilane, dimethyldimethoxysilane, ethanol, deionized water, hydrochloric acid and tetrabutyl titanate described in step B2 is 1g:5mL:8mL:30mL:10mL:1mL:3mL, and the mass fraction of hydrochloric acid is 5%.

[0053] The amount of γ-aminopropyltriethoxysilane used in step B3 is 3% of the mass of the precursor, and the mass ratio of the modified precursor, carboxymethyl cellulose, and dicyclohexylcarbodiimide is 1:5:0.5.

[0054] Example 3

[0055] A method for preparing a battery nanofiber barrier film specifically comprises the following steps:

[0056] Step A1: Tetramethyltetraphenylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, tetramethylammonium hydroxide and dimethyl sulfoxide are uniformly mixed, nitrogen is introduced for protection, and the mixture is reacted for 5 hours at a speed of 150 r / min and a temperature of 95° C. to obtain a modified monomer;

[0057] Step A2: The modified filler, thionyl chloride and tetrahydrofuran are mixed, and the reaction is carried out at a speed of 150 r / min and a temperature of 50° C. for 1.5 hours to obtain a functional filler; the modified monomer, 4,4'-diaminodiphenyl ether, 3,3'-dihydroxybenzidine, pyromellitic dianhydride and N,N-dimethylformamide are mixed, nitrogen is introduced for protection, and the mixture is stirred at a speed of 300 r / min and a temperature of 30° C. for 25 hours to obtain a polyamic acid solution;

[0058] Step A3: Mix the functional filler, nanocellulose and polyamic acid solution evenly, stir and add potassium carbonate to a pH value of 9 at a rotation speed of 150 r / min, stir for 6 hours, adjust the pH value to 6, and electrospin into a film and dry it at a voltage of 25 kv, a liquid feed volume of 1.5 mL / h, and a receiving distance of 20 cm. Then, keep the temperature at 100°C, 200°C and 250°C for 50 minutes to obtain a battery nanofiber barrier membrane.

[0059] The usage ratio of tetramethyltetraphenylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane and tetramethylammonium hydroxide described in step A1 is 2:1:1.2.

[0060] The modified filler and thionyl chloride described in step A2 are used in a ratio of 1 g:3 mL, and the modified monomer, 4,4'-diaminodiphenyl ether, 3,3'-dihydroxybenzidine, pyromellitic acid dianhydride and N,N-dimethylformamide are used in a ratio of 1 mmol:5 mmol:1 mmol:7 mmol:10 mL.

[0061] The dosage ratio of the functional filler, nanocellulose and polyamic acid solution described in step A3 is 80 mg:5 mg:3 mL.

[0062] The modified filler is prepared by the following steps:

[0063] Step B1: dissolving zirconium tetrachloride in N,N-dimethylformamide, stirring and adding 2,5-dimercaptoterephthalic acid at a speed of 150 r / min and a temperature of 30°C, raising the temperature to 90°C, reacting for 25 hours, filtering to remove the filtrate, dispersing the filter cake in toluene, adding γ-methacryloxypropyltrimethoxysilane and benzophenone, reacting for 3 hours at a speed of 80 r / min and irradiating with 365 nm ultraviolet light, to obtain a zirconium organic framework;

[0064] Step B2: Mix the zirconium organic framework, methyltriethoxysilane, dimethyldimethoxysilane and ethanol uniformly, stir and add deionized water and hydrochloric acid at a speed of 150 r / min and a temperature of 75°C, react for 3 hours, add tetrabutyl titanate, react for 5 hours, distill off the ethanol, heat to 130°C, react for 6 hours, centrifuge to remove the supernatant, place the substrate in a tube furnace, keep warm for 4 hours at a temperature of 550°C under argon protection, and obtain a precursor;

[0065] Step B3: Disperse the precursor in ethanol, stir and add γ-aminopropyltriethoxysilane and deionized water at a speed of 150 r / min and a temperature of 65°C, and react for 3 hours to obtain a modified precursor. Mix the modified precursor, carboxymethyl cellulose, dicyclohexylcarbodiimide and acetone, and react for 5 hours at a speed of 300 r / min and a temperature of 60°C to obtain a modified filler.

[0066] The molar ratio of zirconium tetrachloride, 2,5-dimercaptoterephthalic acid and γ-methacryloxypropyltrimethoxysilane in step B1 is 1:1:2.2, and the amount of benzophenone is 2% of the mass of γ-methacryloxypropyltrimethoxysilane.

[0067] The amount ratio of the zirconium organic framework, methyltriethoxysilane, dimethyldimethoxysilane, ethanol, deionized water, hydrochloric acid and tetrabutyl titanate described in step B2 is 1g:5mL:8mL:30mL:10mL:1mL:3mL, and the mass fraction of hydrochloric acid is 5%.

[0068] The amount of γ-aminopropyltriethoxysilane used in step B3 is 3% of the mass of the precursor, and the mass ratio of the modified precursor, carboxymethyl cellulose, and dicyclohexylcarbodiimide is 1:5:0.5.

[0069] Comparative Example 1

[0070] Compared with Example 1, this comparative example uses modified filler instead of functional filler, and the other steps are the same.

[0071] Comparative Example 2

[0072] Compared with Example 1, this comparative example uses a precursor instead of a functional filler, and the remaining steps are the same.

[0073] Comparative Example 3

[0074] Compared with Example 1, tetrabutyl titanate was not added in this comparative example, and the remaining steps were the same.

[0075] Comparative Example 4

[0076] Compared with Example 1, no modified monomer was added in this comparative example, and the remaining steps were the same.

[0077] Comparative Example 5

[0078] Compared with Example 1, this comparative example did not add 3,3'-dihydroxybenzidine, and the remaining steps were the same.

[0079] The barrier films prepared in Examples 1-3 and Comparative Examples 1-5 were made into samples with a thickness of 30 μm, and the samples were cut into 2×2 cm squares and immersed in a lithium ion liquid electrolyte for 4 h. The electrolyte floating on the membrane surface was wiped off and the liquid absorption rate was calculated. The barrier films prepared in Examples 1-3 and Comparative Examples 1-5 were cut into discs with a diameter of 1.96 cm and fully soaked in the electrolyte. The diaphragm was removed and placed between two stainless steel poles and packaged with a CR2032 button battery shell. The batteries were placed at 25°C, 50°C, and 100°C, respectively. The batteries were charged at a constant current of 1C with a cutoff current of 0.05C. After the batteries were fully charged, they were placed for 5 min, and then discharged at a constant current of 0.5C to a cutoff voltage of 3.0V. The capacity retention rate of 500 cycles was calculated, and the test results are as follows.

[0080]

[0081]

[0082] It can be seen from the above table that the present application has a good effect of absorbing electrolyte and can still be used well under high temperature conditions.

[0083] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

Claims

1. A method for preparing a battery nanofiber barrier film, characterized in that: The specific steps include: Step A1: tetramethyltetraphenylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, tetramethylammonium hydroxide and dimethyl sulfoxide are mixed and reacted to prepare a modified monomer; Step A2: mixing and reacting the modified filler, thionyl chloride and tetrahydrofuran to obtain a functionalized filler, and mixing and stirring the modified monomer, 4,4'-diaminodiphenyl ether, 3,3'-dihydroxybenzidine, pyromellitic acid dianhydride and N,N-dimethylformamide to obtain a polyamic acid solution; Step A3: The functional filler, nanocellulose and polyamic acid solution are mixed and stirred, and potassium carbonate is added to the pH value to 8.5-9. After stirring, the pH is adjusted to be acidic, electrospun into a film and dried, and then kept warm for 40-50 minutes at 100° C., 200° C. and 250° C. in sequence to obtain a battery nanofiber barrier film; The modified filler is prepared by the following steps: Step B1: dissolving zirconium tetrachloride in N,N-dimethylformamide, stirring, and adding 2,5-dimercaptoterephthalic acid, heating to react, filtering to remove the filtrate, dispersing the filter cake in toluene, adding γ-methacryloxypropyltrimethoxysilane and benzophenone, and reacting to obtain a zirconium organic framework; Step B2: Mix and stir the zirconium organic framework, methyltriethoxysilane, dimethyldimethoxysilane and ethanol, add deionized water and hydrochloric acid, react, add tetrabutyl titanate, react, distill to remove ethanol, heat to react, centrifuge to remove supernatant, place the substrate in a tube furnace for high temperature insulation, and obtain a precursor; Step B3: Disperse the precursor in ethanol, stir, add γ-aminopropyltriethoxysilane and deionized water, react to obtain a modified precursor, mix the modified precursor, carboxymethyl cellulose, dicyclohexylcarbodiimide and acetone to obtain a modified filler.

2. The method for preparing a battery nanofiber barrier membrane according to claim 1, characterized in that: The usage ratio of tetramethyltetraphenylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane and tetramethylammonium hydroxide described in step A1 is 2:1:1.

2.

3. The method for preparing a battery nanofiber barrier membrane according to claim 1, characterized in that: The modified filler and thionyl chloride described in step A2 are used in a ratio of 1 g:3 mL, and the modified monomer, 4,4'-diaminodiphenyl ether, 3,3'-dihydroxybenzidine, pyromellitic dianhydride and N,N-dimethylformamide are used in a ratio of 1 mmol:5 mmol:1 mmol:7 mmol:10 mL.

4. The method for preparing a battery nanofiber barrier membrane according to claim 1, characterized in that: The dosage ratio of the functional filler, nanocellulose and polyamic acid solution described in step A3 is 80 mg:5 mg:3 mL.

5. The method for preparing a battery nanofiber barrier membrane according to claim 1, characterized in that: The molar ratio of zirconium tetrachloride, 2,5-dimercaptoterephthalic acid and γ-methacryloxypropyltrimethoxysilane in step B1 is 1:1:2.

2.

6. The method for preparing a battery nanofiber barrier membrane according to claim 1, characterized in that: The amount ratio of the zirconium organic framework, methyltriethoxysilane, dimethyldimethoxysilane, ethanol, deionized water, hydrochloric acid and tetrabutyl titanate described in step B2 is 1g:5mL:8mL:30mL:10mL:1mL:3mL.

7. The method for preparing a battery nanofiber barrier membrane according to claim 1, characterized in that: The amount of γ-aminopropyltriethoxysilane used in step B3 is 3% of the mass of the precursor, and the mass ratio of the modified precursor, carboxymethyl cellulose, and dicyclohexylcarbodiimide is 1:5:0.

5.

8. A battery nanofiber barrier film, characterized in that: Prepared according to any one of claims 1 to 7.