Antimony selenide-Aspergillus niger derived carbon-MXene composite material and preparation method and application thereof
Through the preparation of antimony selenide-Aspergillus niger-derived carbon-MXene composites, the problem of low transportation speed and storage efficiency of alkali metal ions in sodium/potassium ion batteries is solved, and high capacity and cycle stability is achieved, suitable for large-scale Large-scale energy storage equipment and reduce production costs.
Patent Information
- Application Number
- CN202411109872.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-14
AI Technical Summary
The existing sodium/potassium ion batteries are difficult to meet commercial standards due to the low transportation speed and storage efficiency of alkali metal ions, and the problem of shortage of lithium resources has not been effectively solved.
Using antimony selenide-Asperthurium niger-derived carbon-MXene composite material as the negative electrode material, A. niger is cultivated in the MXene dispersion, adsorb antimony metal and MXene, and annealing and selenization treatment to form an inner carbon band of Asperthurium niger. antimony selenide and MXene structure wrapped around the surface of the carbon tape.
It achieves high reversible capacity and excellent cycle stability, and is suitable for large-scale energy storage equipment, reducing production costs and improving material safety.
Smart Images

Figure CN118637621B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of sodium / potassium ion batteries, and in particular relates to an antimony selenide-Aspergillus niger-derived carbon-MXene composite material and a preparation method and application thereof. Background Art
[0002] Sodium / potassium ion batteries (SIBs / PIBs) prepared using sodium / potassium elements, which are abundant and low-cost on the earth, are expected to replace current lithium-ion batteries (LIBs) and solve the problem of lithium resource shortage. However, due to the large ionic radius of sodium and potassium, they are not compatible with graphite materials used as negative electrodes in lithium-ion batteries. Therefore, it is imperative to explore new high-performance electrode materials, improve the transport speed and storage efficiency of larger alkali metal ions, improve battery performance, and meet the standards required for commercialization.
[0003] Aspergillus niger is a fungus with a nanobelt structure of hyphae. The chitin contained in its cell wall can be converted into highly conductive nitrogen-rich carbon fibers through high-temperature carbonization. Aspergillus niger has strong biosorption activity, can efficiently adsorb metal ions, and has low cultivation costs and good biosafety. It is generally used for microbial fermentation or wastewater treatment. By utilizing the biosorption ability of Aspergillus niger to enrich metal ions in metal salt solutions, carbon-metal composite materials can be prepared at low cost.
[0004] Alloy materials are a type of negative electrode material that relies on alloying reactions to store alkali metal ions, mainly including tin, antimony, bismuth, etc. Antimony metal chalcogenides have high theoretical specific capacity and low operating voltage, and are excellent negative electrode materials for alkali metal batteries.
[0005] MXene, or transition metal carbon / nitride, is a two-dimensional nanomaterial. MXene materials have the advantages of rich surface active groups, high conductivity up to the metal level, and low ion migration barrier, which helps to improve the charge transfer kinetics. MXene also has a supporting role, which can maintain the microstructure of the composite material and improve the cycle stability. However, as a two-dimensional material, MXene materials also have structural defects that are easy to stack, and it is necessary to design a reasonable heterostructure to maximize their strengths and avoid their weaknesses. Summary of the invention
[0006] In view of this, the object of the present invention is to provide an antimony selenide-Aspergillus niger derived carbon-MXene composite material and a preparation method and application thereof. The antimony selenide-Aspergillus niger derived carbon-MXene composite material of the present invention is used as a negative electrode material in a sodium / potassium ion battery, which has a high reversible capacity, excellent cycle stability, and high safety, and is suitable for large-scale energy storage equipment such as solar power generation, wind power generation, and backup power supply.
[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0008] The present invention provides a method for preparing an antimony selenide-Aspergillus niger-derived carbon-MXene composite material, comprising the following steps:
[0009] The spherical Aspergillus niger mycelium is cultured in a MXene dispersion to obtain the Aspergillus niger mycelium adsorbed with MXene;
[0010] The MXene-adsorbed Aspergillus niger mycelium is cultured in an antimony salt solution, and the obtained mycelium is freeze-dried to obtain an aerogel;
[0011] The aerogel is subjected to annealing treatment and selenization treatment to obtain an antimony selenide-Aspergillus niger derived carbon-MXene composite material.
[0012] Preferably, the MXene material in the MXene dispersion comprises Ti3C2T x 、Nb2CT x 、V4C3T x and TiVCT x One or more of .
[0013] Preferably, the mass of the MXene material in the MXene dispersion is 10-30% of the dry weight of the spherical Aspergillus niger mycelium.
[0014] Preferably, the antimony salt in the antimony salt solution includes one or more of SbCl3, Sb(NO3)3 and Sb(CH3COO)3.
[0015] Preferably, the concentration of the antimony salt solution is 0.1-0.2 mol / L.
[0016] Preferably, the annealing treatment temperature is 400-1300° C., and the holding time is 2-4 hours.
[0017] Preferably, the selenium source for the selenization treatment is selenium powder, and the mass ratio of the material obtained by annealing treatment to the selenium powder is 1:2-1:5.
[0018] Preferably, the temperature of the selenization treatment is 300-600° C., and the insulation time is 2-4 hours.
[0019] The present invention also provides an antimony selenide-Aspergillus niger derived carbon-MXene composite material obtained by the preparation method described in the above technical scheme, comprising Aspergillus niger derived carbon, antimony selenide embedded in the Aspergillus niger derived carbon ribbon, and MXene wrapped on the surface of the Aspergillus niger derived carbon ribbon.
[0020] The present invention also provides the use of the antimony selenide-Aspergillus niger derived carbon-MXene composite material described in the above technical solution in the negative electrode of a sodium or potassium ion battery.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] The invention provides a method for preparing an antimony selenide-Aspergillus niger derived carbon-MXene composite material, comprising the following steps: culturing spherical Aspergillus niger mycelium in a MXene dispersion to obtain Aspergillus niger mycelium adsorbed with MXene; culturing the Aspergillus niger mycelium adsorbed with MXene in an antimony salt solution, freeze-drying the obtained mycelium to obtain an aerogel; and annealing and selenizing the aerogel to obtain an antimony selenide-Aspergillus niger derived carbon-MXene composite material.
[0023] The present invention cultivates living Aspergillus niger in a MXene dispersion, and under the action of biological adsorption, MXene sheets can be evenly distributed on the surface of the mycelium to avoid stacking. The present invention sequentially carbonizes (annealing) and selenizes the Aspergillus niger mycelium adsorbed with antimony metal and MXene after drying to obtain an antimony selenide-Aspergillus niger derived carbon-MXene composite material. Due to the biological activity of Aspergillus niger, antimony selenide exists inside the mycelium and MXene is wrapped on the surface of the mycelium. The preparation method of the composite material of the present invention has the following advantages: first, the metabolic activity of Aspergillus niger enables the active materials antimony selenide and MXene to be "automatically" evenly distributed, which simplifies the synthesis process and reduces the production cost; second, the Aspergillus niger that has been adsorbed is freeze-dried to obtain a fluffy aerogel, which is subjected to selenization treatment. The resulting nano-sized selenide particles can be completely embedded in the carbon fiber, which can prevent the structural collapse caused by the drastic volume change during the alloying reaction and improve the specific capacity and cycle stability of the composite material; third, the MXene wrapped in the outer layer can not only improve the conductivity of the composite fiber, but also prevent the loss of antimony selenide into the electrolyte through chemical adsorption of surface functional groups, thereby significantly improving the cycle stability of the material.
[0024] The antimony selenide-Aspergillus niger derived carbon-MXene composite material of the present invention has the characteristics of simple preparation, low cost, and green environmental protection. The test results show that the antimony selenide-Aspergillus niger derived carbon-MXene composite material of the present invention is a ternary heterogeneous structure, has a high sodium / potassium storage capacity and excellent cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0026] Figure 1 This is a flow chart for preparing the antimony selenide-Aspergillus niger derived carbon-MXene composite material of the present invention;
[0027] Figure 2 A scanning electron microscope (SEM) image of the antimony selenide-Aspergillus niger-derived carbon-MXene composite material provided in Example 1 of the present invention;
[0028] Figure 3 A transmission electron microscope (TEM) image of the antimony selenide-Aspergillus niger-derived carbon-MXene composite material provided in Example 1 of the present invention;
[0029] Figure 4 The X-ray diffraction (XRD) pattern of the antimony selenide-Aspergillus niger derived carbon-MXene composite material provided in Example 1 of the present invention;
[0030] Figure 5 This is a scanning electron microscope (SEM) image of the antimony selenide-Aspergillus niger derived carbon composite material provided in Example 2 of the present invention;
[0031] Figure 6 An X-ray diffraction (XRD) pattern of the antimony selenide-Aspergillus niger derived carbon composite material provided in Example 2 of the present invention;
[0032] Figure 7 A scanning electron microscope (SEM) image of the Aspergillus niger-derived carbon material provided in Example 3 of the present invention;
[0033] Figure 8 An X-ray diffraction (XRD) pattern of the Aspergillus niger-derived carbon material provided in Example 3 of the present invention;
[0034] Fig. 9 This is a constant current charge and discharge curve diagram of Test Example 1 of the present invention;
[0035] Fig.10 This is a small current cycle performance diagram of Test Example 1 of the present invention;
[0036] Fig.11 This is a high current cycle performance diagram of Test Example 1 of the present invention;
[0037] Fig.12 It is the rate performance diagram of Test Example 1 of the present invention;
[0038] Fig.13 This is a constant current charge and discharge curve diagram of Test Example 2 of the present invention;
[0039] Fig.14 This is a small current cycle performance diagram of Test Example 2 of the present invention;
[0040] Fig.15 This is a high current cycle performance diagram of Test Example 2 of the present invention;
[0041] Fig.16 This is a rate performance diagram of Test Example 2 of the present invention;
[0042] Fig.17 This is a constant current charge and discharge curve diagram of Test Example 3 of the present invention;
[0043] Fig.18 This is a small current cycle performance diagram of Test Example 3 of the present invention;
[0044] Fig.19 This is a high current cycle performance diagram of Test Example 3 of the present invention;
[0045] Fig. 20 It is the rate performance diagram of Test Example 3 of the present invention;
[0046] Fig.21 This is a constant current charge and discharge curve diagram of Test Example 4 of the present invention;
[0047] Fig. 22 This is a small current cycle performance diagram of Test Example 4 of the present invention;
[0048] Fig.23 This is a high current cycle performance diagram of Test Example 4 of the present invention;
[0049] Fig.24 It is the rate performance diagram of Test Example 4 of the present invention;
[0050] Fig.25 This is a constant current charge and discharge curve diagram of Test Example 5 of the present invention;
[0051] Fig.26 This is a small current cycle performance diagram of Test Example 5 of the present invention;
[0052] Fig. 27 This is a high current cycle performance diagram of Test Example 5 of the present invention;
[0053] Fig.28 This is a rate performance diagram of Test Example 5 of the present invention;
[0054] Fig.29 This is a constant current charge and discharge curve diagram of Test Example 6 of the present invention;
[0055] Fig.30 This is a small current cycle performance diagram of Test Example 6 of the present invention;
[0056] Fig.31 This is a high current cycle performance diagram of Test Example 6 of the present invention;
[0057] Fig.32 This is the rate performance diagram of Test Example 6 of the present invention. DETAILED DESCRIPTION
[0058] The present invention provides a method for preparing an antimony selenide-Aspergillus niger-derived carbon-MXene composite material, comprising the following steps:
[0059] The spherical Aspergillus niger mycelium is cultured in a MXene dispersion to obtain the Aspergillus niger mycelium adsorbed with MXene;
[0060] The MXene-adsorbed Aspergillus niger mycelium is cultured in an antimony salt solution, and the obtained mycelium is freeze-dried to obtain an aerogel;
[0061] The aerogel is subjected to annealing treatment and selenization treatment to obtain an antimony selenide-Aspergillus niger derived carbon-MXene composite material.
[0062] In the present invention, unless otherwise specified, the materials and equipment used are commercially available products in the art.
[0063] In the present invention, the Aspergillus niger spores are preferably inoculated into a liquid culture medium for the first culture to obtain spherical Aspergillus niger mycelium.
[0064] In the present invention, the Aspergillus niger spores are preferably purchased from Shanghai Luwei Technology Co., Ltd., and the strain number is LWCC2002 (CMCC(F)98003).
[0065] In the present invention, the solvent of the liquid culture medium is preferably water, and the nutrients preferably include a carbon source and a nitrogen source, wherein the carbon source preferably includes glucose, and the nitrogen source preferably includes peptone; the mass of the carbon source is preferably 5 to 15 g, more preferably 10 g, and the mass of the nitrogen source is preferably 5 to 15 g, more preferably 8 g, per 500 mL of water. Before the inoculation, the liquid culture medium is sterilized in a high pressure steam sterilizer, and the sterilization temperature of the high pressure steam sterilizer is preferably 110 to 121°C, and the sterilization time is preferably 15 minutes to 1 hour.
[0066] In the present invention, the inoculation is preferably carried out using a 1 microliter inoculation loop. The first culture is preferably carried out in a constant temperature shaking incubator, the temperature of the constant temperature shaking incubator is preferably 30-37°C, more preferably 35°C, the shaking rate is preferably 100-200 rpm, more preferably 160 rpm, and the culture time is preferably 40-72 hours, more preferably 40-48 hours.
[0067] In the present invention, after the first culturing, the method preferably further comprises: filtering the obtained culture solution, washing the obtained mycelium, and the washing agent is preferably water, and the water is preferably deionized water.
[0068] The present invention uses Aspergillus niger as the carbon material of the electrode material and performs high-temperature calcination to maintain a typical one-dimensional structure.
[0069] After obtaining the spherical Aspergillus niger mycelium, the present invention performs a second culture on the spherical Aspergillus niger mycelium in a MXene dispersion to obtain the Aspergillus niger mycelium adsorbed with MXene.
[0070] In the present invention, the MXene material in the MXene dispersion preferably includes Ti3C2T x 、Nb2CT x 、V4C3T x and TiVCT x One or more of the above, the dispersant is preferably deionized water; the MXene material is preferably a few-layer MXene, and the concentration of the MXene dispersion is preferably 0.1 mg / mL.
[0071] In the present invention, the mass of the MXene material in the MXene dispersion is preferably 10-30% of the dry weight of the spherical Aspergillus niger mycelium. The mass of the MXene material of the present invention can obtain a composite material with high capacity and good stability.
[0072] In the present invention, the second culture is preferably carried out in a constant temperature shaking incubator, the temperature of the constant temperature shaking incubator is preferably 25-37°C, more preferably 35°C, the shaking rate is preferably 100-200prm, more preferably 160rpm, and the culture time is preferably 24-48 hours.
[0073] In the present invention, after the second culture, the method preferably further comprises: filtering the obtained culture solution, washing the obtained mycelium, and the washing agent is preferably anhydrous ethanol.
[0074] After obtaining the Aspergillus niger mycelium adsorbed with MXene, the present invention cultured the Aspergillus niger mycelium adsorbed with MXene in an antimony salt solution for a third time, and freeze-dried the obtained mycelium to obtain an aerogel.
[0075] In the present invention, the antimony salt in the antimony salt solution preferably includes one or more of SbCl3 and / or Sb(NO3)3 and Sb(CH3COO)3, and the solvent of the antimony salt solution is preferably anhydrous ethanol. The concentration of the antimony salt solution is preferably 0.1-0.2 mol / L. The concentration of the antimony salt solution of the present invention has a high adsorption capacity and a high capacity of the composite material.
[0076] In the present invention, the third culture is preferably carried out in a constant temperature shaking incubator, the temperature of the constant temperature shaking incubator is preferably 25~37°C, more preferably 35°C, the shaking rate is preferably 100~200prm, more preferably 160rpm, and the culture time is preferably 24~48 hours.
[0077] In the present invention, after the third culture, the step preferably further comprises: filtering the obtained culture solution, washing the obtained mycelium, and the washing agent is preferably anhydrous ethanol.
[0078] In the present invention, the freeze-drying temperature is preferably -40 to -80°C, more preferably -55°C, and the time is preferably 2 to 4 days, more preferably 3 days. Before freeze-drying, the mycelium is pre-frozen in liquid nitrogen.
[0079] After obtaining the aerogel, the present invention performs annealing treatment and selenization treatment on the aerogel to obtain an antimony selenide-Aspergillus niger derived carbon-MXene composite material.
[0080] In the present invention, the annealing treatment is preferably carried out in a protective atmosphere, and the protective gas of the protective atmosphere is preferably argon or nitrogen; the annealing treatment is preferably carried out in a tubular furnace, the annealing treatment temperature is preferably 400~1300°C, more preferably 600°C, the holding time is preferably 2~4 hours, and the heating rate from room temperature to the annealing treatment temperature is preferably 3~5°C / min.
[0081] In the present invention, the annealing treatment preferably further comprises: naturally cooling the obtained material to room temperature.
[0082] In the present invention, the selenization treatment is preferably carried out in a protective atmosphere, and the protective gas of the protective atmosphere is preferably argon or nitrogen; the temperature of the selenization treatment is preferably 300~600°C, more preferably 400°C, the insulation time is preferably 2~4 hours, and the heating rate from room temperature to the selenization treatment temperature is preferably 3~5°C / min.
[0083] In the present invention, the selenization treatment is preferably carried out in a double-layer gasification sleeve, the material obtained by annealing is placed in the inner sleeve, and the selenium powder is placed on the inner wall of the outer sleeve. The mass ratio of the material obtained by annealing to the selenium powder is preferably 1:2~1:5, more preferably 1:4.
[0084] In the present invention, the selenization treatment preferably further includes natural cooling and grinding.
[0085] In the present invention, after the aerogel is annealed and selenized, the mycelium is transformed into a flat, hollow, tubular Aspergillus niger-derived carbon, which can be regarded as an Aspergillus niger-derived carbon ribbon. At the same time, the formed antimony selenide is embedded in the Aspergillus niger-derived carbon ribbon, and the MXene is wrapped on the surface of the Aspergillus niger-derived carbon ribbon.
[0086] The present invention also provides an antimony selenide-Aspergillus niger-derived carbon-MXene composite material obtained by the preparation method described in the above technical scheme.
[0087] In the present invention, the antimony selenide-Aspergillus niger derived carbon-MXene composite material includes Aspergillus niger derived carbon, antimony selenide embedded in the Aspergillus niger derived carbon ribbon, and MXene wrapped on the surface of the Aspergillus niger derived carbon ribbon.
[0088] The present invention also provides the use of the antimony selenide-Aspergillus niger derived carbon-MXene composite material described in the above technical solution in the negative electrode of a sodium or potassium ion battery.
[0089] In the present invention, the antimony selenide-Aspergillus niger derived carbon-MXene composite material is used as an active material (sodium / potassium storage) for the negative electrode of a sodium or potassium ion battery. The negative electrode of the sodium or potassium ion battery is preferably a copper foil with a coating on the surface, the thickness of the coating is preferably 120 microns, and the slurry for preparing the coating preferably includes an active material, a conductive agent, a binder and an organic solvent; the active material is the antimony selenide-Aspergillus niger derived carbon-MXene composite material described in the above technical solution, the conductive agent is preferably acetylene black, the binder is preferably polyvinylidene fluoride (PVDF), and the mass ratio of the active material, the conductive agent and the binder is preferably 7:2:1; the organic solvent is preferably N-methylpyrrolidone (NMP).
[0090] Figure 1 This is a preparation flow chart of the antimony selenide-Aspergillus niger derived carbon-MXene composite material of the present invention: culturing spherical Aspergillus niger mycelium in a liquid culture medium; preparing a few-layer MXene dispersion, placing the mycelium therein for oscillation culture; preparing an antimony salt solution, placing the Aspergillus niger mycelium adsorbed with MXene therein for oscillation culture; filtering out and washing the mycelium, and freeze-drying it to obtain an aerogel; annealing the aerogel in a tubular furnace, and then performing high-temperature vapor phase selenization; grinding the cooled product into powder to obtain an antimony selenide-Aspergillus niger derived carbon-MXene composite material.
[0091] In order to further illustrate the present invention, the antimony selenide-Aspergillus niger derived carbon-MXene composite material provided by the present invention and its preparation method and application are described in detail below in combination with the accompanying drawings and examples, but they should not be construed as limiting the scope of protection of the present invention.
[0092] Example 1
[0093] First, prepare the liquid culture medium. Add 10g glucose, 8g peptone, and 500mL deionized water to a 500mL conical flask, and seal it with a rubber band. Then place the conical flask in a high-pressure steam sterilizer and sterilize it at 121°C for 1h. After cooling naturally to room temperature, open the sealing film on the clean bench, use a 1 μl inoculation loop to dip a small amount of spores on the Aspergillus niger culture on the solid culture medium, and send it into the liquid culture medium. Then seal the sealing film. Pay attention to aseptic operation here. Put the inoculated culture medium into a constant temperature shaking incubator, set the speed to 160 revolutions per minute, and culture it at 35°C for 40h.
[0094] The conical flask containing Aspergillus niger was taken out, the sealing film was opened, and the spherical Aspergillus niger mycelium was filtered out with a food-grade filter. It was rinsed with deionized water several times to wash off most of the culture solution remaining on the mycelium. It can be observed that the color of the mycelium changed from yellow-brown to white. 300 mL of a few-layer MXene dispersion containing 30 mg Ti3C2T x MXene, the dispersant is deionized water, the dispersion method is magnetic stirring for 1 hour, and then ultrasonication at 300W power for 30 minutes; add Aspergillus niger mycelium and seal with sealing film; put the conical flask into a constant temperature shaking incubator, set the speed to 160 revolutions per minute, and culture at 35℃ for 24 hours;
[0095] The conical flask containing Aspergillus niger was taken out, the sealing film was opened, and the spherical Aspergillus niger mycelium was filtered out with a food-grade filter, and the spherical Aspergillus niger mycelium was washed with anhydrous ethanol for multiple times to wash off most of the culture solution remaining on the mycelium, and the mycelium was retained for later use; 300 mL of SbCl3 solution was prepared in a clean conical flask, the solvent was anhydrous ethanol, and the concentration of SbCl3 was 0.1 mol / L, and the Aspergillus niger mycelium was added, and the flask was sealed with a sealing film; the conical flask was placed in a constant temperature shaking incubator, the speed was set to 160 revolutions per minute, and cultured at 35°C for 24 hours;
[0096] Take out the conical flask, open the sealing film, filter out the Aspergillus niger mycelium with a food-grade filter, rinse it with anhydrous ethanol several times to clean off the residual culture solution; quickly freeze the mycelium with liquid nitrogen, then put it into a freeze dryer, and freeze-dry the mycelium into aerogel at a cold trap temperature of -55°C for about 2 days; put the dried aerogel into a tubular furnace, pass argon gas into the tube for 60 minutes before heating, maintain the argon atmosphere for annealing, the heating rate is 3°C / min, and it is kept at 600°C for 2h, and the tail gas is passed into natural water; the material is naturally cooled to room temperature and then taken out;
[0097] A double-layer gasification sleeve is placed in a tubular furnace, and the material and selenium powder are placed in the double-layer gasification sleeve, wherein the material is placed in the inner sleeve, and the selenium powder is placed on the inner wall of the outer sleeve, and the feed ratio is 1:4 (material: selenium powder mass); argon gas is passed into the tube for 60 minutes before heating, and the argon atmosphere is maintained for annealing treatment, with a heating rate of 3°C / min, and maintained at 400°C for 2h, and the tail gas is passed into natural water; the material is taken out after naturally cooling to room temperature, and the product is ground into powder to obtain antimony selenide-Aspergillus niger derived carbon-MXene composite material.
[0098] Example 2
[0099] First, prepare the liquid culture medium. Add 10g glucose, 8g peptone, and 500mL deionized water to a 500mL conical flask, and seal it with a rubber band. Then place the conical flask in a high-pressure steam sterilizer and sterilize it at 121°C for 1h. After cooling naturally to room temperature, open the sealing film on the clean bench, use a 1 μl inoculation loop to dip a small amount of spores on the Aspergillus niger culture on the solid culture medium, and send it into the liquid culture medium. Then seal the sealing film, and pay attention to aseptic operation here. Put the inoculated culture medium into a constant temperature shaking incubator, set the speed to 160 revolutions per minute, and culture it at 35°C for 40h.
[0100] The conical flask containing Aspergillus niger was taken out, the sealing film was opened, and the spherical Aspergillus niger mycelium was filtered out with a food-grade filter, and the spherical Aspergillus niger mycelium was washed with deionized water for several times to wash off most of the culture solution remaining on the mycelium. It can be observed that the color of the mycelium changed from yellow-brown to white; 300 mL of SbCl3 solution was prepared in the cleaned conical flask, the solvent was anhydrous ethanol, the concentration of SbCl3 was 0.1 mol / L, the Aspergillus niger mycelium was added, and the flask was sealed with a sealing film; the conical flask was placed in a constant temperature shaking incubator, the speed was set to 160 revolutions per minute, and cultured at 35°C for 24 hours;
[0101] Take out the conical flask, open the sealing film, filter out the Aspergillus niger mycelium with a food-grade filter, rinse it with anhydrous ethanol several times to clean off the residual culture solution; freeze the mycelium with liquid nitrogen, then put it into a freeze dryer, and freeze-dry the mycelium into aerogel at a cold trap temperature of -55°C, which takes about 2 days; put the dried aerogel into a tubular furnace, and pass argon gas into the tube for 60 minutes before heating, maintain the argon atmosphere for annealing, the heating rate is 3°C / min, and it is kept at 600°C for 2h, and the tail gas is passed into natural water; the material is naturally cooled to room temperature and then taken out;
[0102] A double-layer gasification sleeve is placed in a tubular furnace, and the material and selenium powder are placed in the double-layer gasification sleeve, wherein the material is placed in the inner sleeve, and the selenium powder is placed on the inner wall of the outer sleeve, and the feed ratio is 1:4 (material: selenium powder mass); argon gas is passed into the tube for 60 minutes before heating, and the argon atmosphere is maintained for annealing treatment, with a heating rate of 3°C / min, and maintained at 400°C for 2h, and the tail gas is passed into natural water; the material is taken out after naturally cooling to room temperature, and the product is ground into powder to obtain antimony selenide-Aspergillus niger derived carbon composite material.
[0103] Example 3
[0104] First, prepare the liquid culture medium. Add 10g glucose, 8g peptone, and 500mL deionized water to a 500mL conical flask, and seal it with a rubber band. Then place the conical flask in a high-pressure steam sterilizer and sterilize it at 121°C for 1h. After cooling naturally to room temperature, open the sealing film on the clean bench, use a 1 μl inoculation loop to dip a small amount of spores on the Aspergillus niger culture on the solid culture medium, and send it into the liquid culture medium. Then seal the sealing film, and pay attention to aseptic operation here. Put the inoculated culture medium into a constant temperature shaking incubator, set the speed to 160 revolutions per minute, and culture it at 35°C for 40h.
[0105] The conical flask containing the cultured Aspergillus niger was taken out, the sealing film was opened, and the spherical Aspergillus niger mycelium was filtered out with a food-grade filter, and the mycelium was rinsed with deionized water for several times to wash away most of the culture solution remaining on the mycelium. It can be observed that the color of the mycelium was washed from yellow-brown to white;
[0106] The mycelium was frozen with liquid nitrogen and then placed in a freeze dryer. The mycelium was freeze-dried into aerogel at a cold trap temperature of -55°C, which took about 3 days. The dried aerogel was placed in a tubular furnace, and argon was introduced into the tube for 60 minutes before heating. The argon atmosphere was maintained for annealing treatment at a heating rate of 3°C / min and maintained at 600°C for 2 hours. The exhaust gas was introduced into natural water. The material was taken out after naturally cooling to room temperature, and the product was ground into powder to obtain a biomass-derived carbon material.
[0107] The samples obtained in Example 1 were subjected to scanning electron microscopy (SEM), transmission electron microscopy (TEM), and X-ray diffraction (XRD) tests. The test results corresponded to Figure 2 , 3 , 4; The samples obtained in Example 2 were subjected to scanning electron microscopy (SEM) and X-ray diffraction (XRD) tests, and the test results corresponded to Figure 5 , 6 The samples obtained in Example 3 were subjected to scanning electron microscopy (SEM) and X-ray diffraction (XRD) tests, and the test results corresponded to Figure 7 , 8 .
[0108] Comparative Examples 1 to 3 show the SEM images of the samples obtained. Figure 2 , 5 , 7. By Figure 7 It can be seen that the Aspergillus niger derived carbon is a smooth carbon ribbon with a width of 0.5 to 3 microns; Figure 5 It can be seen that after compounding with antimony selenide, the carbon ribbon becomes fuller, which is due to the growth of antimony selenide inside the carbon ribbon; Figure 2 It can be seen that after compounding with the MXene material, a large number of wrinkles appear on the surface of the carbon ribbon. These wrinkles are the MXene material wrapped around the outside of the carbon ribbon.
[0109] Depend on Figure 3 , i.e., the TEM image of the sample obtained in Example 1, it can be seen that the antimony selenide particles are inside the Aspergillus niger derived carbon ribbon.
[0110] The XRD patterns of the samples obtained in Comparative Examples 1 to 3 are Figure 4 , 6 , 8. By Figure 8 It can be seen that the Aspergillus niger derived carbon is a kind of amorphous carbon; Figure 4 , 6 It can be seen that the XRD patterns of the samples obtained in Examples 1 and 2 completely correspond to those of antimony selenide.
[0111] The materials prepared in Examples 1 to 3 are used as energy storage active materials for the negative electrode of sodium / potassium ion batteries:
[0112] Test Example 1
[0113] The composite material obtained in Example 1 was used as an energy storage active material, acetylene black was used as a conductive agent, and polyvinylidene fluoride (PVDF) was used as a binder. The active material: conductive agent: binder was dissolved in an organic solvent N-methylpyrrolidone (NMP) at a mass ratio of 7:2:1, and stirred for 2 hours to obtain a slurry, which was evenly coated on a battery-grade copper foil with a coating thickness of about 120 microns, and vacuum dried at 80°C for 12 hours. After drying, the copper foil coated with the slurry was cut off and used to assemble a CR2032 button battery in an argon-filled glove box, using a NaClO4 electrolyte with a concentration of 1 mol / L, a solvent of a 1:1 volume ratio of ethylene carbonate / diethyl carbonate (EC / DEC) mixed solution, which contained 5% by mass of fluoroethylene carbonate, a Whatman GF / D glass fiber filter paper as a diaphragm, and a sodium foil as a counter electrode.
[0114] The obtained half-cell was subjected to constant current charge and discharge test, and the curve is shown in Fig. 9 .Depend on Fig. 9It can be seen that the discharge capacity of the first cycle is 584.7 mAh / g, the coulombic efficiency of the first cycle is 52.4%, the discharge capacity of the 10th cycle is 270.1 mAh / g, and the coulombic efficiency is 96.9%.
[0115] The obtained half-cell was subjected to a low current cycle performance test, i.e., a constant current charge-discharge cycle was performed at a current density of 0.1 A / g. The performance diagram is shown in Fig.10 .Depend on Fig.10 It can be seen that after 100 cycles, the discharge specific capacity is 222.7 mAh / g, and the capacity retention rate relative to the second cycle is 69.1%.
[0116] The obtained half-cell was subjected to a high current cycle performance test, i.e., a constant current charge-discharge cycle was performed at a current density of 1 A / g. The performance diagram is shown in Fig.11 .Depend on Fig.11 It can be seen that after 100 cycles, the discharge specific capacity is 193.1 mAh / g, and the capacity retention rate relative to the 12th cycle is 95.1%.
[0117] The obtained half-cell was subjected to rate performance test, and the performance graph is shown in Fig.12 .Depend on Fig.12 It can be seen that after 10 cycles at current densities of 0.1, 0.2, 0.5, 1, 2, and 5 A / g, respectively, the discharge specific capacities were 247.4, 225.4, 199.6, 181.5, 162.1, and 131.9 mAh / g, and the capacity retention rates were 100, 91.1, 80.7, 73.4, 65.5, and 53.3%, respectively.
[0118] Test Example 2
[0119] The composite material obtained in Example 1 was used as an energy storage active material, acetylene black was used as a conductive agent, and polyvinylidene fluoride (PVDF) was used as a binder. The active material: conductive agent: binder was dissolved in an organic solvent N-methylpyrrolidone (NMP) at a mass ratio of 7:2:1, and stirred for 2 hours to obtain a slurry, which was evenly coated on a battery-grade copper foil with a coating thickness of about 120 microns, and vacuum dried at 80°C for 12 hours. After drying, the copper foil coated with the slurry was cut off and used to assemble a CR2032 button battery in an argon-filled glove box, using a 1 mol / L potassium bis(fluorosulfonyl)imide (KFSI) electrolyte, a solvent was a 1:1 volume ratio of ethylene carbonate / diethyl carbonate (EC / DEC) mixed solution, which contained 5% by mass of fluoroethylene carbonate, a Whatman GF / D glass fiber filter paper was used as a diaphragm, and a potassium foil was used as a counter electrode.
[0120] The obtained half-cell was subjected to constant current charge and discharge test, and the curve is shown in Fig.13 .Depend on Fig.13It can be seen that the discharge capacity of the first cycle is 813.3 mAh / g, the coulombic efficiency of the first cycle is 56.2%, and the discharge capacity of the 10th cycle is 406.1 mAh / g, and the coulombic efficiency is 98.6%.
[0121] The obtained half-cell was subjected to a low current cycle performance test, i.e., a constant current charge-discharge cycle was performed at a current density of 0.1 A / g. The performance diagram is shown in Fig.14 .Depend on Fig.14 It can be seen that after 30 cycles, the discharge specific capacity is 392.6 mAh / g, and the capacity retention rate relative to the second cycle is 82.6%.
[0122] The obtained half-cell was subjected to a high current cycle performance test, i.e., a constant current charge-discharge cycle was performed at a current density of 1 A / g. The performance diagram is shown in Fig.15 .Depend on Fig.15 It can be seen that after 100 cycles, the discharge specific capacity is 419.5 mAh / g, and the capacity retention rate relative to the 12th cycle is 89.8%.
[0123] The obtained half-cell was subjected to rate performance test, and the performance graph is shown in Fig.16 .Depend on Fig.16 It can be seen that after 10 cycles at current densities of 0.1, 0.2, 0.5, 1, 2, and 5 A / g, respectively, the discharge specific capacities are 472.6, 430.9, 388.8, 352.7, 249.1, and 165.7 mAh / g, and the capacity retention rates are 100, 91.2, 82.3, 74.6, 52.7, and 35.1%, respectively.
[0124] Test Example 3
[0125] The composite material obtained in Example 2 was used as an energy storage active material, acetylene black was used as a conductive agent, and polyvinylidene fluoride (PVDF) was used as a binder. The active material: conductive agent: binder was dissolved in an organic solvent N-methylpyrrolidone (NMP) at a mass ratio of 7:2:1, and stirred for 2 hours to obtain a slurry, which was evenly coated on a battery-grade copper foil with a coating thickness of about 120 microns, and vacuum dried at 80°C for 12 hours. After drying, the copper foil coated with the slurry was cut off and used to assemble a CR2032 button battery in an argon-filled glove box, using a NaClO4 electrolyte with a concentration of 1 mol / L, a solvent of a 1:1 volume ratio of ethylene carbonate / diethyl carbonate (EC / DEC) mixed solution, which contained 5% by mass of fluoroethylene carbonate, a Whatman GF / D glass fiber filter paper as a diaphragm, and a sodium foil as a counter electrode.
[0126] The obtained half-cell was subjected to constant current charge and discharge test, and the curve is shown in Fig.17 .Depend on Fig.17It can be seen that the discharge capacity of the first cycle is 285.9 mAh / g, the coulombic efficiency of the first cycle is 54.1%, the discharge capacity of the 10th cycle is 136.5 mAh / g, and the coulombic efficiency is 98.2%.
[0127] The obtained half-cell was subjected to a low current cycle performance test, i.e., a constant current charge-discharge cycle was performed at a current density of 0.1 A / g. The performance diagram is shown in Fig.18 .Depend on Fig.18 It can be seen that after 50 cycles, the discharge specific capacity is 123.3 mAh / g, and the capacity retention rate relative to the second cycle is 79.3%.
[0128] The obtained half-cell was subjected to a high current cycle performance test, i.e., a constant current charge-discharge cycle was performed at a current density of 1 A / g. The performance diagram is shown in Fig.19 .Depend on Fig.19 It can be seen that after 100 cycles, the discharge specific capacity is 98.9 mAh / g, and the capacity retention rate relative to the 11th cycle is 97.8%.
[0129] The obtained half-cell was subjected to rate performance test, and the performance graph is shown in Fig. 20 .Depend on Fig. 20 It can be seen that after 10 cycles at current densities of 0.1, 0.2, 0.5, 1, 2, and 5 A / g, respectively, the discharge specific capacities are 123.7, 118.2, 109.9, 94.5, 88.8, and 71.8 mAh / g, and the capacity retention rates are 100, 95.6, 88.8, 76.4, 71.8, and 58.0%, respectively.
[0130] Test Example 4
[0131] The composite material obtained in Example 2 was used as an energy storage active material, acetylene black was used as a conductive agent, and polyvinylidene fluoride (PVDF) was used as a binder. The active material: conductive agent: binder was dissolved in an organic solvent N-methylpyrrolidone (NMP) at a mass ratio of 7:2:1, and stirred for 2 hours to obtain a slurry, which was evenly coated on a battery-grade copper foil with a coating thickness of about 120 microns, and vacuum dried at 80°C for 12 hours. After drying, the copper foil coated with the slurry was cut off and used to assemble a CR2032 button battery in an argon-filled glove box, using a 1 mol / L potassium bis(fluorosulfonyl)imide (KFSI) electrolyte, a solvent was a 1:1 volume ratio of ethylene carbonate / diethyl carbonate (EC / DEC) mixed solution, which contained 5% by mass fraction of fluoroethylene carbonate, a Whatman GF / D glass fiber filter paper was used as a diaphragm, and a potassium foil was used as a counter electrode.
[0132] The obtained half-cell was subjected to constant current charge and discharge test, and the curve is shown in Fig.21 .Depend on Fig.21It can be seen that the discharge capacity of the first cycle is 718.8 mAh / g, the coulombic efficiency of the first cycle is 57.8%, the discharge capacity of the 10th cycle is 289.1 mAh / g, and the coulombic efficiency is 97.7%.
[0133] The obtained half-cell was subjected to a low current cycle performance test, i.e., a constant current charge-discharge cycle was performed at a current density of 0.1 A / g. The performance diagram is shown in Fig. 22 .Depend on Fig. 22 It can be seen that after 100 cycles, the discharge specific capacity is 135.3 mAh / g, and the capacity retention rate relative to the second cycle is 32.2%.
[0134] The obtained half-cell was subjected to a high current cycle performance test, i.e., a constant current charge-discharge cycle was performed at a current density of 1 A / g. The performance diagram is shown in Fig.23 .Depend on Fig.23 It can be seen that after 100 cycles, the discharge specific capacity is 96.9 mAh / g, and the capacity retention rate relative to the 12th cycle is 56.7%.
[0135] The obtained half-cell was subjected to rate performance test, and the performance graph is shown in Fig.24 .Depend on Fig.24 It can be seen that after 10 cycles at current densities of 0.1, 0.2, 0.5, 1, 2, and 5 A / g, respectively, the discharge specific capacities are 305.2, 229.0, 171.6, 128.5, 88.2, and 39.6 mAh / g, and the capacity retention rates are 100, 75.0, 56.2, 42.1, 28.9, and 13.0%, respectively.
[0136] Test Example 5
[0137] The biomass-derived carbon material obtained in Example 3 was used as an energy storage active material, acetylene black was used as a conductive agent, and polyvinylidene fluoride (PVDF) was used as a binder. The active material: conductive agent: binder were dissolved in an organic solvent N-methylpyrrolidone (NMP) at a mass ratio of 7:2:1, stirred for 2 hours to obtain a slurry, which was evenly coated on a battery-grade copper foil with a coating thickness of about 120 microns, and vacuum dried at 80°C for 12 hours. After drying, the copper foil coated with the slurry was cut off and used to assemble a CR2032 button battery in an argon-filled glove box, using a NaClO4 electrolyte with a concentration of 1 mol / L, a solvent of a 1:1 volume ratio of ethylene carbonate / diethyl carbonate (EC / DEC) mixed solution, which contained 5% by mass of fluoroethylene carbonate, a Whatman GF / D glass fiber filter paper as a diaphragm, and a sodium foil as a counter electrode.
[0138] The obtained half-cell was subjected to constant current charge and discharge test, and the curve is shown in Fig.25 .Depend on Fig.25It can be seen that the discharge capacity of the first cycle is 424.4 mAh / g, the coulombic efficiency of the first cycle is 33.1%, the discharge capacity of the 10th cycle is 140.8 mAh / g, and the coulombic efficiency is 92.4%.
[0139] The obtained half-cell was subjected to a low current cycle performance test, i.e., a constant current charge-discharge cycle was performed at a current density of 0.1 A / g. The performance diagram is shown in Fig.26 .Depend on Fig.26 It can be seen that after 100 cycles, the discharge specific capacity is 93.7 mAh / g, and the capacity retention rate relative to the second cycle is 81.4%.
[0140] The obtained half-cell was subjected to a high current cycle performance test, i.e., a constant current charge-discharge cycle was performed at a current density of 1 A / g. The performance diagram is shown in Fig. 27 .Depend on Fig. 27 It can be seen that after 100 cycles, the discharge specific capacity is 53.6 mAh / g, and the capacity retention rate relative to the 12th cycle is 93.7%.
[0141] The obtained half-cell was subjected to rate performance test, and the performance graph is shown in Fig.28 .Depend on Fig.28 It can be seen that after 10 cycles at current densities of 0.1, 0.2, 0.5, 1, 2, and 5 A / g, respectively, the discharge specific capacities are 154.5, 123.5, 89.6, 72.3, 55.5, and 29.4 mAh / g, and the capacity retention rates are 100, 79.9, 58.0, 46.8, 35.9, and 19.0%, respectively.
[0142] Test Example 6
[0143] The biomass-derived carbon material obtained in Example 3 was used as an energy storage active material, acetylene black was used as a conductive agent, and polyvinylidene fluoride (PVDF) was used as a binder. The active material: conductive agent: binder were dissolved in an organic solvent N-methylpyrrolidone (NMP) at a mass ratio of 7:2:1, stirred for 2 hours to obtain a slurry, which was evenly coated on a battery-grade copper foil with a coating thickness of about 120 microns, and vacuum dried at 80°C for 12 hours. After drying, the copper foil coated with the slurry was cut off and used to assemble a CR2032 button battery in an argon-filled glove box, using a 1 mol / L potassium bis(fluorosulfonyl)imide (KFSI) electrolyte, a solvent was a 1:1 volume ratio of ethylene carbonate / diethyl carbonate (EC / DEC) mixed solution, which contained 5% by mass of fluoroethylene carbonate, a Whatman GF / D glass fiber filter paper was used as a separator, and a potassium foil was used as a counter electrode.
[0144] The obtained half-cell was subjected to constant current charge and discharge test, and the curve is shown in Fig.29 .Depend on Fig.29It can be seen that the discharge capacity of the first cycle is 380.4 mAh / g, the coulombic efficiency of the first cycle is 39.3%, the discharge capacity of the 10th cycle is 159.4 mAh / g, and the coulombic efficiency is 97.5%.
[0145] The obtained half-cell was subjected to a low current cycle performance test, i.e., a constant current charge-discharge cycle was performed at a current density of 0.1 A / g. The performance diagram is shown in Fig.30 .Depend on Fig.30 It can be seen that after 100 cycles, the discharge specific capacity is 155.8 mAh / g, and the capacity retention rate relative to the second cycle is 94.1%.
[0146] The obtained half-cell was subjected to a high current cycle performance test, i.e., a constant current charge-discharge cycle was performed at a current density of 1 A / g. The performance diagram is shown in Fig.31 .Depend on Fig.31 It can be seen that after 100 cycles, the discharge specific capacity is 48.9 mAh / g, and the capacity retention rate relative to the 12th cycle is 63.8%.
[0147] The obtained half-cell was subjected to rate performance test, and the performance graph is shown in Fig.32 .Depend on Fig.32 It can be seen that after 10 cycles at current densities of 0.1, 0.2, 0.5, 1, 2, and 5 A / g, respectively, the discharge specific capacities are 171.6, 140.1, 106.6, 83.3, 60.4, and 18.1 mAh / g, and the capacity retention rates are 100, 81.6, 62.1, 48.5, 35.2, and 10.5%, respectively.
[0148] Comparing the electrochemical performance test results of test examples 1 to 6, it can be seen that: when Aspergillus niger derived carbon is used alone as the negative electrode active material of the sodium / potassium ion battery, although the battery has good cycle stability, the capacity is low; after Aspergillus niger derived carbon is compounded with antimony selenide, the capacity is significantly improved, but the cycle stability decreases; and the antimony selenide-Aspergillus niger derived carbon-MXene composite material provided by the present invention has both a high mass specific capacity and excellent cycle stability. Among them, test example 1 has the best electrochemical performance of sodium ion batteries, and test example 2 has the best electrochemical performance of potassium ion batteries.
[0149] Although the above-mentioned embodiments have made a detailed description of the present invention, they are only some embodiments of the present invention, rather than all embodiments. People can also obtain other embodiments based on the embodiments of the present invention without creative work, and these embodiments all fall within the scope of protection of the present invention.
Claims
1. A method for preparing an antimony selenide-Aspergillus niger-derived carbon-MXene composite material, characterized in that: The following steps are involved: The spherical Aspergillus niger mycelium is cultured in a MXene dispersion to obtain the Aspergillus niger mycelium adsorbed with MXene; the mass of the MXene material in the MXene dispersion is 10-30% of the dry weight of the spherical Aspergillus niger mycelium; The MXene-adsorbed Aspergillus niger mycelium is cultured in an antimony salt solution, and the obtained mycelium is freeze-dried to obtain an aerogel; The aerogel is subjected to annealing treatment and selenization treatment to obtain an antimony selenide-Aspergillus niger derived carbon-MXene composite material; the antimony selenide-Aspergillus niger derived carbon-MXene composite material includes Aspergillus niger derived carbon, antimony selenide embedded in the Aspergillus niger derived carbon ribbon, and MXene wrapped on the surface of the Aspergillus niger derived carbon ribbon.
2. The preparation method according to claim 1, characterized in that: The MXene material in the MXene dispersion includes Ti3C2T x 、Nb2CT x 、V4C3T x and TiVCT x One or more of .
3. The preparation method according to claim 1, characterized in that: The antimony salt in the antimony salt solution includes one or more of SbCl3, Sb(NO3)3 and Sb(CH3COO)3.
4. The preparation method according to claim 1 or 3, characterized in that: The concentration of the antimony salt solution is 0.1-0.2 mol / L.
5. The preparation method according to claim 1, characterized in that: The annealing treatment is carried out at a temperature of 400-1300° C. and a heat preservation time of 2-4 hours.
6. The preparation method according to claim 1, characterized in that: The selenium source for the selenization treatment is selenium powder, and the mass ratio of the material obtained by annealing treatment to the selenium powder is 1:2-1:
5.
7. The preparation method according to claim 1 or 6, characterized in that: The temperature of the selenization treatment is 300-600° C., and the insulation time is 2-4 hours.
8. The antimony selenide-Aspergillus niger derived carbon-MXene composite material obtained by the preparation method according to any one of claims 1 to 7, characterized in that: The invention comprises carbon derived from Aspergillus niger, antimony selenide embedded in the carbon ribbon derived from Aspergillus niger and MXene wrapped on the surface of the carbon ribbon derived from Aspergillus niger.