A large single crystal Prussian white sodium ion positive electrode material and preparation method thereof
By combining Na and manganese sources into a mixed solution at room temperature and using the method of acid dissociation of cations, the problem of uneven HCN generation and precipitation in the preparation of Prussian white sodium ion positive electrode material was solved, and a low content was obtained Large single crystal materials with water volume and high capacity achieve better thermal stability and uniformity.
Patent Information
- Application Number
- CN202411102185.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-12
AI Technical Summary
The existing preparation method of Prussian white sodium ion positive electrode material has the problems of risk of HCN generation, difficulty in regulating the reaction rate, high moisture content and uneven precipitation.
The Na and manganese source were mixed solution at room temperature, and the reaction was added dropwise by acid dissociation of cations to prepare a large single crystal Prussian white sodium ion positive electrode material with low moisture content. The stirring and aging reaction were used to control the precipitation uniformity by controlling the precipitation. and particle size.
The generation of toxic gases is avoided, and uniform precipitation of Na and Mn is achieved, and the thermal stability and capacity of the synthetic positive electrode material are improved, and a large single crystal Prussian white sodium ion positive electrode material with low moisture content and high capacity is obtained.
Smart Images

Figure CN118637639B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a large single crystal Prussian white sodium ion positive electrode material and a preparation method thereof, belonging to the technical field of sodium ion batteries. Background Art
[0002] As a "substitute" product for lithium-ion batteries, sodium-ion batteries have received attention from various countries. The electrode material used in sodium-ion batteries is mainly sodium salt, which has more abundant reserves and sources and is cheaper than lithium salt. Since sodium ions have a larger radius than lithium ions, sodium-ion batteries are a preferred alternative when weight and energy density requirements are not high. Prussian blue sodium-ion positive electrode materials are favored by the industry due to their simple preparation process and wide and low-cost raw material sources.
[0003] At present, the synthesis method of Prussian white cathode material is generally to add manganese or iron source solution into Na4Fe(CN)6·10H2O solution and react at a constant temperature of 40-60°C for several hours. However, there is a risk of HCN production under heating conditions, and the reaction rate is not easy to control during the reaction, so a complexing agent needs to be added to control the reaction rate. The water content of Prussian white cathode material synthesized by conventional methods is high, the precipitation of Na and Mn is uneven, and the ratio is not easy to control.
[0004] Therefore, more research is needed on the synthesis methods of Prussian white sodium ion cathode materials. Summary of the invention
[0005] In view of the deficiencies in the prior art, the present invention proposes a large single crystal Prussian white sodium ion positive electrode material and a preparation method thereof. The method can synthesize the large single crystal Prussian white sodium ion positive electrode material at room temperature, and prepare Na and manganese sources into a mixed solution to make the precipitation of Na and Mn more uniform.
[0006] The technical solution of the present invention is a method for preparing a large single crystal Prussian white sodium ion positive electrode material, comprising the following steps:
[0007] Step 1, Na4Fe(CN)6·10H2O and ethylenediaminetetraacetic acid manganese sodium salt are mixed and dissolved to prepare a first solution A;
[0008] Step 2: Add the diluted acid as the second solution B dropwise into the first solution A under stirring, perform an aging reaction after the addition is completed, and finally wash and dry to obtain a Prussian white sodium ion positive electrode material with a low water content.
[0009] Furthermore, the stirring speed is 500-1000 rpm / min.
[0010] Furthermore, the aging reaction time is 2 hours.
[0011] Furthermore, the molar ratio of Na4Fe(CN)6·10H2O to ethylenediaminetetraacetic acid manganese sodium salt is 1:(1-1.05).
[0012] Furthermore, the acid is ascorbic acid, sulfuric acid, hydrochloric acid, nitric acid, acetic acid or citric acid.
[0013] At the same time, the present invention also provides a large single crystal Prussian white sodium ion positive electrode material obtained by the above preparation method, whose chemical formula is Na x Mn[Fe(CN)6] y , where 1.90≤x<2.00, 0.90≤y<1.
[0014] Furthermore, the particle size D of the large single crystal Prussian white sodium ion positive electrode material is 50 2~6μm.
[0015] Furthermore, the large single crystal Prussian white sodium ion positive electrode material has a specific surface area of 7.5 to 9.5 m 2 / g.
[0016] Furthermore, the water content of the large single crystal Prussian white sodium ion positive electrode material is less than 10%.
[0017] Furthermore, the Na:Mn ratio of the large single crystal Prussian white sodium ion positive electrode material is (1.90-2.00): 1
[0018] Another object of the present invention is to provide a positive electrode plate, comprising a positive electrode current collector and a positive electrode active material, wherein the positive electrode active material comprises the above-mentioned large single crystal Prussian white sodium ion positive electrode material.
[0019] Another object of the present invention is to provide a battery comprising the above-mentioned positive electrode plate.
[0020] Another object of the present invention is to provide an electrical device comprising the above-mentioned battery, wherein the battery is used to provide electrical energy.
[0021] Due to the adoption of the above technical scheme, the advantages of the present invention are: the present invention adopts the method of acid dissociation of cations to synthesize the Prussian white sodium ion positive electrode material with low water content at room temperature, avoiding the generation of toxic gas. Moreover, before the reaction, Na and manganese source are mixed in liquid phase to form a mixed solution, so that the precipitation of Na and Mn is more uniform, and at the same time, the synthesized positive electrode material has large primary particles, good thermal stability, low water content and high capacity. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a SEM image of the large single crystal Prussian white sodium ion positive electrode material of the present invention. DETAILED DESCRIPTION
[0023] In order to better understand the technical solutions of the embodiments of the present application, they are further described below in conjunction with some preferred embodiments of the present application.
[0024] In this specification, amounts, ratios and other numerical values are sometimes presented herein in a range format. It should be understood that such a range format is used for convenience and brevity, and should be flexibly understood to include not only the values explicitly specified as range limits, but also all individual values or sub-ranges encompassed within the range, as if each value and sub-range were explicitly specified.
[0025] The chemical formula of the large single crystal Prussian white sodium ion positive electrode material proposed in this application is Na x Mn[Fe(CN)6] y , where 1.90≤x<2.00, 0.90≤y<1. The synthesis method is:
[0026] (1) Na4Fe(CN)6·10H2O and ethylenediaminetetraacetic acid manganese sodium salt are mixed and dissolved to prepare a first solution A;
[0027] (2) The diluted acid is added dropwise as the second solution B into the first solution A. After the addition is completed, an aging reaction is performed. Finally, after washing and drying, a Prussian white sodium ion positive electrode material with a low water content is obtained.
[0028] The preparation method of the Prussian white sodium ion positive electrode material provided in the embodiment of the present application only needs to be synthesized at room temperature, and the Na and manganese sources are prepared into a mixed solution, which is more uniform.
[0029] The acid used in the synthesis method is ascorbic acid, sulfuric acid, hydrochloric acid, nitric acid, acetic acid or citric acid.
[0030] According to some embodiments of the present application, the particle size D of the large single crystal Prussian white sodium ion positive electrode material is 50 The particle size is 2-6 μm, the water content is less than 10%, and the specific surface area is 7.5-9.5 m 2 / g, Na:Mn of positive electrode material = (1.90~2.00):1.
[0031] According to some embodiments of the present application, the stirring speed is 500-1000 rpm / min.
[0032] According to some embodiments of the present application, the aging reaction time is 2 hours, the purpose of which is to allow the crystals to grow and make the crystals more perfect.
[0033] According to some embodiments of the present application, the above compound can be used as a positive electrode material for a sodium ion battery. For example, the above compound, Ketjen black, and a binder polyvinylidene fluoride (PVDF) are added to N-methylpyrrolidone (NMP) (the weight ratio of the compound to NMP is 3:1) at a weight ratio of 86:7:7, and the mixture is fully mixed, stirred to form a uniform slurry to prepare a positive electrode material (or a positive electrode active substance), coated on an aluminum foil current collector, dried, and pressed to obtain a positive electrode sheet, which can constitute an electrode assembly with a negative electrode sheet.
[0034] The present application also provides a battery, specifically a sodium ion battery, which comprises the above-mentioned electrode assembly. The sodium ion battery can be used in digital products, electric vehicles or energy storage fields.
[0035] For example, a sodium ion secondary battery can generally be composed of an electrode assembly, an electrolyte and a separator. Specifically, the electrode assembly may include a positive electrode sheet and a negative electrode sheet. As mentioned above, the positive electrode sheet may be made of materials including a positive electrode current collector and a positive electrode active material coated on the positive electrode current collector, as well as conventional adhesives, conventional conductive additives and the like. The positive electrode active material may include the above-mentioned compound proposed in this application. The negative electrode is made of materials including a current collector and a conventional negative electrode active material coated on the current collector, as well as conventional adhesives, conventional conductive additives and the like. The separator is a PP / PE film commonly used in this industry, which is used to separate the positive electrode from the negative electrode.
[0036] Some further embodiments of the present application further provide an electrical device, which includes the above-mentioned battery, and the above-mentioned battery is used to provide power. The electrical device may include digital products, electric vehicles, energy storage devices, etc.
[0037] The large single crystal Prussian white sodium ion positive electrode material and its preparation method proposed in this application are explained below through specific examples. The reagents or instruments not described in this application text are all contents that can be routinely confirmed by ordinary technicians in this field.
[0038] The reagents used in the following examples are shown in Table 1-1.
[0039] Table 1-1 Information on chemical reagents used in the examples of this application
[0040] ;
[0041] The equipment and analysis methods used in the following examples are as follows:
[0042] The mixing ball milling equipment is the SHQM double-ball ball mill of Lianyungang Chunlong Experimental Instrument Co., Ltd.
[0043] This application uses a fully automatic specific surface area and porosity analyzer (TriStarⅡ 3020, Murray McTicker Co., Ltd., USA) to test and analyze the specific surface area.
[0044] The moisture content is detected by a synchronous differential thermal analysis tester with an upper limit of 500°C and a heating rate of 10°C / min. The weight percentage of the weight loss part is the moisture content.
[0045] The element content test method is as follows: accurately weigh 0.2000g of the sample (accurate to 0.0001g) into a clean 100mL glass beaker. Add 10mL (1:1) aqua regia solution to the beaker (with a blank test), cover with a watch glass, place the beaker on a hot plate and heat the solution until it evaporates to near dryness, stop heating, remove the beaker and cool to room temperature. Rinse the watch glass and the side of the beaker with deionized water for at least 3 times, transfer all the solution to a 50mL volumetric flask, dilute with deionized water, and shake well. Transfer 1mL of the sample to a 100mL volumetric flask, dilute to volume, and shake well. The above solution was tested using an inductively coupled plasma emission spectrometer (Thermo Fisher Scientific Inc. / icap7400, USA) in accordance with the first part of YS / T 1006.2-2014.
[0046] Average particle size test: MS3000 laser particle size analyzer is used for testing, the method is as follows:
[0047] Take an appropriate amount of sample in a 100ml beaker, first rinse along the inner wall of the beaker with a wash bottle, then rinse the sample stuck to the bottom of the beaker with a wash bottle, and control the amount of pure water added to the beaker to 20~30mL, and the ultrasonic time is 5min (stir for 10s before, during and after ultrasonication, and the stirring rate is about 2r / s). Add 100±10ml of pure water to the injector of the MS3000 laser particle size analyzer, adjust the speed to 3000r / min, click start, and the instrument will automatically align the light and measure the background and wait for prompts to operate. Transfer the sample after ultrasonication to the stirring tank, and then rinse the beaker with a wash bottle to ensure that all samples are transferred. After the sample is completely added, the software automatically starts measuring. After the measurement is completed, the data is automatically saved.
[0048] The specific embodiments are as follows.
[0049] Example 1
[0050] Dissolve 0.1mol of Na4Fe(CN)6·10H2O and 0.105mol of ethylenediaminetetraacetic acid sodium manganese salt in 1L of distilled water to form a mixed solution A. Dissolve 2mol of ascorbic acid in 1L of distilled water to form solution B. Slowly add solution B to solution A under stirring at 500rmp / min, and control the dropping time for 1h. After the addition is completed, continue stirring and aging the reaction for 2h. The white precipitate after filtering and washing 3 times was dried at 150℃ for 10h to obtain Prussian white material 1, and the particle size, specific surface, Tg and battery tests were carried out. The data are shown in Table 1.
[0051] Example 2
[0052] Dissolve 0.1mol of Na4Fe(CN)6·10H2O and 0.1mol of ethylenediaminetetraacetic acid manganese sodium salt in 1L of distilled water to form a mixed solution A. Dissolve 2mol of sulfuric acid in 1L of distilled water to form solution B. Slowly add solution B to solution A under stirring at 500rmp / min, and control the dropping time for 1h. After the addition is completed, continue stirring and aging the reaction for 2h. The white precipitate after filtering and washing 3 times was dried at 150℃ for 10h to obtain Prussian white material 2, and the particle size, specific surface, Tg and battery tests were carried out. The data are shown in Table 1.
[0053] Example 3
[0054] Dissolve 0.1mol of Na4Fe(CN)6·10H2O and 0.105mol of ethylenediaminetetraacetic acid sodium manganese salt in 1L of distilled water to form a mixed solution A. Dissolve 2mol of hydrochloric acid in 1L of distilled water to form solution B. Slowly add solution B to solution A under stirring at 1000rmp / min, and control the dropping time for 1h. After the addition is completed, continue stirring and aging the reaction for 2h. The white precipitate after filtering and washing 3 times was dried at 150℃ for 10h to obtain Prussian white material 3, and the particle size, specific surface, Tg and battery tests were carried out. The data are shown in Table 1.
[0055] Example 4
[0056] Dissolve 0.1 mol of Na4Fe(CN)6·10H2O and 0.1 mol of ethylenediaminetetraacetic acid sodium manganese salt in 1L of distilled water to form a mixed solution A. Dissolve 2 mol of nitric acid in 1L of distilled water to form solution B. Slowly add solution B to solution A under stirring at 800rmp / min, and control the dropping time for 1h. After the addition is completed, continue stirring and aging the reaction for 2h. The white precipitate after filtering and washing 3 times was dried at 150℃ for 10h to obtain Prussian white material 4, and the particle size, specific surface, Tg and battery tests were carried out. The data are shown in Table 1.
[0057] Example 5
[0058] Dissolve 0.1 mol of Na4Fe(CN)6·10H2O and 0.102 mol of ethylenediaminetetraacetic acid sodium manganese salt in 1L of distilled water to form a mixed solution A. Dissolve 2 mol of acetic acid in 1L of distilled water to form a solution B. Slowly add solution B to solution A under stirring at 800 rpm, and control the dropping time for 1 hour. After the addition is completed, continue stirring and aging the reaction for 2 hours. The white precipitate after filtering and washing 3 times was dried at 150°C for 10 hours to obtain Prussian white material 5, and the particle size, specific surface, Tg and battery tests were carried out. The data are shown in Table 1.
[0059] Example 6
[0060] Dissolve 0.1 mol of Na4Fe(CN)6·10H2O and 0.1 mol of sodium manganese ethylenediaminetetraacetic acid in 1L of distilled water to form a mixed solution A. Dissolve 2 mol of citric acid in 1L of distilled water to form solution B. Slowly add solution B to solution A under stirring at 800 rpm, and control the dropping time for 1 hour. After the addition is completed, continue stirring and aging the reaction for 2 hours. The white precipitate after filtering and washing 3 times was dried at 150°C for 10 hours to obtain Prussian white material 6, and the particle size, specific surface, Tg and battery tests were carried out. The data are shown in Table 1.
[0061] Table 1 Characterization data of compounds obtained in Examples
[0062] ;
[0063] As shown in Table 1, the single crystal positive electrode material prepared by the above-mentioned embodiment of the present application has a water content of less than 10% and a specific surface area of 7.5 to 9.5 m 2 / g, the particle size is between 2.0 and 6.0μm, the primary large particle single crystal morphology, the Na:Mn ratio is between (1.90 and 2.00):1:, and the gram capacity can reach up to 147 mAh / g.
[0064] It can be seen from Table 1 that in the embodiments, the preparation methods of the present invention can synthesize large-sized primary particles with large single crystal morphology. Compared with other methods, the present invention only needs to be synthesized at room temperature, and the Na and manganese sources are mixed evenly in the solution, and the Na and Mn precipitated are more evenly distributed.
Claims
1. A method for preparing a large single crystal Prussian white sodium ion positive electrode material, characterized in that The following steps are involved: Step 1, Na4Fe(CN)6·10H2O and ethylenediaminetetraacetic acid manganese sodium salt are mixed and dissolved to prepare a first solution A, wherein the molar ratio of Na4Fe(CN)6·10H2O to ethylenediaminetetraacetic acid manganese sodium salt is 1:(1-1.05); Step 2, slowly dropping an acid having a concentration of 2 mol / L as the second solution B into the first solution A under stirring conditions for 1 hour, and the stirring speed is 500-1000 rpm / min; after the dropwise addition is completed, an aging reaction is performed, and the aging reaction time is 2 hours; finally, after washing and drying, a Prussian white sodium ion positive electrode material is obtained; The chemical formula of the Prussian white sodium ion positive electrode material is Na x Mn[Fe(CN)6] y , wherein 1.90≤x<2.00, 0.90≤y<1; the water content of the Prussian white sodium ion positive electrode material is less than 10%.
2. The method for preparing a large single crystal Prussian white sodium ion positive electrode material according to claim 1, characterized in that: The acid is ascorbic acid, sulfuric acid, hydrochloric acid, nitric acid, acetic acid or citric acid.
3. The method for preparing the large single crystal Prussian white sodium ion positive electrode material according to claim 1, characterized in that: Its particle size D 50 2~6μm.
4. The method for preparing a large single crystal Prussian white sodium ion positive electrode material according to claim 1, characterized in that: Its specific surface area is 7.5~9.5m 2 / g.
5. A positive electrode sheet, comprising a positive electrode current collector and a positive electrode active material, characterized in that: The positive electrode active material comprises the large single crystal Prussian white sodium ion positive electrode material according to any one of claims 1 to 4.
6. A battery, characterized in that: It includes the positive electrode sheet as claimed in claim 5.
7. An electrical equipment, characterized in that: It comprises the battery according to claim 6, wherein the battery is used to provide electrical energy.
Citation Information
Patent Citations
Prussian blue positive electrode material, sodium ion battery and preparation method and application thereof
CN111377462A
SNCR efficient aid, preparation method and application thereof
CN113967407A
Preparation method and application of Prussian blue analogue material
CN116534871A
Preparation method of ferromanganese-based Prussian blue sodium battery positive electrode material and positive electrode material prepared by method
CN117430134A
Method for rapidly preparing prussian blue analogue with monoclinic crystal structure
US20210043932A1